Synthesis method and application of tetraoxacycloalkene-based lithium extraction membrane electrode material
By using tetraoxycycloene porous membrane electrode material, the problem of structural changes in the traditional positive electrode material during the lithium ion embedding and detachment process is solved, efficient lithium ion adsorption and desorption are achieved, and the stability and circulation efficiency of the material are improved. Reduces potential demand and useless energy consumption.
Patent Information
- Application Number
- CN202411042910.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The crystal structure changes of traditional inorganic positive electrode materials during the lithium ion embedding and disengagement process lead to low stability and cycling efficiency, and insufficient conductivity. The electrode surface voltage needs to be increased to meet the minimum de-embedding potential of the electrode, resulting in useless energy consumption.
Using a porous membrane electrode material based on tetraoxycycloene, a planar fully conjugated porous structure with a D4h symmetric point group is used to precisely control the adsorption and desorption process of lithium ions through electrostatic force, avoid crystal structure changes and improve conductivity.
It significantly improves the adsorption capacity and adsorption and desorption efficiency of lithium ions, avoids crystal structure collapse, improves the stability and cycling efficiency of materials, reduces potential demand, and reduces useless energy consumption.
Smart Images

Figure CN118978688A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a lithium extraction membrane electrode material based on tetraoxocycloolefin polymer, a synthesis method and application thereof, and belongs to the technical field of polymer materials and lithium extraction from salt lakes. Background Art
[0002] Compared with lithium extraction from ore, lithium extraction from salt lakes has the advantages of low production cost and environmental friendliness, so it occupies an important position in the development of global lithium resources. However, the level of development and utilization of lithium resources in my country's salt lakes is low, and the salt lake lithium extraction industry accounts for only about 10% of the world's lithium salt industry. The main reasons for this situation are the technical barriers to lithium extraction from salt lakes and the constraints of the geographical and ecological environment. For this reason, it is urgent to develop new salt lake lithium extraction technologies.
[0003] The electrochemical deintercalation method of lithium extraction from salt lake brine is an innovative direct lithium extraction process developed in recent years. Its essence is based on the working principle of lithium batteries, with lithium-rich lithium materials as anodes and lithium-deficient lithium materials as cathodes. After power is turned on, the anode delithium is put into the anolyte, the cathode is intercalated with lithium, and the position of the anolyte and brine are exchanged. Then, the voltage is adjusted to continue the delithiation and intercalation process. After repeated repetitions, the lithium ion concentration in the anolyte will continue to increase. According to public data reports, this technology can, first, increase the overall lithium recovery rate by 30% to 50%; second, it has strong adaptability to raw materials and can directly process original brine, old brine and brine at any stage; third, the lithium extraction device is modular and can form production lines of different sizes.
[0004] The idea of electrochemical deintercalation is ingenious and the process principle is feasible. The key to this technology lies in the selection and design of electrode materials. Ideal electrode materials should have good ionic or electronic conductivity, high specific capacity, excellent cycle stability and safety. For example, the positive and negative electrode materials in lithium-ion batteries achieve electrical energy storage through electrochemical deintercalation. Positive electrode materials such as lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt oxide (NMC), etc., and negative electrode materials such as graphite, silicon-based materials, etc., all achieve electrical energy storage by embedding or deintercalating lithium ions during the charging and discharging process.
[0005] As early as 1993, Kanoh et al. initially studied the working principle of electrodes with λ-MnO2 as positive electrode materials in different metal chloride solutions, and defined positive electrode materials with ion sieving properties as electrochemical ion pumps (EIP). With the development in recent years, the electrochemical deintercalation method has derived a reliable rocking chair electrochemical cycle system with nickel cobalt manganese oxide (NCM / NMC), lithium iron phosphate (LiFePO4), and lithium sulfide (Li2S) as positive electrode materials. This system cleverly controls the electrical properties of the electrode surface by controlling the externally applied electric field or current, thereby regulating the adsorption and deintercalation process and speed of lithium ions. At the same time, the appropriate intercalation structure and electrochemical properties in the positive electrode material are used to efficiently separate magnesium and lithium ions. Therefore, this type of system performs well in extracting lithium from brine and shows considerable advantages.
[0006] As an emerging technology for selectively extracting lithium ions from salt lakes, electrochemical deintercalation has many advantages but also has some potential defects and challenges.
[0007] Chinese patent CN118064873A adopts the traditional method of preparing positive electrode materials for lithium-ion batteries and applies it to the field of lithium extraction from salt lakes. The lithium source, iron source, and phosphorus source are mixed in proportion, and surfactants and complexing agents are added for calcination by fire method to obtain a lithium iron phosphate sintered body. The sintered body is then initially ground into 200 mesh particles and subjected to air jet pulverization to finally obtain lithium iron phosphate particles.
[0008] Chinese patent CN202380011985.5 discloses a lithium-based montmorillonite-coated lithium iron phosphate core-shell material, which uses an electrode preparation method that modifies the surface of lithium iron phosphate.
[0009] The above two processes can essentially be described as typical preparation processes for battery-grade lithium iron phosphate cathode materials. The main problem here is that as lithium ions are inserted and extracted from the crystal structure of traditional inorganic cathode materials, the crystal size and structure will change significantly. Specifically, when lithium ions are embedded, the lattice volume will expand, and when lithium ions are extracted, the lattice volume will shrink. This volume change will cause the collapse of the material lattice, thereby affecting the material stability and cycle efficiency of electrochemical deintercalation. Secondly, the intrinsic electrochemical performance of traditional cathode materials is generally 10 -12 S / cm~10 -9 S / cm varies. Due to its intrinsic structural problems, its conductivity is extremely poor. It is necessary to mix glucose in the preparation of the positive electrode material for fire sintering and use acetylene black and PVDF to enhance its conductivity. Finally, due to its insufficient conductivity, during the electrochemical deintercalation process, the electrode surface voltage needs to be increased to meet the minimum deintercalation potential of the electrode. Excessive potential will induce surface dielectric effect, especially brine electrolyte will aggravate its ionization effect, resulting in excessive useless energy consumption in the form of current. Summary of the invention
[0010] In view of the shortcomings of the prior art, the object of the present invention is to provide a porous membrane electrode material for brine electrochemical deintercalation method, so as to improve the electrical adsorption capacity and prevent its structural collapse.
[0011] Another object of the present invention is to provide a method for synthesizing the porous membrane electrode material.
[0012] Another object of the present invention is to provide applications of the porous membrane electrode material.
[0013] To achieve the above-mentioned purpose, the present invention provides a tetraoxocycloene-based lithium extraction membrane electrode material, which is an organic skeleton polymer, composed of tetraoxa[8]cycloene repeating structural units, including a clear hollow structure of 16 crown 4, and the tetraoxa[8]cycloene is composed of four conjugated benzofuran parts, which together form a mixed aromatic-antiaromatic unit. This material adopts a completely different adsorption principle from the lithium iron phosphate electrode material. The lithium iron phosphate electrode uses an electrochemical reaction method to adsorb and deintercalate lithium ions under the action of an electric field, which belongs to the electrochemical electrolysis method. However, this material has a special π conjugation and multifaceted aromaticity due to its planar fully conjugated porous structure of the D4h symmetric point group. This aromaticity can lead to the maintenance of a paratropic ("antiaromatic") current in the internal cyclooctatetraene (COT) core of the tetraoxocycloene polymer, while maintaining a bitropic ("aromatic") current at the outer edge. Due to the effect of electromagnetic relations on lithium ions and the cavity size effect, the material inherently possesses semiconductor properties and electrostatic adsorption capabilities for lithium. Applying electric field or electromagnetic force on this basis can completely and precisely control the adsorption and desorption process of lithium ions, which is an electrostatic force adsorption method.
[0014] The above-mentioned synthesis method of tetraoxocyclopentene-based lithium-extraction membrane electrode material comprises the following steps:
[0015] A) Weigh 5,8-dihydroxy-1,4-naphthoquinone monomer and place it in a reaction system, add 2 to 4 times the amount of the monomer substance as an auxiliary agent and 1 to 2 times the amount of the catalyst, evacuate the reaction system so that the internal pressure is maintained at 0.02 atm to 0.15 atm, and let it stand for 0.5 h to 2 h to obtain a purple solution;
[0016] B) adding 1 to 3 times the amount of the monomer substance as an activator, heating the reaction, reacting at 100° C. to 200° C. for 12 h to 48 h to obtain a black solid;
[0017] C) After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 4 hours to 16 hours, and the solid is separated and washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0018] D) The washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0019] The auxiliary agent in step A includes sodium chloride, potassium chloride, magnesium chloride, calcium chloride or a mixture thereof.
[0020] The catalyst in step A includes aluminum chloride, ferric chloride, titanium chloride, zinc chloride and phosphorus pentachloride.
[0021] The activating agent in step B includes methanesulfonic acid, benzenesulfonic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, and phosphoric acid.
[0022] The above-mentioned tetraoxocyclopentane-based lithium extraction membrane electrode adsorption material is applied to the membrane electrode material of salt lake brine electrochemical deintercalation method.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention is based on tetraoxocyclopentene lithium extraction membrane electrode material, which is an organic skeleton polymer. As a new type of lithium extraction membrane electrode material, the adsorption capacity of lithium ions can reach 149.6 mg / g, which has significant advantages over the existing lithium iron phosphate electrode material.
[0025] 2. The present invention is based on tetraoxocyclopentene lithium-extraction membrane electrode materials, which are organic skeleton polymers with a planar fully conjugated porous structure of D4h symmetric point group, giving it special π conjugation and multifaceted aromaticity. This structure makes the material intrinsically semiconductor and electrostatically adsorb lithium. Compared with lithium iron phosphate as an electrode material, it has significant electrochemical characteristics and lithium ion adsorption and desorption efficiency, and eliminates the crystal structure changes and even collapse of traditional inorganic positive electrode materials during the insertion and extraction of lithium ions, thereby affecting the stability and cycle efficiency of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the chemical structure of tetraoxocycloene polymer;
[0027] Figure 2 is the XRD pattern of tetraoxocyclopentene polymer;
[0028] Figure 3 The NMR of tetraoxocyclopentane polymer 13 Figure C;
[0029] Figure 4 This is the FT-IR graph of tetraoxocycloene polymer. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0031] The present invention provides a lithium extraction membrane electrode material based on tetraoxadiene, which is an organic skeleton polymer, such as Figure 1 It is shown that it is composed of tetraoxa[8]cycloolefin repeating structural units and contains a clear hollow structure of 16-crown 4. The tetraoxa[8]cycloolefin is composed of four conjugated benzofuran parts, which together form a mixed aromatic-antiaromatic unit. Figure 2 is the XRD pattern of tetraoxocyclopentene polymer, Figure 3 The NMR of tetraoxocyclopentane polymer 13 Figure C, Figure 4 This is the FT-IR graph of tetraoxocycloene polymer.
[0032] This material uses a completely different adsorption principle from lithium iron phosphate electrode materials. Lithium iron phosphate electrodes use electrochemical reactions to adsorb and deintercalate lithium ions under the action of an electric field, which is an electrochemical electrolysis method. This material has a special π conjugation and multifaceted aromaticity due to its planar fully conjugated porous structure of the D4h symmetry point group. This aromaticity can lead to the maintenance of a paratropic ("anti-aromatic") current in the internal cyclooctatetraene (COT) core of the tetraoxocycloene polymer and a bitropic ("aromatic") current at the outer edge. Due to the effect of electromagnetic relations on lithium ions and the cavity size effect, this material inherently possesses semiconductor properties and electrostatic adsorption capabilities for lithium. On this basis, applying electric field forces or electromagnetic forces can completely and precisely control the adsorption and desorption process of lithium ions, which is an electrostatic force adsorption method.
[0033] The above-mentioned synthesis method of tetraoxocyclopentene-based lithium-extraction membrane electrode material comprises the following steps:
[0034] A) Weigh 5,8-dihydroxy-1,4-naphthoquinone monomer and place it in a reaction system, add 2 to 4 times the amount of the monomer substance as an auxiliary agent and 1 to 2 times the amount of the catalyst, evacuate the reaction system so that the internal pressure is maintained at 0.02 atm to 0.15 atm, and let it stand for 0.5 h to 2 h to obtain a purple solution;
[0035] B) adding 1 to 3 times the amount of the monomer substance as an activator, heating the reaction, reacting at 100° C. to 200° C. for 12 h to 48 h to obtain a black solid;
[0036] C) After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 4 hours to 16 hours, and the solid is separated and washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0037] D) The washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0038] The auxiliary agent in step A includes sodium chloride, potassium chloride, magnesium chloride, calcium chloride or a mixture thereof.
[0039] The catalyst in step A includes aluminum chloride, ferric chloride, titanium chloride, zinc chloride and phosphorus pentachloride.
[0040] The activating agent in step B includes methanesulfonic acid, benzenesulfonic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, and phosphoric acid.
[0041] Some examples of the synthesis of tetraoxocyclopentane-based lithium-extraction membrane electrode materials are listed below.
[0042]
Example 1
[0043] Preparation of tetraoxocyclopentane-based lithium-extraction membrane electrode materials
[0044] First, 1.0 mol of 5,8-dihydroxy-1,4-naphthoquinone monomer was weighed and placed in a reaction system, and 1 times the amount of sodium chloride, 1 times potassium chloride and 2 times phosphorus pentachloride of the monomer substance were added, and the reaction system was vacuumed to maintain the internal pressure at 0.12 atm and allowed to stand for 2 hours to obtain a purple solution;
[0045] Then, p-toluenesulfonic acid, which is twice the amount of the monomer substance, was added, heated to react at 200° C. for 36 h to obtain a black solid;
[0046] After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 16 hours, and the solid is separated and washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0047] Finally, the washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0048]
Example 2
[0049] Preparation of tetraoxocyclopentane-based lithium-extraction membrane electrode materials
[0050] First, 1.0 mol of 5,8-dihydroxy-1,4-naphthoquinone monomer was weighed and placed in a reaction system, 4 times the amount of sodium chloride and 1 times the amount of ferric chloride were added, and the reaction system was vacuumed to maintain the internal pressure at 0.08 atm and allowed to stand for 0.5 h to obtain a purple solution;
[0051] Then, phosphoric acid of 1 times the amount of the monomer substance was added, heated for reaction, and reacted at 150° C. for 12 h to obtain a black solid;
[0052] After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 8 hours, and the solid and liquid are separated, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0053] Finally, the washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0054]
Example 3
[0055] Preparation of tetraoxocyclopentane-based lithium-extraction membrane electrode materials
[0056] First, 1.0 mol of 5,8-dihydroxy-1,4-naphthoquinone monomer was weighed and placed in a reaction system, and 2 times the amount of sodium chloride, 1 times the amount of calcium chloride, and 1.5 times the amount of titanium chloride were added to the reaction system, and the reaction system was vacuumed to maintain an internal pressure of 0.15 atm and allowed to stand for 1.0 h to obtain a purple solution;
[0057] Then, 1 times the amount of the monomer substance was added with methanesulfonic acid, and the mixture was heated to react at 100° C. for 24 h to obtain a black solid;
[0058] After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 4 hours, and the solid and liquid are separated, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0059] Finally, the washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0060]
Example 4
[0061] Preparation of tetraoxocyclopentane-based lithium-extraction membrane electrode materials
[0062] First, 1.0 mol of 5,8-dihydroxy-1,4-naphthoquinone monomer was weighed and placed in a reaction system, and 2 times the amount of magnesium chloride, 2 times the amount of calcium chloride, and 2 times the amount of aluminum chloride were added to the reaction system. The reaction system was evacuated to maintain an internal pressure of 0.02 atm and allowed to stand for 0.5 h to obtain a purple solution.
[0063] Then, add trifluoromethanesulfonic acid 3 times the amount of the monomer substance, heat to react, and react at 180° C. for 48 hours to obtain a black solid;
[0064] After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 12 hours, and the solid and liquid are separated, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0065] Finally, the washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0066]
Example 5
[0067] Preparation of tetraoxocyclopentane-based lithium-extraction membrane electrode materials
[0068] First, 1.0 mol of 5,8-dihydroxy-1,4-naphthoquinone monomer was weighed and placed in a reaction system, 3 times the amount of magnesium chloride and 1.5 times the amount of aluminum chloride were added, and the reaction system was vacuumed to maintain the internal pressure at 0.06 atm and allowed to stand for 1.5 hours to obtain a purple solution;
[0069] Then, benzenesulfonic acid was added in an amount twice that of the monomer substance, and the mixture was heated to react at 130° C. for 36 h to obtain a black solid.
[0070] After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 12 hours, and the solid and liquid are separated, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0071] Finally, the washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0072] [Comparative Example 1]
[0073] Preparation of tetraoxocyclopentane-based lithium-extraction membrane electrode materials
[0074] First, 1.0 mol of 1,4,5,8-naphthalenetetraol monomer was weighed and placed in a reaction system, and 1 times the amount of sodium chloride, 1 times potassium chloride and 2 times phosphorus pentachloride were added according to the amount of the monomer substance, and the reaction system was vacuumed to maintain the internal pressure at 0.12 atm and allowed to stand for 2 hours to obtain a purple solution;
[0075] Then, p-toluenesulfonic acid, which is twice the amount of the monomer substance, was added, heated to react at 200° C. for 36 h to obtain a black solid;
[0076] After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 16 hours, and the solid is separated and washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0077] Finally, the washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0078] [Comparative Example 2]
[0079] Preparation of tetraoxocyclopentane-based lithium-extraction membrane electrode materials
[0080] First, 1.0 mol of juglone monomer was weighed and placed in a reaction system, and 1 times the amount of sodium chloride, 1 times potassium chloride and 2 times phosphorus pentachloride of the monomer substance were added, and the reaction system was vacuumed to maintain the internal pressure at 0.12 atm and allowed to stand for 2 hours to obtain a purple solution;
[0081] Then, p-toluenesulfonic acid, which is twice the amount of the monomer substance, was added, heated to react at 200° C. for 36 h to obtain a black solid;
[0082] After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 16 hours, and the solid is separated and washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;
[0083] Finally, the washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
[0084] [Comparative Example 3]
[0085] Preparation of lithium iron phosphate electrode material
[0086] First, 151.85 g of ferrous phosphate, 37.45 g of lithium carbonate, and 12.98 g of glucose were weighed and mixed and ground to obtain a mixture slurry; then, the mixture slurry was placed in an electric blast drying oven and dried at 105°C to constant weight to obtain a mixture dry material; the mixture dry material was crushed and ground, sintered under nitrogen protection, calcined at 700°C for 10 hours, and then kept warm for 6 hours to obtain a sintered material; finally, the sintered material was crushed and sieved, 3.28 g of vanadium pentoxide and 7.18 g of graphene were added, mixed evenly, placed in a tubular electric furnace, nitrogen was introduced, calcined at 750°C for 5 hours, and then kept warm for 2 hours to obtain a lithium iron phosphate electrode material.
[0087] [Simulation experiment on lithium extraction from salt lake brine by electrochemical deintercalation method]
[0088] 1. Preparation of electrode material / DMF / PVDF degassing spin coating solution
[0089] First, the electrode materials obtained in the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 3 are weighed, crushed, ground, and sieved with a 200-mesh standard sieve. The sieved material is dispersed in an appropriate amount of N,N-dimethylformamide (DMF), ultrasonically shaken, and fully mixed to obtain an electrode material / DMF dispersion; then, polyvinylidene fluoride (PVDF) powder and carbon black powder are added to the dispersion in a ratio of electrode material: carbon black powder: PVDF mass ratio of 8:1:1, and stirred at 60°C to 80°C for 4h to 12h until PVDF is completely dissolved to obtain an electrode material / DMF / PVDF spin-coating liquid; finally, the electrode material / DMF / PVDF spin-coating liquid is transferred to a planetary stirring degassing machine for degassing for 1h to 4h to obtain a homogeneous electrode material / DMF / PVDF degassing spin-coating liquid.
[0090] 2. Preparation of electrode material / PVDF composite electrode membrane
[0091] First, 3 to 7 drops of the prepared electrode material / DMF / PVDF degassing spin-coating liquid are taken with a dropper and dropped on a 2.5 cm×2.5 cm ITO glass to obtain a coated glass; then, the coated glass is placed on a coater and spin-coated at a spin-coating rate of 200 to 500 rpm for 12 to 30 seconds to obtain a coated glass; subsequently, the coated glass is placed on a heating table and heated at 80°C for 30 to 50 minutes until the solvent DMF is completely evaporated to obtain a uniformly coated glass; finally, the electrode film on the glass sheet on the coated glass is peeled off with pointed tweezers, weighed, and a copper foil of appropriate size is applied to one side of the electrode film for compaction to obtain an electrode material / PVDF composite electrode film.
[0092] 3. Electrochemical deintercalation test of salt lake brine
[0093] Simulated brine:
[0094] Na + 102.4g / L, Mg 2+ 15.9g / L, Li + 0.81g / L, Cl - 201.9g / L, Ca 2+ 2.78g / L, K + 16.3g / L, SO4 2- 20.8g / L, PH7.4.
[0095] Test method:
[0096] First, the prepared lithium iron phosphate material (Comparative Example 3) was used as a cathode, nickel foam was used as an anode, and a 1 mol / L sodium chloride aqueous solution was used as an electrolyte. A constant voltage power supply was used to pre-electrolyze lithium at a DC voltage of 1.0 V until the current was less than 2 mA / g to obtain a lithium-deficient electrode material (lithium iron phosphate lithium-deficient electrode);
[0097] Then, a lithium iron phosphate under-lithiation electrode (Comparative Example 3) and a tetraoxocyclopentane polymer electrode (Examples 1 to 5 and Comparative Examples 1 and 2) were used as anodes, nickel foam was used as cathodes, 100 ml of simulated brine was used as supporting electrolyte, the temperature was controlled at 15° C., electrochemical adsorption was performed at a DC voltage of 1.0 V for 60 min to obtain a saturated lithium anode;
[0098] Finally, the saturated lithium anode was transferred to 100 ml of 1 mol / L sodium chloride and 0.5 mol / L hydrochloric acid electrolyte, the electrode was reversed, and a constant current of 1.0 V was applied for desorption. The desorption time was controlled at about 80 min.
[0099] Take samples of the solution before and after brine adsorption, use ICP-MS to determine the content of lithium ions, and calculate the adsorption capacity of the electrode material for lithium ions Q according to the following formula: t .
[0100] Adsorption capacity calculation formula:
[0101] Q t =(C0-C t )×V / m
[0102] Among them, Q t ——Adsorption capacity, C0——Lithium ion concentration of solution before adsorption, C t ——Lithium ion concentration of the solution after adsorption, V——volume of the solution, m——mass of the adsorbent.
[0103] Test results: mg / g
[0104]
[0105] Test conclusion:
[0106] 1. The present invention is based on tetraoxocyclopentene lithium extraction membrane electrode material, which is an organic skeleton polymer. As a new type of lithium extraction membrane electrode material, the adsorption capacity of lithium ions can reach 149.6 mg / g, which has significant advantages over the existing lithium iron phosphate electrode material.
[0107] 2. The present invention is based on tetraoxocyclopentene lithium-extraction membrane electrode materials, which are organic skeleton polymers with a planar fully conjugated porous structure of D4h symmetric point group, giving it special π conjugation and multifaceted aromaticity. This structure makes the material intrinsically semiconductor and electrostatically adsorb lithium. Compared with lithium iron phosphate as an electrode material, it has significant electrochemical characteristics and lithium ion adsorption and desorption efficiency, and eliminates the crystal structure changes and even collapse of traditional inorganic positive electrode materials during the insertion and extraction of lithium ions, thereby affecting the stability and cycle efficiency of the material.
[0108] 3. The present invention is based on tetraoxocyclopentane lithium-extraction membrane electrode materials, optimizes the experimental conditions, obtains tetraoxocyclopentane polymers under relatively mild conditions, and confirms the important role of 5,8-dihydroxy-1,4-naphthoquinone monomers in the synthesis.
[0109] The membrane electrode material for lithium extraction from salt lakes based on tetraoxocycloolefin polymers of the present invention solves many problems in the prior art, shows great application prospects, and lays a solid foundation for new technologies for efficient, stable and environmentally friendly lithium extraction from salt lakes.
[0110] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A method for synthesizing a membrane electrode material based on tetraoxocyclopentane lithium extraction, characterized in that: The steps include: A) Weigh 5,8-dihydroxy-1,4-naphthoquinone monomer and place it in a reaction system, add 2 to 4 times the amount of the monomer substance as an auxiliary agent and 1 to 2 times the amount of the catalyst, evacuate the reaction system so that the internal pressure is maintained at 0.02 atm to 0.15 atm, and let it stand for 0.5 h to 2 h to obtain a purple solution; B) adding 1 to 3 times the amount of the monomer substance as an activator, heating the reaction, reacting at 100° C. to 200° C. for 12 h to 48 h to obtain a black solid; C) After the reaction is completed, the mixture is cooled to room temperature, and 2N hydrochloric acid is added to a mixture of water and methanol in a volume ratio of 1:1 to acidify the obtained black solid, and the mixture is stirred and slurried for 4 hours to 16 hours, and the solid is separated and washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer; D) The washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxocyclopentene-based lithium extraction membrane electrode material.
2. The method for synthesizing a membrane electrode material based on tetraoxocyclopentane lithium extraction according to claim 1, characterized in that: The auxiliary agent in step A includes sodium chloride, potassium chloride, magnesium chloride, calcium chloride or a mixture thereof.
3. The method for synthesizing a tetraoxocyclopentene-based lithium-extraction membrane electrode material according to claim 1, characterized in that: The catalyst in step A includes aluminum chloride, ferric chloride, titanium chloride, zinc chloride and phosphorus pentachloride.
4. The method for synthesizing a tetraoxocyclopentene-based lithium-extraction membrane electrode material according to claim 1, characterized in that: The activating agent in step B includes methanesulfonic acid, benzenesulfonic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, and phosphoric acid.
5. A tetraoxocyclopentene-based lithium-extraction membrane electrode material prepared by the synthesis method according to claims 1 to 4, which is an organic skeleton polymer, characterized in that: The tetraoxa[8]cycloolefin-based lithium extraction membrane electrode material adsorption material is composed of a tetraoxa[8]cycloolefin repeating structural unit, including a clear hollow structure of 16-crown-4, and the tetraoxa[8]cycloolefin is composed of four conjugated benzofuran parts, which together form a mixed aromatic-antiaromatic unit.
6. The tetraoxocyclopentane-based lithium extraction membrane electrode adsorption material according to claim 5 is used to separate and enrich lithium ions in salt lake brine.