Ceramic blank containing lithium tailings and ceramic tile using ceramic blank
By adjusting the ratio of white mud, bauxite and kaolin in the ceramic blank formulation, combining lithium tailings and waste mud slag, optimizing the silicon-aluminum ratio and the addition of magnesium soil and wollastonite, the ceramics caused by lithium tailings are solved. Reduced brick strength and crack problems improve whiteness and reduce production costs.
Patent Information
- Application Number
- CN202411042118.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The large addition of lithium tailings in ceramic blank formulations leads to reduced strength of ceramic tiles and structural cracks, and is difficult to effectively utilize, affecting its whiteness and production costs.
By adjusting the addition amount of white mud, bauxite and raw ore kaolin in the ceramic blank formulation, combining lithium tailings, waste mud slag and other raw materials, the silicon-aluminum ratio and the ratio of magnesium soil and wollastonite are optimized, and firing is controlled. after shrinkage and whiteness.
The large-scale use of lithium tailings has been achieved without affecting the shrinkage and strength of ceramic tiles, which improves the whiteness of ceramic tiles and reduces production costs.
Smart Images

Figure BDA0004972649430000081 
Figure BDA0004972649430000091 
Figure BDA0004972649430000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building ceramics, and in particular to a ceramic blank containing lithium tailings and a ceramic brick using the same. Background Art
[0002] Lithium tailings, as industrial waste residues generated in the production process of lithium materials, are closely related to the rapid development of the lithium materials industry. For every ton of lithium carbonate produced, eight to ten tons of lithium tailings will be produced. With the surge in market demand for lithium materials, the output of lithium tailings has also increased year by year. However, the utilization value of lithium tailings itself is low, and it is forced to be stored because it is difficult to use effectively. This treatment method not only occupies a large amount of land resources, but also poses a potential threat to the ecological environment.
[0003] Therefore, the efficient utilization and proper treatment of lithium tailings have become an urgent problem to be solved. Since lithium tailings contain potassium oxide and sodium oxide, which have a fluxing effect, they have a good fluxing effect. In order to reduce the production cost of ceramic tiles and improve the utilization rate of lithium tailings, the existing technology adds lithium tailings to the ceramic blank formula, utilizes the fluxing effect of lithium tailings, reduces the calcination temperature and calcination time of the ceramic blank, realizes low-cost, green production, and improves the competitiveness of ceramic products.
[0004] However, due to the limitations of the performance of lithium tailings, the large amount of lithium tailings added to the formula will easily reduce the strength of ceramic tiles. Specifically, the large amount of lithium tailings added to the formula also means that the content of potassium oxide and sodium oxide in the ceramic blank formula is relatively high. Since potassium oxide and sodium oxide have large thermal expansion coefficients, the large amount of lithium tailings used will easily lead to excessive shrinkage during the calcination of the ceramic blank, resulting in cracks in the fired ceramic blank, affecting its structural strength. Summary of the invention
[0005] The purpose of the present invention is to propose a ceramic blank containing lithium tailings and a ceramic tile using the same, which can realize the large-scale use of lithium tailings while ensuring that the shrinkage rate of the ceramic tile meets the production requirements, and is also beneficial to improving the whiteness of the ceramic tile, so as to overcome the shortcomings of the prior art.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] A ceramic blank containing lithium tailings includes the following raw materials in parts by mass: 15 to 40 parts of potassium-sodium feldspar, 15 to 34 parts of waste mud, 0 to 5 parts of bauxite, 0 to 5 parts of magnesia soil, 0 to 10 parts of white mud, 0 to 10 parts of bentonite, 2 to 13 parts of raw kaolin, 10 to 35 parts of lithium tailings and 0 to 10 parts of wollastonite;
[0008] According to mass percentage, the Li2O content of the lithium tailings is 0.2-3%.
[0009] Preferably, the particle size of the lithium tailings is ≤0.6 mm.
[0010] Preferably, the lithium tailings include the following chemical components in terms of mass percentage: SiO2 65-75%, Al2O3 15-25%, Fe2O3 0-0.5%, TiO2 0-0.1%, CaO 0-1%, MgO 0-1%, K2O 1-5%, Na2O 1-10% and Li2O 0.2-3%, with the remainder being loss on ignition.
[0011] Preferably, the waste mud residue includes recycled waste brick powder, recycled polishing residue, recycled pressure mud and field core mixed mud;
[0012] In terms of mass proportions, the following raw materials are included: 15-40 parts of potassium and sodium feldspar, 5-10 parts of recycled waste brick powder, 3-7 parts of recycled polishing slag, 2-7 parts of recycled compressed mud, 5-10 parts of field mixed mud, 0-5 parts of bauxite, 0-5 parts of magnesia clay, 0-10 parts of white mud, 0-10 parts of bentonite, 2-13 parts of raw kaolin, 10-35 parts of lithium tailings and 0-10 parts of wollastonite.
[0013] Preferably, the recycled waste brick powder comprises the following chemical components in terms of mass percentage: SiO2 73.27%, Al2O3 17.64%, Fe2O3 1.42%, TiO2 0.26%, CaO 0.74%, MgO 0.73%, K2O 2.63% and Na2O1.66%, with the remainder being loss on ignition;
[0014] The recycled polishing slag includes the following chemical components in terms of mass percentage: SiO2 68.90%, Al2O3 19.13%, Fe2O3 1.24%, TiO2 0.22%, CaO 2.40%, MgO 1.20%, K2O 3.04% and Na2O2.22%, with the remainder being loss on ignition;
[0015] The recycled compressed mud includes the following chemical components in terms of mass percentage: SiO2 73.25%, Al2O3 17.38%, Fe2O3 1.52%, TiO2 0.29%, CaO 0.94%, MgO 0.53%, K2O 2.42% and Na2O 1.85%, and the rest is loss on ignition;
[0016] According to mass percentage, the field core mixed mud includes the following chemical components: SiO2 66.60%, Al2O3 21.08%, Fe2O3 1.81%, TiO2 0.38%, CaO 0.14%, MgO 0.22%, K2O 2.09% and Na2O 0.56%, and the rest is ignition loss.
[0017] Preferably, the kaolinite includes Tianhong clay and Shuangjiang clay;
[0018] In terms of mass proportions, the following raw materials are included: 15-40 parts of potassium-sodium feldspar, 5-10 parts of recycled waste brick powder, 3-7 parts of recycled polishing slag, 2-7 parts of recycled compressed mud, 5-10 parts of field mixed mud, 0-5 parts of bauxite, 0-5 parts of magnesia clay, 0-10 parts of white mud, 0-10 parts of bentonite, 2-10 parts of Tianhong mud, 0-3 parts of Shuangjiang mud, 10-35 parts of lithium tailings and 0-10 parts of wollastonite.
[0019] Preferably, the Tianhong mud comprises the following chemical components in terms of mass percentage: SiO2 68.33%, Al2O3 20.17%, Fe2O3 1.68%, TiO2 0.19%, CaO 0.19%, MgO 0.22%, K2O 2.04% and Na2O 0.57%, and the rest is loss on ignition;
[0020] According to mass percentage, the Shuangjiang mud includes the following chemical components: SiO2 64.43%, Al2O3 22.42%, Fe2O3 1.80%, TiO2 0.32%, CaO 0.09%, MgO 0.29%, K2O 1.95% and Na2O 0.34%, and the rest is loss on ignition.
[0021] Preferably, the bauxite comprises the following chemical components in terms of mass percentage: SiO2 32.01%, Al2O3 47.52%, Fe2O3 2.86% and loss on ignition 13.40%;
[0022] The magnesia soil comprises the following chemical components in terms of mass percentage: SiO2 62.12%, Al2O3 0.36%, Fe2O3 0.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, with the remainder being loss on ignition;
[0023] The white mud comprises the following chemical components in terms of mass percentage: SiO2 51.61%, Al2O3 30.10%, Fe2O3 1.88%, TiO2 0.16%, CaO 0.17%, MgO 0.24%, K2O 3.52% and Na2O 0.88%, with the remainder being loss on ignition;
[0024] The bentonite comprises the following chemical components in terms of mass percentage: SiO2 73.40%, Al2O3 16.20%, Fe2O3 1.63%, TiO2 0.27%, CaO 0.20%, MgO 0.31%, K2O 2.36% and Na2O 0.48%, with the remainder being loss on ignition.
[0025] In terms of weight percentage, a ceramic green body containing lithium tailings includes the following raw materials: 24 parts of potassium and sodium feldspar, 7.5 parts of recycled waste brick powder, 4.5 parts of recycled polishing slag, 4 parts of recycled compressed mud, 6 parts of Tianxin mixed mud, 5 parts of bauxite, 2.5 parts of magnesia clay, 6 parts of white mud, 2 parts of bentonite, 5.5 parts of Tianhong mud, 3 parts of Shuangjiang mud, 25 parts of lithium tailings and 5 parts of wollastonite.
[0026] A ceramic tile is prepared using the ceramic blank containing lithium tailings, and the whiteness of the ceramic tile is greater than 20°.
[0027] The technical solution provided by the present invention may include the following beneficial effects:
[0028] 1. In order to ensure that the shrinkage rate of ceramic tiles meets the production requirements and realize the large-scale use of lithium tailings, this scheme proposes a ceramic green body containing lithium tailings. In order to balance the technical problem of excessive expansion coefficient of the green body caused by the large amount of lithium tailings added, this scheme adjusts the addition amount of white mud, bauxite and raw kaolin in the formula, thereby adjusting the silicon-aluminum ratio in the formula system, and the whiteness can also be appropriately improved; in addition, this scheme also adjusts the addition amount of magnesia clay and wollastonite containing magnesium and calcium elements in the formula, so as to adjust the shrinkage rate of the green body after firing, thereby solving the technical problem that the large-scale use of lithium tailings easily leads to excessive shrinkage of the ceramic green body during the calcination process, resulting in cracks in the ceramic green body after firing, affecting its structural strength.
[0029] 2. After the formula structure of this scheme is adjusted, a large amount of waste mud can be introduced into the raw material formula and used together with lithium tailings as the main raw material of ceramic blanks, which greatly reduces the preparation cost of ceramic blanks. DETAILED DESCRIPTION
[0030] A ceramic blank containing lithium tailings, comprising the following raw materials by weight: 15-40 parts of potassium-sodium feldspar, 15-34 parts of waste mud, 0-5 parts of bauxite, 0-5 parts of magnesia clay, 0-10 parts of white mud, 0-10 parts of bentonite, 2-13 parts of raw kaolin, 10-35 parts of lithium tailings and 0-10 parts of wollastonite;
[0031] According to mass percentage, the Li2O content of the lithium tailings is 0.2-3%.
[0032] Due to the limitations of the performance of lithium tailings, the large amount of lithium tailings added to the formula will easily reduce the strength of ceramic tiles. Specifically, the large amount of lithium tailings added to the formula also means that the content of potassium oxide and sodium oxide in the ceramic blank formula is relatively high. Since potassium oxide and sodium oxide have large thermal expansion coefficients, the large amount of lithium tailings used will easily lead to excessive shrinkage during the calcination of the ceramic blank, resulting in cracks in the fired ceramic blank, affecting its structural strength.
[0033] Therefore, in order to ensure that the shrinkage rate of ceramic tiles meets the production requirements and to achieve the large-scale use of lithium tailings, this scheme proposes a ceramic green body containing lithium tailings. In order to balance the technical problem of excessive expansion coefficient of the green body caused by the large-scale addition of lithium tailings, this scheme adjusts the addition amount of white mud, bauxite and raw kaolin in the formula, thereby adjusting the silicon-aluminum ratio in the formula system, and the whiteness can also be appropriately improved; in addition, this scheme also adjusts the addition amount of magnesia clay and wollastonite containing magnesium and calcium elements in the formula, so as to adjust the shrinkage rate of the green body after firing, thereby solving the technical problem that the large-scale use of lithium tailings easily leads to excessive shrinkage of the ceramic green body during the calcination process, resulting in cracks in the ceramic green body after firing, affecting its structural strength.
[0034] In addition, after the formula structure of this solution is adjusted, a large amount of waste mud can be introduced into the raw material formula and used together with lithium tailings as the main raw material of ceramic green materials, which greatly reduces the preparation cost of ceramic green materials.
[0035] Further, the particle size of the lithium tailings is ≤0.6 mm. The present invention also optimizes the particle size of the lithium tailings, and the lithium tailings with the above particle size are easier to ball mill.
[0036] To further illustrate, the lithium tailings include the following chemical components in terms of mass percentage: SiO2 65-75%, Al2O3 15-25%, Fe2O3 0-0.5%, TiO2 0-0.1%, CaO 0-1%, MgO 0-1%, K2O 1-5%, Na2O 1-10% and Li2O 0.2-3%, with the remainder being loss on ignition.
[0037] Preferably, the lithium tailings include the following chemical components in mass percentage: SiO2 69.56%, Al2O3 18.7%, Fe2O3 0.48%, TiO2 0.06%, CaO 0.88%, MgO 0.21%, K2O 2.72%, Na2O 4.22% and Li2O 0.27%, and the rest is loss on ignition.
[0038] Further, the waste mud residue includes recycled waste brick powder, recycled polishing residue, recycled pressure mud and field mixed mud;
[0039] In terms of mass proportions, the following raw materials are included: 15-40 parts of potassium and sodium feldspar, 5-10 parts of recycled waste brick powder, 3-7 parts of recycled polishing slag, 2-7 parts of recycled compressed mud, 5-10 parts of field mixed mud, 0-5 parts of bauxite, 0-5 parts of magnesia clay, 0-10 parts of white mud, 0-10 parts of bentonite, 2-13 parts of raw kaolin, 10-35 parts of lithium tailings and 0-10 parts of wollastonite.
[0040] In a preferred embodiment of the present technical solution, the waste mud residue used in the present solution may include recycled materials commonly found in the ceramic field, namely, recycled waste brick powder, recycled polishing residue and recycled pressed mud, which is beneficial to saving the processing cost of recycled materials and further reducing the production cost of ceramic blanks.
[0041] It is further explained that the recycled waste brick powder includes the following chemical components in terms of mass percentage: SiO2 73.27%, Al2O3 17.64%, Fe2O3 1.42%, TiO2 0.26%, CaO 0.74%, MgO 0.73%, K2O2.63% and Na2O 1.66%, with the remainder being loss on ignition;
[0042] The recycled polishing slag includes the following chemical components in terms of mass percentage: SiO2 68.90%, Al2O3 19.13%, Fe2O3 1.24%, TiO2 0.22%, CaO 2.40%, MgO 1.20%, K2O 3.04% and Na2O2.22%, with the remainder being loss on ignition;
[0043] The recycled compressed mud includes the following chemical components in terms of mass percentage: SiO2 73.25%, Al2O3 17.38%, Fe2O3 1.52%, TiO2 0.29%, CaO 0.94%, MgO 0.53%, K2O 2.42% and Na2O 1.85%, and the rest is loss on ignition;
[0044] According to mass percentage, the field core mixed mud includes the following chemical components: SiO2 66.60%, Al2O3 21.08%, Fe2O3 1.81%, TiO2 0.38%, CaO 0.14%, MgO 0.22%, K2O 2.09% and Na2O 0.56%, and the rest is ignition loss.
[0045] It is further explained that the raw kaolin includes Tianhong clay and Shuangjiang clay;
[0046] In terms of mass proportions, the following raw materials are included: 15-40 parts of potassium-sodium feldspar, 5-10 parts of recycled waste brick powder, 3-7 parts of recycled polishing slag, 2-7 parts of recycled compressed mud, 5-10 parts of field mixed mud, 0-5 parts of bauxite, 0-5 parts of magnesia clay, 0-10 parts of white mud, 0-10 parts of bentonite, 2-10 parts of Tianhong mud, 0-3 parts of Shuangjiang mud, 10-35 parts of lithium tailings and 0-10 parts of wollastonite.
[0047] In a more preferred embodiment of the present technical solution, adding two raw kaolins with different chemical compositions to adjust the silicon-aluminum ratio in the formula is more conducive to stabilizing the quality of the green body after firing.
[0048] Further, according to the mass percentage, the Tianhong mud includes the following chemical components: SiO2 68.33%, Al2O3 20.17%, Fe2O3 1.68%, TiO2 0.19%, CaO 0.19%, MgO 0.22%, K2O2.04% and Na2O0.57%, and the rest is the loss on ignition;
[0049] According to mass percentage, the Shuangjiang mud includes the following chemical components: SiO2 64.43%, Al2O3 22.42%, Fe2O3 1.80%, TiO2 0.32%, CaO 0.09%, MgO 0.29%, K2O 1.95% and Na2O 0.34%, and the rest is loss on ignition.
[0050] Further, the bauxite comprises the following chemical components in terms of mass percentage: SiO2 32.01%, Al2O3 47.52%, Fe2O3 2.86% and loss on ignition 13.40%;
[0051] The magnesia soil comprises the following chemical components in terms of mass percentage: SiO2 62.12%, Al2O3 0.36%, Fe2O3 0.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, with the remainder being loss on ignition;
[0052] The white mud comprises the following chemical components in terms of mass percentage: SiO2 51.61%, Al2O3 30.10%, Fe2O3 1.88%, TiO2 0.16%, CaO 0.17%, MgO 0.24%, K2O 3.52% and Na2O 0.88%, with the remainder being loss on ignition;
[0053] The bentonite comprises the following chemical components in terms of mass percentage: SiO2 73.40%, Al2O3 16.20%, Fe2O3 1.63%, TiO2 0.27%, CaO 0.20%, MgO 0.31%, K2O 2.36% and Na2O 0.48%, with the remainder being loss on ignition.
[0054] To further explain, a ceramic green body containing lithium tailings includes the following raw materials, in terms of mass percentage: 24 parts of potassium and sodium feldspar, 7.5 parts of recycled waste brick powder, 4.5 parts of recycled polishing slag, 4 parts of recycled compressed mud, 6 parts of Tianxin mixed mud, 5 parts of bauxite, 2.5 parts of magnesia clay, 6 parts of white mud, 2 parts of bentonite, 5.5 parts of Tianhong mud, 3 parts of Shuangjiang mud, 25 parts of lithium tailings and 5 parts of wollastonite.
[0055] The technical solution also provides an optimal formula for a ceramic blank containing lithium tailings, the whiteness of the ceramic blank after firing can reach 23.3°, and the shrinkage rate is 10.52, and it is not easy to crack.
[0056] A ceramic tile is prepared using the ceramic blank containing lithium tailings, and the whiteness of the ceramic tile is greater than 20°.
[0057] This solution can ensure that the shrinkage rate of ceramic tiles meets the production requirements, realize the large-scale use of lithium tailings, and is also beneficial to improve the whiteness of ceramic tiles to overcome the shortcomings of the existing technology.
[0058] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0059] Example Group
[0060] Ceramic blanks were prepared according to the raw material formula in Table 1, and ceramic tiles were obtained after pressing and firing. The conventional shrinkage and whiteness tests in the field of building ceramics were performed on the ceramic tiles of each embodiment, and the results are shown in Table 2.
[0061] Table 1 Raw material formula of ceramic blank containing lithium tailings
[0062]
[0063]
[0064] in:
[0065] The recycled waste brick powder includes the following chemical components in terms of mass percentage: SiO2 73.27%, Al2O3 17.64%, Fe2O3 1.42%, TiO2 0.26%, CaO 0.74%, MgO 0.73%, K2O 2.63% and Na2O 1.66%, with the rest being loss on ignition.
[0066] The recovered polishing slag includes the following chemical components according to mass percentage: SiO2 68.90%, Al2O3 19.13%, Fe2O3 1.24%, TiO2 0.22%, CaO 2.40%, MgO 1.20%, K2O 3.04% and Na2O 2.22%, and the rest is loss on ignition.
[0067] According to mass percentage, the recycled compressed mud includes the following chemical components: SiO2 73.25%, Al2O3 17.38%, Fe2O3 1.52%, TiO2 0.29%, CaO 0.94%, MgO 0.53%, K2O 2.42% and Na2O 1.85%, and the rest is loss on ignition.
[0068] According to mass percentage, Tianxin mixed mud includes the following chemical components: SiO2 66.60%, Al2O3 21.08%, Fe2O3 1.81%, TiO2 0.38%, CaO 0.14%, MgO 0.22%, K2O 2.09% and Na2O 0.56%, and the rest is loss on ignition.
[0069] In terms of mass percentage, bauxite includes the following chemical components: SiO2 32.01%, Al2O3 47.52%, Fe2O3 2.86% and loss on ignition 13.40%.
[0070] According to mass percentage, magnesia soil includes the following chemical components: SiO2 62.12%, Al2O3 0.36%, Fe2O30.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, and the rest is loss on ignition.
[0071] In terms of mass percentage, white mud includes the following chemical components: SiO2 51.61%, Al2O3 30.10%, Fe2O31.88%, TiO2 0.16%, CaO 0.17%, MgO 0.24%, K2O 3.52% and Na2O 0.88%, and the rest is loss on ignition.
[0072] In terms of mass percentage, bentonite includes the following chemical components: SiO2 73.40%, Al2O3 16.20%, Fe2O3 1.63%, TiO2 0.27%, CaO 0.20%, MgO 0.31%, K2O 2.36% and Na2O 0.48%, with the rest being loss on ignition.
[0073] In terms of mass percentage, Tianhong clay includes the following chemical components: SiO2 68.33%, Al2O3 20.17%, Fe2O31.68%, TiO2 0.19%, CaO 0.19%, MgO 0.22%, K2O 2.04% and Na2O 0.57%, and the rest is loss on ignition.
[0074] According to mass percentage, Shuangjiang mud includes the following chemical components: SiO2 64.43%, Al2O3 22.42%, Fe2O31.80%, TiO2 0.32%, CaO 0.09%, MgO 0.29%, K2O 1.95% and Na2O 0.34%, and the rest is loss on ignition.
[0075] Table 2 Test items for ceramic tiles fired from ceramic blanks containing lithium tailings
[0076]
[0077]
[0078] From the test results in Table 2, it can be seen that this solution can ensure that the shrinkage rate of ceramic tiles meets the production requirements and realize the large-scale use of lithium tailings. At the same time, the whiteness of the ceramic tiles is greater than 20°, thereby overcoming the shortcomings of the prior art.
[0079] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A ceramic blank containing lithium tailings, characterized in that: The raw materials include, by weight: 15-40 parts of potassium-sodium feldspar, 15-34 parts of waste sludge, 0-5 parts of bauxite, 0-5 parts of magnesia soil, 0-10 parts of white mud, 0-10 parts of bentonite, 2-13 parts of raw kaolin, 10-35 parts of lithium tailings and 0-10 parts of wollastonite; According to mass percentage, the Li2O content of the lithium tailings is 0.2-3%.
2. A ceramic blank containing lithium tailings according to claim 1, characterized in that: The particle size of the lithium tailings is ≤0.6 mm.
3. A ceramic blank containing lithium tailings according to claim 1, characterized in that: According to mass percentage, the lithium tailings include the following chemical components: SiO2 65-75%, Al2O3 15-25%, Fe2O30-0.5%, TiO2 0-0.1%, CaO 0-1%, MgO 0-1%, K2O 1-5%, Na2O 1-10% and Li2O 0.2-3%, and the rest is ignition loss.
4. A ceramic blank containing lithium tailings according to claim 1, characterized in that: The waste mud residue includes recycled waste brick powder, recycled polishing residue, recycled pressure mud and field mixed mud; In terms of mass proportions, the following raw materials are included: 15-40 parts of potassium and sodium feldspar, 5-10 parts of recycled waste brick powder, 3-7 parts of recycled polishing slag, 2-7 parts of recycled compressed mud, 5-10 parts of field mixed mud, 0-5 parts of bauxite, 0-5 parts of magnesia clay, 0-10 parts of white mud, 0-10 parts of bentonite, 2-13 parts of raw kaolin, 10-35 parts of lithium tailings and 0-10 parts of wollastonite.
5. A ceramic blank containing lithium tailings according to claim 4, characterized in that: The recycled waste brick powder includes the following chemical components in terms of mass percentage: SiO2 73.27%, Al2O3 17.64%, Fe2O3 1.42%, TiO2 0.26%, CaO 0.74%, MgO 0.73%, K2O 2.63% and Na2O 1.66%, with the remainder being loss on ignition; The recycled polishing slag includes the following chemical components in terms of mass percentage: SiO2 68.90%, Al2O3 19.13%, Fe2O3 1.24%, TiO2 0.22%, CaO 2.40%, MgO 1.20%, K2O 3.04% and Na2O 2.22%, with the remainder being loss on ignition; The recycled compressed mud includes the following chemical components in terms of mass percentage: SiO2 73.25%, Al2O3 17.38%, Fe2O3 1.52%, TiO2 0.29%, CaO 0.94%, MgO 0.53%, K2O 2.42% and Na2O 1.85%, and the rest is loss on ignition; According to mass percentage, the field core mixed mud includes the following chemical components: SiO2 66.60%, Al2O3 21.08%, Fe2O3 1.81%, TiO2 0.38%, CaO 0.14%, MgO 0.22%, K2O 2.09% and Na2O 0.56%, and the rest is ignition loss.
6. A ceramic blank containing lithium tailings according to claim 4, characterized in that: The raw kaolin includes Tianhong clay and Shuangjiang clay; In terms of mass proportions, the following raw materials are included: 15-40 parts of potassium-sodium feldspar, 5-10 parts of recycled waste brick powder, 3-7 parts of recycled polishing slag, 2-7 parts of recycled compressed mud, 5-10 parts of field mixed mud, 0-5 parts of bauxite, 0-5 parts of magnesia clay, 0-10 parts of white mud, 0-10 parts of bentonite, 2-10 parts of Tianhong mud, 0-3 parts of Shuangjiang mud, 10-35 parts of lithium tailings and 0-10 parts of wollastonite.
7. A ceramic blank containing lithium tailings according to claim 6, characterized in that: According to mass percentage, the Tianhong mud includes the following chemical components: SiO2 68.33%, Al2O3 20.17%, Fe2O31.68%, TiO2 0.19%, CaO 0.19%, MgO 0.22%, K2O 2.04% and Na2O 0.57%, and the rest is loss on ignition; According to mass percentage, the Shuangjiang mud includes the following chemical components: SiO2 64.43%, Al2O3 22.42%, Fe2O31.80%, TiO2 0.32%, CaO 0.09%, MgO 0.29%, K2O 1.95% and Na2O 0.34%, and the rest is loss on ignition.
8. A ceramic blank containing lithium tailings according to claim 1, characterized in that: The bauxite comprises the following chemical components in terms of mass percentage: SiO2 32.01%, Al2O3 47.52%, Fe2O3 2.86% and loss on ignition 13.40%; The magnesia soil comprises the following chemical components in terms of mass percentage: SiO2 62.12%, Al2O3 0.36%, Fe2O3 0.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, with the remainder being loss on ignition; The white mud comprises the following chemical components in terms of mass percentage: SiO2 51.61%, Al2O3 30.10%, Fe2O31.88%, TiO2 0.16%, CaO 0.17%, MgO 0.24%, K2O 3.52% and Na2O 0.88%, with the remainder being loss on ignition; The bentonite comprises the following chemical components in percentage by mass: SiO2 73.40%, Al2O3 16.20%, Fe2O3 1.63%, TiO2 0.27%, CaO 0.20%, MgO 0.31%, K2O 2.36% and Na2O 0.48%, with the remainder being loss on ignition.
9. A ceramic blank containing lithium tailings according to claim 6, characterized in that: In terms of mass, the raw materials include: 24 parts of potassium and sodium feldspar, 7.5 parts of recycled waste brick powder, 4.5 parts of recycled polishing slag, 4 parts of recycled compressed mud, 6 parts of Tianxin mixed mud, 5 parts of bauxite, 2.5 parts of magnesia clay, 6 parts of white mud, 2 parts of bentonite, 5.5 parts of Tianhong mud, 3 parts of Shuangjiang mud, 25 parts of lithium tailings and 5 parts of wollastonite.
10. A ceramic tile, characterized in that: The ceramic brick is prepared using the ceramic blank containing lithium tailings as described in any one of claims 1 to 9, and the whiteness of the ceramic brick is greater than 20°.
Citation Information
Patent Citations
Lightweight high-strength foamed ceramic plate and preparation method thereof
CN109133975A
Ceramic green body, ceramic tile and preparation method of ceramic green body
CN115893978A
Ceramic blank based on lithium slag, ceramic green body, ceramic tile and preparation method of ceramic blank
CN116715506A
Ceramic blank, ceramic body, ceramic rock plate and preparation method thereof
CN116813307A
Sinterable and / or fusible ceramic mass, production and use thereof
US20160058558A1
Cited By