Method for regulating and controlling diameter of de-alloying rod without changing de-alloying topological structure

By combining laser powder bed melting technology and liquid metal dealloying with wire cutting and nitric acid solution treatment, the problem of topological structure destruction caused by chemical dealloying methods was solved, achieving high-temperature stable dealloyed topology and rod diameter control, thus improving the mechanical properties of the material.

CN118976909APending Publication Date: 2024-11-19SHANGHAI JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411084465.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The topological structures prepared by the chemical dealloying method in the prior art have extremely fine rod diameters, which are easily destroyed after subsequent heat treatment. Furthermore, the dealloying process with liquid metal produces a rough and porous structure, which is difficult to maintain the stability of the topological structure at high temperatures.

Method used

TiFeCu precursors were prepared using laser powder bed melting technology, combined with wire cutting and liquid metal dealloying treatment. The dealloying temperature and time were controlled, and the residues were then removed in nitric acid solution to ensure the integrity of the topological structure.

Benefits of technology

It was achieved that the stability of the topology was maintained at high temperatures, and the diameter of the dealloyed rod was controlled to avoid the destruction of the topology and improve the mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976909A_ABST
    Figure CN118976909A_ABST
Patent Text Reader

Abstract

The invention discloses a method for regulating and controlling the diameter of a dealloying rod without changing a dealloying topological structure, which comprises the following steps: printing Ti, Fe and Cu metal mixed powder by adopting a laser powder bed melting technology to prepare a TiFeCu precursor, carrying out linear cutting on the TiFeCu precursor, putting the TiFeCu precursor into a vacuum tube furnace to carry out liquid metal dealloying, taking Mg as molten pool metal, controlling the dealloying temperature to be 800-850 DEG C, controlling the time to be 20-60 minutes, and carrying out cooling to obtain the dealloying rod. And the LMD porous material containing the dealloying topological structure is put into a nitric acid solution to be soaked so as to remove Mg solidified on the LMD porous material. In order to solve the problem that in a chemical dealloying method, the topological structure rod diameter is prone to being damaged after subsequent heat treatment, the LMD technology is adopted, the high-temperature stable TiFeCu dealloying topological structure rod diameter is obtained by adjusting the dealloying temperature and time of the LMD process on the premise that the complete topological structure is guaranteed, and the method is suitable for large-scale industrial production. And the diameter of the de-alloying rod is regulated without changing the de-alloying topological structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of additive manufacturing, and in particular relates to a method for controlling the diameter of a dealloyed rod without changing a dealloyed topological structure. Background Art

[0002] In the prior art, the topological structure prepared by the chemical dealloying method has a very fine rod diameter (usually at the nanometer level), and its topological structure is often destroyed after subsequent heat treatment, such as Figure 1 As shown. Liquid metal dealloying (LMD) in a metal melt is a high-temperature process with the advantage of a high reaction rate. However, the significant increase in ligament diameter at high temperatures leads to a rough porous structure. This coarsening phenomenon is known to occur through the diffusion of thermally activated atoms. Therefore, in theory, lowering the dealloying temperature can effectively inhibit the coarsening.

[0003] For LMD, the minimum dealloying temperature is limited by the melting temperature of the molten pool metal. Even at this lower limit temperature, the rod diameter is usually in the submicron level, which is an order of magnitude larger than the rod diameter obtained when dealloying in a chemical solution. It is a technical challenge to obtain a thicker ligament structure while ensuring the integrity of the topological structure.

[0004] In the prior art, for example, patent document CN115921898A discloses a method for preparing porous copper by combining laser powder bed melting technology with dealloying method, wherein copper-containing powder is printed by laser powder bed melting technology, and a precursor material with designable macroscopic structure, uniform element distribution and density is obtained by adjusting parameters such as laser power, hatch spacing, scanning speed, etc., which is then immersed in an acid solution or an alkaline solution for dealloying to obtain a porous copper material with a controllable micropore-ligament double continuous network structure, and the additive manufacturing technology is used to realize the manufacture of complex structures and high-precision parts, and enhance the designability of the pore size and structure of the porous material. Patent document CN112126803A discloses a method for preparing a high entropy alloy nanoporous material, wherein the high entropy alloy master alloy is homogenized, cooled and then cold rolled, and subjected to liquid dealloying treatment or solid dealloying treatment. The process of liquid dealloying treatment is to mix the high entropy alloy master alloy strip with water and then conduct a hydrothermal reaction; the process of solid dealloying treatment is to roast the high entropy alloy master alloy strip under vacuum, and the obtained high entropy alloy nanoporous material has a uniform three-dimensional, open, and mutually permeable porous network structure with a porosity greater than 10%. It can be seen that a stable topological structure is a prerequisite for the performance stability of metamaterials. At present, there is no report on the use of LMD to control the rod diameter of the TiFeCu dealloyed topological structure to obtain a high-temperature stable dealloyed topological structure. Summary of the invention

[0005] In order to solve the problem that the diameter of the topological structure rod prepared by chemical dealloying in the prior art is extremely fine (usually at the nanometer level), which easily leads to the destruction of the topological structure after subsequent heat treatment, the purpose of the present invention is to provide a method for regulating the diameter of the dealloyed rod without changing the dealloyed topological structure, and the LMD technology is used to regulate the rod diameter of the TiFeCu dealloyed topological structure to obtain a high-temperature stable dealloyed topological structure.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention provides a method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure, comprising the following steps:

[0008] S1: Ti, Fe and Cu metal mixed powders were printed using laser powder bed fusion technology to produce TiFeCu precursor;

[0009] S2: The printed TiFeCu precursor is wire-cut and then placed in a vacuum tube furnace for liquid metal dealloying, wherein the molten pool metal is Mg, the temperature of the liquid metal dealloying is 800-850° C., and the time is 20-60 min, to obtain an LMD porous material containing a dealloyed topological structure;

[0010] S3: The LMD porous material is immersed in a nitric acid solution to remove the Mg solidified thereon.

[0011] Preferably, in step S1, the TiFeCu precursor consists of 35wt% Ti, 2wt% Fe and 63wt% Cu in terms of mass percentage.

[0012] Preferably, in step S1, the printing parameters include: laser power of 90 W, scanning speed of 1400 mm / s, lift amount of 0.03 mm, and track spacing of 0.08 mm.

[0013] Preferably, in step S2, the size of the sample after wire cutting is 2×2×4 mm.

[0014] Preferably, in step S2, the temperature of the liquid metal dealloying is 800° C. and the time is 60 min.

[0015] Preferably, in step S3, the concentration of the nitric acid solution is 2-4 mol / L, and the soaking time is 4-6 h.

[0016] More preferably, in step S3, the concentration of the nitric acid solution is 3 mol / L, and the immersion time is 5 h.

[0017] Preferably, in step S3, the average rod diameter of the dealloyed topological structure is 0.9-2.2 μm.

[0018] Compared with the prior art, the beneficial effect of the present invention is that: in order to solve the problem that the topological structure of the topological structure rod prepared by the chemical dealloying method is destroyed after subsequent heat treatment, the LMD technology is adopted to adjust the dealloying temperature and time of the LMD process while ensuring the complete topological structure, so as to control the rod diameter of the TiFeCu dealloying topological structure, obtain a high-temperature stable dealloying topological structure, and realize the control of the dealloying rod diameter without changing the dealloying topological structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a fracture morphology diagram of the CuMn alloy after chemical dealloying in the prior art.

[0020] Figure 2 The following are pictures of the actual printed TiFeCu precursor and experimental equipment in the examples.

[0021] Figure 3 This is a composition distribution diagram of the printed TiFeCu precursor in the embodiment.

[0022] Figure 4 The fracture morphology and ligament diameter distribution diagram of the LMD porous material at different dealloying temperatures and times in the embodiment.

[0023] Figure 5 This is the EDS analysis of the fracture of the LMD porous material at different dealloying temperatures and times in the example.

[0024] Figure 6 The mechanical properties of the LMD porous material change at different dealloying temperatures and times in the examples. DETAILED DESCRIPTION

[0025] In order to more fully understand and demonstrate the technical solutions, purposes and advantages of the present invention, the technical effects produced by the present invention are further described in detail and completely in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all. It should be pointed out that for those of ordinary skill in the art, other embodiments obtained without departing from the concept of the present invention all belong to the protection scope of the present invention.

[0026] Example 1

[0027] This embodiment proposes a method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure, and the steps are as follows:

[0028] S1: Laser powder bed fusion technology is used to prepare Ti 35 Fe2Cu 63The dealloyed precursor, wherein the printing parameters are as follows: laser power: 90 W; scanning speed: 1400 mm / s; lift: 0.03 mm; track spacing: 0.08 mm.

[0029] S2: Against Ti 35 Fe2Cu 63 The dealloyed precursor composition is characterized, such as Figure 3 As shown, it can be seen that there is segregation, and the actual composition is Ti 57 Fe2Cu 41 .

[0030] S3: The printed precursor was cut into 2×2×4 mm samples by wire cutting technology and placed in a vacuum tube furnace for liquid metal dealloying to obtain LMD porous materials. The LMD process was: 800°C, 20 min.

[0031] S4: The dealloyed LMD porous material was immersed in a 3 mol / L nitric acid solution for 5 h to remove the Mg solidified on the porous material.

[0032] S5: Scanning electron microscopy was used to characterize the fracture morphology and composition of LMD porous material samples, such as Figure 4 a. Figure 5 As shown in a, the Cu element in the alloy system and the residual Mg element in the LMD process are completely removed and the topological structure is intact, where the average rod diameter of the topological structure is 0.96 μm.

[0033] S6: Compression performance tests were performed on LMD porous material samples under different process conditions to evaluate their mechanical properties, and the maximum compressive stress was 60.5 MPa.

[0034] Example 2

[0035] This embodiment proposes a method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure, and the steps are as follows:

[0036] S1: Laser powder bed fusion technology is used to prepare Ti 35 Fe2Cu 63 The dealloyed precursor, wherein the printing parameters are as follows: laser power: 90 W; scanning speed: 1400 mm / s; lift: 0.03 mm; track spacing: 0.08 mm.

[0037] S2: Against Ti 35 Fe2Cu 63 The dealloyed precursor composition is characterized, such as Figure 3 As shown, it can be seen that there is segregation, and the actual composition is Ti 57 Fe2Cu 41 .

[0038] S3: The printed precursor was cut into 2×2×4 mm samples by wire cutting technology and placed in a vacuum tube furnace for liquid metal dealloying to obtain LMD porous materials. The LMD process was: 800°C, 60 min.

[0039] S4: The dealloyed LMD porous material was immersed in a 3 mol / L nitric acid solution for 5 h to remove the Mg solidified on the porous material.

[0040] S5: Scanning electron microscopy was used to characterize the fracture morphology and composition of LMD porous material samples, such as Figure 4 b. Figure 5 As shown in b, the Cu element in the alloy system and the residual Mg element in the LMD process are completely removed and the topological structure is intact, with the average rod diameter of the topological structure being 1.22 μm.

[0041] S6: Compression performance tests were performed on LMD porous material samples under different process conditions to evaluate their mechanical properties, and the maximum compressive stress was 48.7 MPa.

[0042] Example 3

[0043] This embodiment proposes a method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure, and the steps are as follows:

[0044] S1: Laser powder bed fusion technology is used to prepare Ti 35 Fe2Cu 63 The dealloyed precursor, wherein the printing parameters are as follows: laser power: 90 W; scanning speed: 1400 mm / s; lift: 0.03 mm; track spacing: 0.08 mm.

[0045] S2: Against Ti 35 Fe2Cu 63 The dealloyed precursor composition is characterized, such as Figure 3 As shown, it can be seen that there is segregation, and the actual composition is Ti 57 Fe2Cu 41 .

[0046] S3: The printed precursor was cut into 2×2×4 mm samples by wire cutting technology and placed in a vacuum tube furnace for liquid metal dealloying to obtain LMD porous materials. The LMD process was: 850°C, 60 min.

[0047] S4: The dealloyed LMD porous material was immersed in a 3 mol / L nitric acid solution for 5 h to remove the Mg solidified on the porous material.

[0048] S5: Scanning electron microscopy was used to characterize the fracture morphology and composition of LMD porous material samples, such as Figure 4 c. Figure 5 As shown in c, the Cu element in the alloy system and the residual Mg element in the LMD process are completely removed and the topological structure is intact, where the average rod diameter of the topological structure is 2.10 μm.

[0049] S6: Compression tests were performed on LMD porous material specimens under different process conditions to evaluate their mechanical properties, with a maximum compressive stress of 45 MPa.

[0050] like Figure 5 As shown, the EDS analysis of the fracture of the LMD porous materials in Examples 1 to 3 shows that the Cu element in the alloy system and the Mg introduced in the LMD process are completely removed.

[0051] like Figure 6 As shown, from the changes in the mechanical properties of the LMD porous materials in Examples 1 to 3, it can be seen that with the increase of the LMD temperature and the extension of the holding time, the mechanical properties of the dealloyed rods after coarsening tend to decrease, which are 60.5, 48.7, and 45 MPa, respectively, but their topological structures remain intact.

[0052] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure, characterized in that: The following steps are involved: S1: Ti, Fe and Cu metal mixed powders were printed using laser powder bed fusion technology to produce TiFeCu precursor; S2: The printed TiFeCu precursor is wire-cut and then placed in a vacuum tube furnace for liquid metal dealloying, wherein the molten pool metal is Mg, the temperature of the liquid metal dealloying is 800-850° C., and the time is 20-60 min, to obtain an LMD porous material containing a dealloyed topological structure; S3: The LMD porous material is immersed in a nitric acid solution to remove the Mg solidified thereon.

2. The method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure according to claim 1, characterized in that: In step S1, the TiFeCu precursor consists of 35wt% Ti, 2wt% Fe and 63wt% Cu in terms of mass percentage.

3. The method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure according to claim 1, characterized in that: In step S1, the printing parameters include: laser power of 90W, scanning speed of 1400mm / s, lift amount of 0.03mm, and track spacing of 0.08mm.

4. The method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure according to claim 1, characterized in that: In step S2, the size of the sample after wire cutting is 2×2×4 mm.

5. The method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure according to claim 1, characterized in that: In step S2, the temperature of the liquid metal dealloying is 800° C. and the time is 60 minutes.

6. The method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure according to claim 1, characterized in that: In step S3, the concentration of the nitric acid solution is 2-4 mol / L, and the soaking time is 4-6 hours.

7. The method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure according to claim 6, characterized in that: In step S3, the concentration of the nitric acid solution is 3 mol / L, and the soaking time is 5 h.

8. The method for controlling the diameter of a dealloyed rod without changing the dealloyed topological structure according to claim 1, characterized in that: In step S3, the average rod diameter of the dealloyed topological structure is 0.9-2.2 μm.

Citation Information

Patent Citations

  • Preparation method of high-entropy alloy nano-porous material

    CN112126803A

  • Method for preparing porous copper through combination of laser powder bed melting technology and dealloying method

    CN115921898A