Block polymer for cathode catalyst layer, cathode catalyst layer slurry, membrane electrode and preparation method

By using non-fluorinated polyamide-sulfonated imine block polymer (FOS) as the cathode catalyst ionomer in a high-temperature proton exchange membrane fuel cell, the problems of uneven phosphoric acid distribution and loss were solved, thereby improving the proton conductivity and battery performance.

CN118978691AActive Publication Date: 2024-11-19SHANGHAI INST OF SPACE POWER SOURCES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411032611.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

In existing high-temperature proton exchange membrane fuel cells, uneven distribution of phosphoric acid in the catalyst layer leads to catalyst poisoning and blockage of mass transfer channels, and phosphoric acid loss causes a decline in battery performance.

Method used

Non-fluorinated polyamide-sulfonated imide block polymer (FOS) is used as the cathode catalyst layer ionomer, and sulfonylimide groups are used as proton transport carriers to construct more three-phase reaction interfaces. The acid retention capacity is enhanced by rigid-flexible block structure.

Benefits of technology

It improves the proton conductivity and phosphoric acid retention capacity of the cathode catalyst layer, increases the three-phase interface, and enhances the performance and lifespan of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978691A_ABST
    Figure CN118978691A_ABST
Patent Text Reader

Abstract

The invention provides a block polymer for a cathode catalyst layer, cathode catalyst layer slurry, a membrane electrode and a preparation method. The membrane electrode comprises a cathode GDE, a proton exchange membrane and an anode GDE, the cathode / anode GDE comprises a cathode gas diffusion layer and a cathode / anode catalyst layer applied to one side of the micropore layer on the cathode gas diffusion layer; and the cathode catalyst layer comprises a cathode catalyst and a non-fluorinated polyamide-sulfonated imine block polymer (FOS). When the FOS is adopted as the ionomer of the cathode catalyst layer, the proton conductivity of the cathode catalyst layer is improved, the three-phase interface structure of the catalyst, the ionomer and oxygen is optimized, and the full utilization of Pt active sites is facilitated; a cavity structure is formed through a flexible section in a rigid-flexible block structure in the FOS, more free phosphoric acid is stored, the acid retention capacity of the cathode catalyst layer is enhanced, uniform distribution of phosphoric acid in the cathode catalyst layer is ensured, and the problem that the battery performance is remarkably reduced due to the fact that the impedance of a membrane electrode is increased due to loss of phosphoric acid is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-temperature proton exchange membrane fuel cells, and in particular relates to a block polymer for a cathode catalyst layer, a cathode catalyst layer slurry, a membrane electrode and a preparation method. Background Art

[0002] Proton exchange membrane fuel cells (PEMFCs) are considered the most promising fuel cells due to their high energy conversion efficiency, high power density, no pollutant emissions, and low operating noise. According to the different operating temperatures, PEMFCs are divided into low-temperature PEMFCs (LT-PEMFCs) based on Nafion membranes and high-temperature PEMFCs (HT-PEMFCs) based on polybenzimidazole (PBI) membranes doped with phosphoric acid (PA). Currently, the relatively successful low-temperature PEMFCs have high requirements for fuel gas purity and complex water and heat management systems, which limit their application scenarios. Therefore, HT-PEMFCs with operating temperatures above 120°C have attracted much attention due to their fast reaction kinetics, high tolerance to fuel / air impurities, simple plate design, and better heat and water management, making them expected to become the next generation of PEMFCs for use in hydrogen fuel vehicles and combined heat and power (CHP) systems. However, since PA is the main proton transport carrier in HT-PEMFC, PA will cover the active sites of Pt in the catalyst layer, causing catalyst poisoning and greatly reducing activity. At the same time, the unevenly distributed PA will block the mass transfer channel of the catalyst layer, making it more difficult to diffuse oxygen, and causing acid flooding under high current density working conditions of the battery. In addition, as the battery working time increases, the PA in the membrane electrode will be lost to the external environment along with the fuel gas and water vapor, causing acid deficiency in the catalyst layer and the membrane, reducing the proton transport channel of the membrane electrode, reducing the effective three-phase reaction interface in the catalyst layer, and ultimately causing a sharp decline in battery performance.

[0003] The commonly used solution at present is to introduce a certain amount of hydrophobic polymers such as polytetrafluoroethylene (PTFE) into the catalyst layer. PTFE molecules can improve the distribution of PA in the catalyst layer and bond the catalyst particles into a whole, thereby improving battery performance. However, on the one hand, PTFE molecules are not conductive and cannot play a role in constructing proton transmission channels in the catalyst layer, which reduces the reactive sites of the catalyst and is not conducive to improving battery performance. On the other hand, PTFE molecules are hydrophobic substances and do not have the ability to retain phosphoric acid, which makes it impossible to control the loss of phosphoric acid during battery operation, affecting the performance and life of high-temperature proton exchange membrane fuel cells. Summary of the invention

[0004] In order to overcome the deficiencies in the prior art, the inventors have conducted intensive research and provided a block polymer for a cathode catalyst layer, a cathode catalyst layer slurry, a membrane electrode and a preparation method, using FOS as a cathode catalyst layer ionomer, and utilizing the sulfonimide group in FOS as a proton transport carrier to construct more effective three-phase reaction interfaces, thereby further increasing the proton transport channels of the cathode catalyst layer; on the other hand, a cavity structure is formed by the rigid-flexible block structure in FOS, thereby increasing the acid retention capacity of the catalyst layer, effectively overcoming the problem of phosphoric acid loss, and improving the performance and service life of the battery.

[0005] The technical solution provided by the present invention is as follows:

[0006] In a first aspect, a method for preparing a block polymer for a cathode catalyst layer comprises:

[0007] Step 1: Add p-toluenesulfonamide, sodium hydroxide and deionized water to a reaction vessel equipped with a reflux condenser; after the reaction mixture is stirred and evenly mixed at 95±5°C, slowly add benzenesulfonyl chloride to the solution, and stir at 95±5°C until the reaction is complete; then adjust the pH value of the solution to neutral, filter out the white precipitate, adjust the pH value of the solution to 1-2 again, filter out the white precipitate, and recrystallize to obtain product 1;

[0008] Step 2: LiOH·H2O and product 1 are completely dissolved in deionized water, KMnO4 is slowly added into the reaction vessel, the reaction mixture is stirred at 95±5°C until the reaction is complete, filtered, the filtrate is acidified, the final product is collected, and vacuum dried to obtain product 2;

[0009] Step 3: Add the product II, 5-aminoisophthalic acid dimethyl ester, LiCl, triphenyl phosphite TPP, pyridine, and a mixture of aprotic organic solvents into a reaction vessel, and stir at 100±5°C under an inert atmosphere to complete the reaction; after the reaction is completed, the mixture is distilled under reduced pressure, and then poured into a sufficient amount of cold isopropanol, filtered to obtain a white precipitate, washed, and vacuum dried to obtain the product III;

[0010] Step 4: Add product 3 and deionized water to a reaction container and stir to dissolve; then dissolve NaOH in deionized water and then dropwise add it to the mixture, stir overnight at room temperature, adjust the pH of the solution to 1-2 with concentrated HCl to obtain a yellow powder, and vacuum dry to obtain SIDA;

[0011] Step 5: Mix 4,4'-(9-fluorenylidene)diphenylamine FDA, 1,8-octanedioic acid, SIDA, LiCl, triphenyl phosphite, pyridine and aprotic organic solvent, and stir to react in an inert atmosphere; after the reaction is completed, cool the mixture to 70±5°C, then pour it into cold methanol, filter to obtain a light yellow precipitate, wash it continuously with methanol and deionized water, and dry it under reduced pressure to obtain a non-fluorinated polyamide-sulfonated imine polymer (FOS) for a cathode catalyst layer.

[0012] In combination with the first aspect, in step 1, the molar ratio of p-toluenesulfonamide, benzenesulfonyl chloride and sodium hydroxide is (1-1.05):1:(1-1.05).

[0013] In combination with the first aspect, in step 3, the molar ratio of product 2 to dimethyl 5-aminoisophthalate is 1:1 to 1.05.

[0014] In combination with the first aspect, in step 5, the molar ratio of 4,4'-(9-fluorenylene)diphenylamine FDA, 1,8-suberic acid and SIDA is 1: x%:(100-x)%, x%=10% to 90%.

[0015] In a second aspect, a block polymer for a cathode catalyst layer is prepared by the method for preparing a block polymer for a cathode catalyst layer described in the first aspect.

[0016] In a third aspect, a cathode catalyst layer slurry comprises a cathode catalyst and the non-fluorinated polyamide-sulfonated imine block polymer FOS described in the second aspect, wherein the mass ratio of the non-fluorinated polyamide-sulfonated imine block polymer FOS to the carbon carrier in the cathode catalyst is (5-15):100.

[0017] In a fourth aspect, a cathode gas diffusion electrode comprises a cathode gas diffusion layer and a cathode catalyst layer applied on one side of a microporous layer of the cathode gas diffusion layer; the cathode catalyst layer is prepared using the cathode catalyst layer slurry described in the third aspect.

[0018] In the fifth aspect, a membrane electrode comprises a cathode GDE, a proton exchange membrane and an anode GDE; the cathode GDE comprises a cathode gas diffusion layer and a cathode catalyst layer applied on one side of a microporous layer on the cathode gas diffusion layer; the anode GDE comprises an anode gas diffusion layer and an anode catalyst layer applied on one side of a microporous layer on the anode gas diffusion layer; the cathode catalyst layer is prepared using the cathode catalyst layer slurry described in the third aspect.

[0019] In a sixth aspect, a method for preparing a membrane electrode comprises:

[0020] S1, uniformly dispersing an anode catalyst and an anode hydrophobic binder in a water-alcohol solution to form an anode catalyst slurry;

[0021] S2, coating the anode catalyst slurry on the anode gas diffusion layer to obtain an anode GDE;

[0022] S3, uniformly dispersing the cathode catalyst and the dissolved non-fluorinated polyamide-sulfonated imine polymer (FOS) solution in an organic solvent to form a cathode catalyst slurry;

[0023] S4, coating the cathode catalyst slurry on the cathode gas diffusion layer to obtain a cathode GDE;

[0024] S5, laminating the anode GDE, the proton exchange membrane and the cathode GDE in sequence, and compounding them by hot pressing to obtain a membrane electrode.

[0025] In a seventh aspect, a high-temperature proton exchange membrane fuel cell adopts the cathode gas diffusion electrode described in the fourth aspect, or adopts the membrane electrode described in the fifth aspect.

[0026] A block polymer for a cathode catalyst layer, a cathode catalyst layer slurry, a membrane electrode and a preparation method provided by the present invention have the following beneficial effects:

[0027] The present invention adopts FOS as the cathode catalyst layer ionomer, utilizes the sulfonimide group in FOS as the proton transfer carrier, optimizes the three-phase interface structure of the catalyst, the ionomer and oxygen or air, further increases the proton transfer channel of the cathode catalyst layer, improves the proton conductivity of the cathode catalyst layer, and is conducive to the full utilization of the Pt active site; through the rigid-flexible block structure in FOS to form a cavity structure, more free phosphoric acid is stored, the acid retention capacity of the cathode catalyst layer is enhanced, the effective distribution of phosphoric acid in the cathode catalyst layer is guaranteed, and the problem of significant decrease in battery performance caused by increased membrane electrode impedance due to phosphoric acid loss is solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of the structure of a high-temperature proton exchange membrane fuel cell;

[0029] Figure 2 is the SEM image of FOS;

[0030] Figure 3 is the NMR result of FOS;

[0031] Figure 4 is the infrared spectrum of FOS;

[0032] Figure 5 The membrane electrode polarization characteristic curves of different cathode catalyst layers of Example 1-2 and Comparative Example 1-2;

[0033] Figure 6 It is the membrane electrode impedance diagram of different cathode catalyst layers of Example 1-2 and Comparative Example 1-2. DETAILED DESCRIPTION

[0034] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0035] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.

[0036] like Figure 1 As shown, the high temperature proton exchange membrane fuel cell comprises:

[0037] The membrane electrode comprises a cathode GDE 10, a proton exchange membrane 1 and an anode GDE 20. The cathode GDE 10 comprises a cathode gas diffusion layer 12 and a cathode catalyst layer 11 applied on one side of the cathode gas diffusion layer; the anode GDE 20 comprises an anode gas diffusion layer 22 and an anode catalyst layer 21 applied on one side of the anode gas diffusion layer;

[0038] A cathode monopolar plate 13 and a first end plate 14 disposed on the cathode 10 side; and

[0039] An anode monopolar plate 23 and a second end plate 24 are provided on the anode 20 side.

[0040] The proton exchange membrane is a polybenzimidazole membrane (PBI), and the PBI is treated by doping with phosphoric acid.

[0041] The cathode gas diffusion layer 12 includes a support layer 121 and a microporous layer 122. The support layer 121 is located on the side of the microporous layer 122 away from the proton exchange membrane 1. The anode gas diffusion layer 22 includes a support layer 221 and a microporous layer 222. The support layer 221 is located on the side of the microporous layer 222 away from the proton exchange membrane 1.

[0042] The operating temperature of the high-temperature proton exchange membrane fuel cell is 140℃-220℃, and the proton exchange membrane used is a phosphoric acid-doped PBI membrane. When the high-temperature proton exchange membrane fuel cell is working, hydrogen is introduced into the anode side, and a HOR reaction (hydrogen oxidation reaction) occurs to generate H+, and air or oxygen is introduced into the cathode side, and an ORR (oxygen reduction reaction) reaction occurs at the cathode to generate water.

[0043] In the membrane electrode, the cathode catalyst layer includes a cathode catalyst and a non-fluorinated polyamide-sulfonated imine block polymer (FOS). As a proton transport functionalized polymer (non-fluorinated polyamide-sulfonated imine block polymer molecule, FOS) constructed with a nanoscale three-phase interface, the molecular formula is shown in Formula I. It is an ionic polymer with a block structure. The decomposition temperature of FOS is as high as 345°C, which can fully meet the use conditions of 140-220°C in HT-PEMFC, and the proton conductivity of FOS has a trend of increasing with increasing temperature.

[0044]

[0045] A non-fluorinated polyamide-sulfonated imine polymer (FOS) with a block structure is introduced into the cathode catalyst layer of the membrane electrode. Due to the presence of groups in the FOS molecular structure, it can be precisely anchored next to the active site of the supported catalyst (such as PtCo / C) through hydrogen bonding, etc., to achieve the construction of a nanoscale three-phase interface on the catalyst surface. The introduction of this non-fluorinated polyamide-sulfonated imine block polymer with good proton conductivity reduces the catalytic layer's dependence on traditional non-conductive polymer ionomers (such as PTFE, etc.), and the introduction of sulfonyl imide ions improves proton conductivity.

[0046] The preparation method of non-fluorinated polyamide-sulfonated imine polymer (FOS) comprises the following steps:

[0047] Step 1: The synthesis process of 4-methyldiphenylsulfonyl imide (hereinafter referred to as product 1) is as follows: p-toluenesulfonamide, sodium hydroxide and deionized water are added to a reaction vessel equipped with a reflux condenser. After the reaction mixture is stirred and evenly mixed at 95±5°C, benzenesulfonyl chloride is slowly added dropwise to the solution within 1 to 2 hours, and stirred at 95±5°C overnight. Thereafter, the pH value of the solution is adjusted to 7 with dilute HCl, the white precipitate is removed by filtration, and the pH value of the solution is adjusted to 1 to 2 with dilute HCl again, the white precipitate is obtained by filtration, and recrystallization is performed to obtain product 1.

[0048] In this step, the molar ratio of p-toluenesulfonamide, benzenesulfonyl chloride and sodium hydroxide is (1-1.05):1:(1-1.05).

[0049] In this step, after the reaction is completed, the pH value of the solution is adjusted to 7 with dilute HCl, and the white precipitate p-toluenesulfonamide is filtered out to increase the product concentration of product 1.

[0050] Step 2: The synthesis process of product II is as follows: LiOH·H2O and product I are completely dissolved in deionized water at 95±5°C, KMnO4 is slowly added to the reaction vessel within 1 to 2 hours, the reaction mixture is stirred at 95±5°C overnight, MnO2 and unreacted KMnO4 are filtered out, the filtrate is acidified with concentrated HCl, the final product is collected, and vacuum dried at 100±5°C for at least 24 hours to obtain product II.

[0051] In this step, the molar ratio of LiOH·H2O, product 1 and KMnO4 is (1-1.1):1:(2-2.1).

[0052] Step 3: The synthesis process of 5-(4-(N-phenylsulfonyl)sulfonamido)benzamido)isophthalic acid dimethyl ester (hereinafter referred to as product three) is as follows: product two, a mixture of 5-aminoisophthalic acid dimethyl ester, LiCl, triphenyl phosphite TPP, N-methylpyrrolidone (NMP) and pyridine are added to a reaction vessel, and stirred overnight at 100±5°C under an argon atmosphere. After the reaction is completed, the mixture is distilled under reduced pressure, then poured into a sufficient amount of cold isopropanol, filtered to obtain a white precipitate, and then washed with isopropanol and deionized water. The final product is vacuum dried at 100±5°C overnight to obtain product three.

[0053] In this step, the molar ratio of the product II to dimethyl 5-aminoisophthalate is 1:1 to 1.05.

[0054] Step 4: Product 3 is hydrolyzed in an alkaline aqueous solution to obtain sulfonyl imide diacid monomer (hereinafter referred to as SIDA): Product 3 and deionized water are added to a reaction vessel and stirred to dissolve. Then NaOH is dissolved in deionized water and then added dropwise to the mixture within 1 to 2 hours, stirred at room temperature overnight, and concentrated HCl is used to adjust the solution pH to 1 to 2 to obtain yellow powder SIDA, which is vacuum dried at 100±5°C for at least 24 hours.

[0055] In this step, the molar ratio of product three to NaOH is 1:4-8.

[0056] Step 5: Final synthesis of FOS: 4,4'-(9-fluorenyl)diphenylamine FDA, 1,8-octanedioic acid, SIDA, LiCl and triphenyl phosphite were mixed with NMP and pyridine, and stirred in an argon atmosphere for 2-3 hours. After the reaction was completed, the mixture was cooled to 70±5°C, then poured into cold methanol, filtered to obtain a light yellow precipitate, washed continuously with methanol and deionized water, and dried under reduced pressure at 100±5°C for at least 12 hours to obtain polymer FOS.

[0057] In this step, the molar ratio of 4,4'-(9-fluorenylene)diphenylamine FDA, 1,8-suberic acid and SIDA is 1: x%:(100-x)%, x%=10% to 90%, preferably x%=30% to 70%.

[0058] In this step, the stirring reaction time in the argon atmosphere should not exceed 3 h to ensure the yield of the reactant.

[0059] The non-fluorinated polyamide-sulfonated imide polymer (FOS) with a block structure introduced into the cathode catalyst layer not only has a high proton conductivity, but also because of the introduction of more sulfonyl imide groups in its side chain, it can enhance the movement of protons between the catalyst layers and also play a role in building a three-phase interface. In addition, the rigidity of FOS —Flexibility The block structure can achieve effective enrichment of phosphoric acid (PA), which greatly ensures the effective distribution of phosphoric acid in the cathode catalyst layer, ensures the long-term retention capacity of PA, greatly increases the three-phase interface in the electrode, and improves the catalyst utilization as well as the performance and service life of the battery.

[0060] The cathode catalyst is at least one of Pt / C, PtFe / C or PtCo / C; wherein the mass fraction of the precious metal is 5% to 70%. The loading of the precious metal in the cathode catalyst layer is 0.5-1.0 mg / cm 2 The “noble metal” described herein refers to Pt (platinum).

[0061] In the cathode catalyst layer, the mass ratio of the non-fluorinated polyamide-sulfonated imine block polymer FOS to the carbon carrier in the cathode catalyst is (5-15):100.

[0062] In the membrane electrode, the cathode gas diffusion layer includes a support layer and a microporous layer, and the support layer is located on the side of the microporous layer away from the proton exchange membrane. The support layer is carbon paper and / or carbon cloth, and the microporous layer includes carbon powder and PTFE, and the content of PTFE in the microporous layer is 5%-25%. The carbon powder is at least one of activated carbon, graphitized carbon, carbon nanotubes, carbon nanobelts, and carbon nanospheres. The cathode catalyst layer is coated on the cathode gas diffusion layer to form a cathode GDE.

[0063] In the membrane electrode, the anode catalyst layer comprises an anode catalyst and an anode hydrophobic binder, wherein the anode catalyst comprises at least one of Pt / C, PtFe / C or PtCo / C, wherein the mass fraction of the precious metal is 5% to 70%. The loading of the precious metal in the anode catalyst layer is 0.3-0.5 mg / cm 2The anode hydrophobic binder is at least one of PTFE, polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-chlorotrifluoroethylene copolymer (ECTFE), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), and polydimethylsiloxane (PDMS).

[0064] In the membrane electrode, the anode catalyst layer is coated on the anode gas diffusion layer to form the anode GDE. The structure of the anode gas diffusion layer is the same as that of the cathode gas diffusion layer, and the material selection range is the same as that of the cathode gas diffusion layer. When used, different raw material components and contents are selected according to specific requirements.

[0065] The present invention also provides a method for preparing the above-mentioned membrane electrode, the method comprising:

[0066] S1, uniformly dispersing an anode catalyst and an anode hydrophobic binder in a hydroalcohol solution to form an anode catalyst slurry; the hydroalcohol solution may be water-isopropanol.

[0067] S2, coating the anode catalyst slurry on the anode gas diffusion layer to obtain an anode GDE;

[0068] S3, uniformly dispersing the cathode catalyst and the dissolved non-fluorinated polyamide-sulfonated imine polymer (FOS) solution in an organic solvent as a cathode catalyst slurry; the organic solvent may be N,N-dimethylacetamide (DMAC) and N-methylpyrrolidone (NMP).

[0069] S4, coating the cathode catalyst slurry on the cathode gas diffusion layer to obtain a cathode GDE;

[0070] S5, laminating the anode GDE, the proton exchange membrane and the cathode GDE in sequence, and compounding them by hot pressing to obtain a membrane electrode.

[0071] The solid content of the anode catalyst slurry and the cathode catalyst slurry is maintained at 0.2-0.25.

[0072] Example

[0073] The preparation method of the non-fluorinated polyamide-sulfonated imine polymer (FOS) in Example 1 and Comparative Examples 1-2 comprises the following steps:

[0074] Step 1: The synthesis process of 4-methyldiphenylsulfonyl imide (hereinafter referred to as product 1) is as follows: p-toluenesulfonamide (17.12 g, 100 mmol), sodium hydroxide (4.22 g, 105 mmol) and 150 mL of deionized water are added to a 250 mL double-necked round-bottom flask equipped with a reflux condenser. After the reaction mixture is stirred and evenly mixed at 95°C, benzenesulfonyl chloride (17.66 g, 100 mmol) is slowly added dropwise to the solution within 2 hours, and stirred at 95°C overnight. After that, the pH value of the solution is adjusted to 7 with dilute HCl, and the white precipitate is removed by filtration. The pH value of the solution is adjusted to 1 with dilute HCl again, and the white precipitate is obtained by filtration. Recrystallization is performed to obtain product 1, the mass of product 1 is 20.22 g, and the yield is about 65%.

[0075] Step 2: LiOH·H2O (2.045 g, 50 mmol) and product 1 (15.57 g, 50 mmol) were completely dissolved in deionized water (300 mL) at 95°C, and KMnO4 (16.583 g, 105 mmol) was slowly added into a 500 mL round-bottom flask within 2 h. The reaction mixture was stirred at 95°C overnight. After filtering to remove MnO2 and unreacted KMnO4, the filtrate was acidified with concentrated HCl, acidified 3 times, and the final product was collected. After vacuum drying at 100°C for 24 h, product 2 was obtained. The mass of product 2 was 14.47 g, and the yield was 84.9%.

[0076] Step 3: 5-(4-(N-phenylsulfonyl)sulfonamido)benzamido)isophthalic acid dimethyl ester (hereinafter referred to as product three): product two (13.654g, 40mmol), 5-aminoisophthalic acid dimethyl ester (8.368g, 40mmol), LiCl (3.2g, 4%), triphenyl phosphite TPP (10mL), NMP (40mL) and pyridine (PY, 30mL) were added to a 100mL double-necked round-bottom flask and stirred overnight at 100°C under an argon atmosphere. After the reaction was completed, the mixture was distilled under reduced pressure, then poured into 500mL of cold isopropanol, filtered to obtain a white precipitate, which was then washed with isopropanol and deionized water. The final product was vacuum dried at 100°C overnight to obtain product three, the mass of product three was 17.57g, and the yield was 82.3%.

[0077] Step 4: Product 3 is hydrolyzed in an alkaline aqueous solution to obtain sulfonyl imide diacid monomer (hereinafter referred to as SIDA): Product 3 (15.35 g, 20 mmol) and 40 mL of deionized water are added to a 150 mL round-bottom flask and stirred to dissolve. NaOH (4.8 g, 120 mmol) is then dissolved in 40 mL of deionized water and then added dropwise to the mixture within 2 h. The mixture is stirred at room temperature overnight. The pH of the solution is adjusted to 1 with concentrated HCl to obtain yellow powder SIDA (8.84 g, 87.6%), which is then dried at 100° C. in vacuo for 24 h.

[0078] Step 5: 4,4'-(9-fluorenyl)diphenylamine FDA (0.6969 g, 2 mmol), 1,8-octanedioic acid [2 (100-x)% mmol], SIDA (2x% mmol), LiCl (0.32 g, 4%) and triphenyl phosphite (TPP, 1 mL) were mixed with NMP (4 mL) and pyridine (3 mL) and stirred in an argon atmosphere for 3 h. After the reaction was completed, the mixture was cooled to 70 ° C and then poured into cold methanol (100 mL), filtered to obtain a light yellow precipitate, washed continuously with methanol and deionized water, and dried at 100 ° C under reduced pressure for 12 h. The yield of the obtained polymer FOS was above 92%.

[0079] Table 1

[0080]

[0081]

[0082] When the non-fluorinated polyamide-sulfonated imine polymer (FOS) in Example 1 and Comparative Examples 1-2 was prepared, x%=50%, and the molar ratio of SIDA, suberic acid and FDA was 1:1:2. The SEM image of FOS is shown in Figure 2 , NMR results are shown in Figure 3 The infrared spectra of FOS at different x values ​​are shown in Figure 4 .

[0083] Example 1

[0084] A method for preparing a high-temperature proton exchange membrane fuel cell membrane electrode assembly is as follows:

[0085] Preparation of gas diffusion layer: First, VulcanXC-72 carbon powder and PTFE emulsion were mixed, and an appropriate amount of ethanol was added. The slurry was prepared by ultrasonic stirring, and then applied to the surface of commercial Toray carbon paper. The carbon powder loading and PTFE content were determined by weighing. Finally, it was placed in a muffle furnace and heat treated at 340°C for 25 minutes, and the gas diffusion layer was obtained after cooling to room temperature.

[0086] Preparation of anode GDE (anode catalyst layer + anode gas diffusion layer): weigh the required Pt / C catalyst, add a small amount of deionized water to stir and moisten, then add a certain amount of PTFE aqueous alcohol solution, and obtain catalyst slurry after ultrasonic dispersion; use a pneumatic spray method to evenly coat the above slurry on the surface of the microporous layer of the anode gas diffusion layer.

[0087] Preparation of cathode GDE (cathode catalyst layer + cathode gas diffusion layer): weigh a certain amount of non-fluorinated polyamide-sulfonated imine block polymer molecules, add a certain amount of DMAC solution, and then stir at room temperature for more than 4 hours to ensure that it is fully dissolved to obtain a non-fluorinated polyamide-sulfonated imine solution. Weigh the required PtCo / C catalyst, add the required DMAC solution, ultrasonically disperse it evenly, then drop an appropriate amount of dissolved and dispersed non-fluorinated polyamide-sulfonated imine solution, and ultrasonically disperse and stir the mixed slurry again to ensure that the non-fluorinated polyamide-sulfonated imine molecules are evenly dispersed in the catalyst slurry to obtain a cathode catalyst layer catalyst slurry; the above slurry is evenly coated on the surface of the microporous layer of the cathode gas diffusion layer by a pneumatic spraying method to obtain a cathode catalyst layer containing non-fluorinated polyamide-sulfonated imine molecules.

[0088] The PBI / H3PO4 composite membrane was prepared by the immersion method: S1, the PBI membrane was cut into a certain size as needed; S2, the cut membrane was immersed in 85wt.% phosphoric acid at 120°C for a corresponding time; S3, the excess phosphoric acid on the membrane surface was absorbed with filter paper, and the membrane was quickly weighed to obtain the phosphoric acid adsorption capacity. The phosphoric acid adsorption capacity MPA / PBI (the mass of adsorbed phosphoric acid / the original mass of the polybenzimidazole membrane) of the membrane was investigated by the mass ratio of phosphoric acid to resin. The cycle S2→S3 was repeated until the phosphoric acid adsorption capacity reached 400wt.%.

[0089] The prepared electrodes (anode GDE, cathode GDE) and the PBI / H3PO4 composite membrane are stacked in a mold in a certain order, and then placed in a hot press to heat-press and mold the membrane electrode to obtain a fuel cell membrane electrode, which is then placed in a sealed bag and stored for later use.

[0090] The active area of ​​the membrane electrode is 4 cm 2 The composition and structure of the cathode and anode gas diffusion layers are the same, both consisting of a support layer and a microporous layer. The support layer is mainly Torray carbon paper with a thickness of 140 microns. The microporous layer is mainly composed of carbon powder and PTFE; the type of carbon powder is Vulcan XC-72; the loading of carbon powder in the microporous layer is 4 mg / cm 2 ; PTFE content 25%; microporous layer thickness 40 microns. The anode catalyst layer is composed of 30wt% Pt / C catalyst (Pt mass fraction is 30wt%) and PTFE, and the platinum loading is 0.3mg / cm 2The content of PTFE in the anode catalyst layer is 20%. The cathode catalyst layer is composed of 46.9wt% PtCo / C (Pt mass fraction is 46.9wt%) and FOS, and the Pt loading is 0.6mgPt / cm 2 , the FOS content is FOS / C=0.15.

[0091] Example 2

[0092] The difference between this embodiment and embodiment 1 is that in the high-temperature proton exchange membrane fuel cell membrane electrode assembly in embodiment 2, the FOS content of the cathode catalyst layer is FOS / C=0.10.

[0093] Comparative Example

[0094] Comparative Example 1

[0095] The difference between this comparative example and Example 1 is that in the high-temperature proton exchange membrane fuel cell membrane electrode assembly in Comparative Example 1, the FOS content of the cathode catalyst layer is FOS / C=0.20.

[0096] Comparative Example 2

[0097] The difference between this comparative example and Example 1 is that in the high-temperature proton exchange membrane fuel cell membrane electrode assembly in Comparative Example 2, the cathode catalyst layer is composed of only 46.9wt% PtCo / C, and the Pt loading is 0.6mgPt / cm 2 .

[0098] Performance Testing

[0099] With reference to GB / T 20042.5-2009, the polarization curve test of the obtained high-temperature proton exchange membrane fuel cell membrane electrode was carried out, and the specific operating conditions were: the single cell operating temperature was 160°C, the anode was fed with pure hydrogen, the cathode was fed with atmospheric pressure air, and the cathode / anode feeds were 3 / 1.5 times the stoichiometric ratio, respectively.

[0100] According to GB / T 20042.5-2009, the membrane electrode impedance of high-temperature proton exchange membrane fuel cell was tested. The specific operating conditions were: the single cell operating temperature was 160°C, the anode was fed with pure hydrogen, the cathode was fed with atmospheric pressure air, and the cathode / anode feeds were 3 / 1.5 times the stoichiometric ratio @0.5A cm -2 , the discharge current density is 0.5A cm -2 .

[0101] Test results are shown in Figures 4-5Among them, no PTFE and no FOS means that the solid component in the preparation of the catalyst layer slurry is only 46.9wt% PtCo / C, representing Comparative Example 2; FOS / C=0.10, 0.15, 0.20 means that the mass ratio of the non-fluorinated polyamide-sulfonated imide (FOS) to carbon in the preparation of the catalyst layer slurry is 0.10, 0.15, 0.20, representing Example 2, Example 1 and Comparative Example 1, respectively.

[0102] See also Figure 5 The membrane electrode polarization characteristic curves of the cathode composition of Example 1-2 of the present invention and the cathode composition of Comparative Example 1-2 were measured. Figure 5 It can be seen that at 0.1A / cm 2 Under the conditions of 0.5A / cm2, the voltages of the membrane electrodes corresponding to the cathode compositions of Examples 1 and 2 of the present invention and the cathode compositions of Comparative Examples 1 and 2 were measured to be 0.618V, 0.637V, 0.581V and 0.619V respectively; under the conditions of 0.5A / cm2, the voltages of the membrane electrodes corresponding to the cathode compositions of Examples 1 and 2 of the present invention were 0. 2 Under the conditions of 0.5% to 1.5% RH, the voltages of the membrane electrodes corresponding to the cathode compositions of Examples 1 and 2 of the present invention and those of Comparative Examples 1 and 2 were measured to be 0.450 V, 0.438 V, 0.307 V and 0.396 V, respectively; the maximum power densities of the membrane electrodes corresponding to the cathode compositions of Examples 1 and 2 of the present invention and those of Comparative Examples 1 and 2 were measured to be 0.264 W / cm 2 , 0.239W / cm 2 , 0.156W / cm 2 and 0.209W / cm 2 Compared with the membrane electrode with cathode composition in comparative example 2, the maximum power density of the membrane electrode with non-fluorinated polyamide-sulfonated imine cathode catalyst layer in embodiment 1 of the present invention is 55 mW / cm higher than that of the corresponding membrane electrode with cathode composition in comparative example 2. 2 In the high current density region, at the same current density, the battery voltage of Example 1 of the present invention is higher than the membrane electrode voltage corresponding to the cathode composition of Comparative Example 2, so that the overall performance of the battery is higher.

[0103] See also Figure 6From the impedance spectrum, it can be seen that compared with Comparative Example 2, Example 1-2 is significantly reduced in the high, medium and low frequency regions of the impedance spectrum. Although both use the same anode composition, there is a gap in the anode impedance part, which shows that FOS has an effect on the redistribution of phosphoric acid. The non-fluorinated polyamide-sulfonated imine polymer (FOS) in the cathode part retains more phosphoric acid in the cathode part, which increases the anode impedance. However, the most significant impedance difference is the charge transfer resistance of the cathode. Example 1-2 is significantly lower than Comparative Example 2. This is mainly due to the introduction of non-fluorinated polyamide-sulfonated imine polymer (FOS) into the cathode part of Example 1-2. Due to its good proton conductivity, it enhances the proton conductivity of the cathode catalyst layer, so that the charge transfer barrier at the three-phase interface of the catalyst layer is reduced. At the same time, its retention effect on PA enables it to still operate stably in the low-frequency mass transfer area.

[0104] In summary, when the present invention uses non-fluorinated polyamide-sulfonated imine polymer (FOS) as the cathode catalyst layer ionomer, the non-fluorinated polyamide-sulfonated imine polymer acts as a carrier for proton transfer by introducing sulfonyl imide groups. In addition, the block structure of FOS rigidity and flexible chains enables it to effectively retain PA in the catalyst layer, which greatly ensures the effective distribution of phosphoric acid in the catalyst layer, greatly increases the three-phase interface in the electrode, and at the same time reduces the phosphoric acid loss problem caused by long-term operation of the battery, thereby improving the catalyst utilization rate and the performance and life of the battery. The introduction of this non-fluorinated polyamide-sulfonated imine polymer reduces the dependence of the catalyst layer on traditional polymer ionomers, while improving the proton transfer efficiency of the three-phase interface, it can optimize the multiphase material transfer of the catalyst layer, and solve the phosphoric acid distribution and loss problems existing in the traditional catalyst layer.

[0105] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0106] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.

Claims

1. A method for preparing a block polymer for a cathode catalyst layer, It is characterized in that include: Step 1: Add p-toluenesulfonamide, sodium hydroxide and deionized water to a reaction vessel equipped with a reflux condenser; after the reaction mixture is stirred and evenly mixed at 95±5°C, slowly add benzenesulfonyl chloride to the solution, and stir at 95±5°C until the reaction is complete; then adjust the pH value of the solution to neutral, filter out the white precipitate, adjust the pH value of the solution to 1-2 again, filter out the white precipitate, and recrystallize to obtain product 1; Step 2: LiOH·H 2 O and the product were completely dissolved in deionized water, and KMnO 4 Slowly add into the reaction vessel, stir the reaction mixture at 95±5°C to complete the reaction, filter, acidify the filtrate, collect the final product, and vacuum dry to obtain product 2; Step 3: Add the product II, 5-aminoisophthalic acid dimethyl ester, LiCl, triphenyl phosphite TPP, pyridine, and a mixture of aprotic organic solvents into a reaction vessel, and stir at 100±5°C under an inert atmosphere to complete the reaction; after the reaction is completed, the mixture is distilled under reduced pressure, and then poured into a sufficient amount of cold isopropanol, filtered to obtain a white precipitate, washed, and vacuum dried to obtain the product III; Step 4: Add product 3 and deionized water to a reaction container and stir to dissolve; then dissolve NaOH in deionized water and then dropwise add it to the mixture, stir overnight at room temperature, adjust the pH of the solution to 1-2 with concentrated HCl to obtain a yellow powder, and vacuum dry to obtain SIDA; Step 5: Mix 4,4'-(9-fluorenylidene)diphenylamine FDA, 1,8-octanedioic acid, SIDA, LiCl, triphenyl phosphite, pyridine and aprotic organic solvent, and stir to react in an inert atmosphere; after the reaction is completed, cool the mixture to 70±5°C, then pour it into cold methanol, filter to obtain a light yellow precipitate, wash it continuously with methanol and deionized water, and dry it under reduced pressure to obtain a non-fluorinated polyamide-sulfonated imine polymer FOS for the cathode catalyst layer.

2. The method for preparing a block polymer for a cathode catalyst layer according to claim 1, It is characterized in that In step 1, the molar ratio of p-toluenesulfonamide, benzenesulfonyl chloride and sodium hydroxide is (1-1.05):1:(1-1.05); and / or In step 3, the molar ratio of product 2 to dimethyl 5-aminoisophthalate is 1:1 to 1.05; and / or In step 5, the molar ratio of 4,4'-(9-fluorenylene)diphenylamine FDA, 1,8-octanedioic acid and SIDA is 1: x%:(100-x)%, x%=10% to 90%.

3. A block polymer for a cathode catalyst layer, It is characterized in that The method for preparing the block polymer for the cathode catalyst layer according to claim 1 or 2 is used to prepare the block polymer.

4. A cathode catalyst layer slurry, It is characterized in that It comprises a cathode catalyst and the non-fluorinated polyamide-sulfonated imine block polymer FOS as claimed in claim 3, wherein the mass ratio of the non-fluorinated polyamide-sulfonated imine block polymer FOS to the carbon carrier in the cathode catalyst is (5-15):

100.

5. A cathode gas diffusion electrode, It is characterized in that It comprises a cathode gas diffusion layer and a cathode catalyst layer applied on one side of the microporous layer of the cathode gas diffusion layer; the cathode catalyst layer is prepared by using the cathode catalyst layer slurry according to claim 4.

6. A membrane electrode, It is characterized in that It comprises a cathode GDE, a proton exchange membrane and an anode GDE; the cathode GDE comprises a cathode gas diffusion layer and a cathode catalyst layer applied on one side of the microporous layer on the cathode gas diffusion layer; the anode GDE comprises an anode gas diffusion layer and an anode catalyst layer applied on one side of the microporous layer on the anode gas diffusion layer; the cathode catalyst layer is prepared by the cathode catalyst layer slurry described in claim 4.

7. The membrane electrode according to claim 6, It is characterized in that The anode catalyst layer comprises an anode catalyst and an anode hydrophobic binder, wherein the anode catalyst comprises at least one of Pt / C, PtFe / C or PtCo / C; the anode hydrophobic binder is at least one of polytetrafluoroethylene PTFE, polyvinylidene fluoride PVDF, tetrafluoroethylene-hexafluoropropylene copolymer FEP, ethylene-chlorotrifluoroethylene copolymer ECTFE, ethylene-tetrafluoroethylene copolymer ETFE, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer PFA, and polydimethylsiloxane PDMS.

8. The membrane electrode according to claim 6, It is characterized in that The cathode catalyst is at least one of Pt / C, PtFe / C or PtCo / C; The proton exchange membrane is a polybenzimidazole membrane PBI, and the PBI is treated by doping with phosphoric acid.

9. A method for preparing a membrane electrode, It is characterized in that include: S1, uniformly dispersing an anode catalyst and an anode hydrophobic binder in a water-alcohol solution to form an anode catalyst slurry; S2, coating the anode catalyst slurry on the anode gas diffusion layer to obtain an anode GDE; S3, uniformly dispersing the cathode catalyst and the dissolved non-fluorinated polyamide-sulfonated imine polymer FOS solution in an organic solvent to form a cathode catalyst slurry; S4, coating the cathode catalyst slurry on the cathode gas diffusion layer to obtain a cathode GDE; S5, laminating the anode GDE, the proton exchange membrane and the cathode GDE in sequence, and compounding them by hot pressing to obtain a membrane electrode.

10. A high temperature proton exchange membrane fuel cell, It is characterized in that The cathode gas diffusion electrode according to claim 5 is used, or the membrane electrode according to claim 6 is used.

Citation Information

Patent Citations

  • Catalysis layer of proton exchange membrane fuel cell and preparation method

    CN101722046A

  • Crosslinkable composition comprising photobase generators

    CN104254581A

  • Preparation method for catalyst slurry for solid polymer electrolyte water electrolysis membrane electrode

    CN108579818A

  • Membrane electrode containing ether-bond-free polybenzimidazole ionomer and based on high-temperature proton exchange membrane and preparation method of membrane electrode

    CN116970170A