Alumina film and composite positive current collector

By using alumina film with high transmittance and moderate alumina layer thickness in the positive electrode current collector of lithium battery and manufacturing it in vacuum evaporation equipment, the problem of low production quality of the positive electrode current collector of lithium battery is solved and hole identification is improved Accuracy and battery welding strength improve the overall performance of the battery.

CN118979222APending Publication Date: 2024-11-19SHENZHEN JINJIA GRP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975230.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The production quality of the positive current collector of existing lithium batteries is low, and the inaccurate hole identification leads to a decrease in the qualification rate of the finished product.

Method used

Design an alumina film, including an alumina layer provided on the upper and lower surfaces of the support layer, with a transmittance of 80% to 98%, a thickness of an alumina layer of 30nm to 60nm, and an aluminum content is added to the aluminum metal layer to increase the binding force , combined with vacuum evaporation equipment for thin film manufacturing.

Benefits of technology

It improves the accuracy of hole recognition of alumina films in CCD detection, reduces the size and number of finished holes, and improves production quality and battery welding strength and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979222A_ABST
    Figure CN118979222A_ABST
Patent Text Reader

Abstract

According to the aluminum oxide film and the composite positive electrode current collector provided by the invention, the aluminum oxide film comprises a supporting layer, aluminum oxide layers are arranged on the upper surface and the lower surface of the supporting layer, the transmittance of the supporting layer is 80%-98%, and the thickness of the aluminum oxide layer on the supporting layer is 30 nm-60 nm. In the invention, the supporting layer (film) is provided with the upper surface and the lower surface in the thickness direction, the aluminum oxide layers are arranged on the upper surface and the lower surface, so that the aluminum oxide film is formed, the inventor finds that the supporting layer with the transmittance of 80%-98% is adopted, then the aluminum oxide with the thickness of 30 nm-60 nm is formed on the supporting layer, and when the aluminum oxide film is subjected to CCD (Charge-Coupled Device) detection, the transmittance of the aluminum oxide film can be greatly improved. The holes are more easily and accurately recognized, the situation that the qualified rate of final finished products is affected due to too many and too large finished product holes caused by follow-up hierarchical machining is avoided, and therefore the production quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium batteries, and in particular to an aluminum oxide film and a composite positive electrode current collector. Background Art

[0002] The composite positive electrode current collector is a current collector used in the positive electrode of a lithium battery. The present invention aims to design a new aluminum oxide film for the composite positive electrode current collector of a lithium battery, which can improve the production quality. Summary of the invention

[0003] In view of the above-mentioned prior art, an object of the present invention is to provide an aluminum oxide film and a composite positive electrode current collector, which can improve production quality.

[0004] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0005] The invention provides an aluminum oxide film, comprising a support layer, wherein the upper and lower surfaces of the support layer are both provided with an aluminum oxide layer, the transmittance of the support layer is 80% to 98%, and the thickness of the aluminum oxide layer on the support layer is 30nm to 60nm.

[0006] Furthermore, in the aluminum oxide film, an aluminum metal layer is disposed on the aluminum oxide layer.

[0007] Furthermore, the aluminum oxide film, the oxide filter layer comprises 80% to 90% aluminum oxide and 20% to 10% aluminum.

[0008] Furthermore, the aluminum oxide film, the aluminum metal layer includes 80% to 90% aluminum and 20% to 10% aluminum oxide.

[0009] Furthermore, in the aluminum oxide film, the aluminum oxide content in the aluminum metal layer is less than the aluminum content in the aluminum oxide layer.

[0010] Furthermore, in the aluminum oxide film, in the aluminum oxide layer, the aluminum oxide content is N, the aluminum content is M, in the aluminum metal layer, the aluminum metal content is K, and the aluminum oxide content is I, then (K*M)>(I*N).

[0011] Furthermore, for the aluminum oxide film, the dyne value of the outer surface of the aluminum oxide layer is 44-46.

[0012] The present invention also provides a composite positive electrode current collector, comprising the aluminum oxide film as described above, wherein a metal aluminum layer is arranged on the surface of the aluminum oxide film.

[0013] Furthermore, in the composite positive electrode current collector, the aluminum oxide film includes a support layer, the upper surface and the lower surface of the support layer are both provided with an aluminum oxide layer, and the density of the metal aluminum layer is greater than the density of the aluminum oxide layer.

[0014] Furthermore, in the composite positive electrode current collector, the support layer is a film made of polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber or polycarbonate material, the thickness of the support layer is 3um-8um, and the density of the alumina layer is 2 to 4 times the density of the support layer.

[0015] The present invention also provides a vacuum evaporation device for manufacturing the above-mentioned aluminum oxide film, including a vacuum chamber, wherein an evaporation boat, a unwinding roller, a guide roller, a bending roller, a water-cooled roller, a tension roller and a winding roller are arranged in the vacuum chamber, the unwinding roller is arranged below the winding roller, and a film is mounted on the unwinding roller. The film released by the unwinding roller passes around the guide roller, the bending roller, the water-cooled roller, and the tension roller in sequence, and is finally wound up by the winding roller. The bending roller and the guide roller are located above the evaporation boat, and an OD transmittance detector is arranged between the tension roller and the water-cooled roller.

[0016] Furthermore, in the vacuum evaporation equipment, a front mirror roller is also provided in the vacuum chamber, and the front mirror roller is provided between the water-cooled roller and the tension roller, and the film rolled out from the water-cooled roller passes through the front mirror roller and the tension roller in sequence.

[0017] Furthermore, in the vacuum evaporation equipment, the OD transmittance detector is arranged between the front mirror roller and the tension roller.

[0018] Furthermore, in the vacuum evaporation equipment, a rear mirror roller is also provided in the vacuum chamber, and the rear mirror roller is provided between the tension roller and the winding roller, and the film between the tension roller and the winding roller passes through the rear mirror roller.

[0019] Furthermore, in the vacuum evaporation equipment, a pay-out roller group is also provided in the vacuum chamber, and the pay-out roller group is provided between the pay-out roller and the guide roller, and the film between the pay-out roller and the guide roller passes through the pre-pay-out roller group.

[0020] Furthermore, in the vacuum evaporation equipment, a front-retracting roller group is also provided in the vacuum chamber, and the front-retracting roller group is provided between the rear mirror roller and the winding roller, and the film between the rear mirror roller and the winding roller passes through the front-retracting roller group.

[0021] Furthermore, in the vacuum evaporation equipment, the pay-out roller group includes a first roller, a second roller and a third roller, and the front rewinding roller group includes a fourth roller, a fifth roller, a sixth roller and a seventh roller. The film paid out by the pay-out roller sequentially passes around the lower sides of the first roller, the second roller and the third roller, and then sequentially passes around the upper side of the guide roller, the upper side of the water-cooled roller, the lower side of the front mirror roller, the upper side of the tension roller, the lower side of the rear mirror roller, and then passes through the lower side of the fourth roller, the upper side of the fifth roller, the upper side of the sixth roller and the upper side of the seventh roller, and is finally rewound by the rewinding roller.

[0022] Compared with the prior art, the present invention provides an aluminum oxide film and a composite positive electrode current collector, wherein the aluminum oxide film includes a support layer, the upper surface and the lower surface of the support layer are both provided with an aluminum oxide layer, the transmittance of the support layer is 80% to 98%, and the thickness of the aluminum oxide layer on the support layer is 30nm to 60nm. In the present invention, the support layer (film) has two upper and lower surfaces in the thickness direction, and aluminum oxide layers are provided on the upper and lower surfaces to form an aluminum oxide film. The inventor found that by using a support layer with a transmittance of 80%-98%, and then forming an aluminum oxide with a thickness of 30nm-60nm on the support layer, the aluminum oxide film is easier to accurately identify holes when passing through CCD (Charge-Coupled Device) detection, avoiding the subsequent layer processing resulting in too many and too large holes in the finished product, affecting the final qualified rate of the finished product, thereby improving the production quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0024] Figure 1 This is a schematic diagram of the structure of the aluminum oxide film provided by the present invention.

[0025] Figure 2 This is a schematic diagram of the structure of the composite positive electrode current collector provided by the present invention.

[0026] Figure 3 This is a schematic structural diagram of the vacuum evaporation equipment provided by the present invention.

[0027] Description of Figure Numbers:

[0028] Support layer 10

[0029] Aluminum oxide layer 20

[0030] Aluminum metal layer 30

[0031] Metal aluminum layer 40

[0032] Vacuum Chamber 101

[0033] Evaporation boat 102

[0034] Unwinding roller 103

[0035] First roller 104

[0036] Second roller 105

[0037] The third roller 106

[0038] Guide roller 107

[0039] Bending roller 108

[0040] Water-cooled roller 109

[0041] Front mirror roller 110

[0042] OD transmittance detector 111

[0043] Tension roller 112

[0044] Rear mirror roller 113

[0045] Fourth roller 114

[0046] Fifth roller 115

[0047] Sixth Roller 116

[0048] Seventh Roll 117

[0049] Winding roller 118 DETAILED DESCRIPTION

[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0052] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0053] like Figure 1 As shown, the present invention provides an aluminum oxide film and a composite positive electrode current collector, wherein the aluminum oxide film includes a support layer 10, and the upper and lower surfaces of the support layer 10 are both provided with an aluminum oxide layer 20, the transmittance of the support layer 10 is 80% to 98%, and the thickness of the aluminum oxide layer 20 on the support layer 10 is 30nm to 60nm. In the present invention, the support layer 10 (film) has two upper and lower surfaces in the thickness direction, and the aluminum oxide layer 20 is provided on the upper and lower surfaces to form an aluminum oxide film. The inventor found that by using a support layer 10 with a transmittance of 80%-98%, and then forming an aluminum oxide with a thickness of 30nm-60nm on the support layer 10, the aluminum oxide film is more likely to accurately identify the holes when passing through the CCD (Charge-Coupled Device) detection, avoiding the subsequent layer processing causing too many and too large holes in the finished product, affecting the qualified rate of the final finished product, and the present invention is conducive to the subsequent judgment of the product holes, and is conducive to screening out unqualified products, thereby improving the production quality.

[0054] Specifically, the support layer 10 can be made of polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, polycarbonate, etc. Further, in the aluminum oxide film provided by the present invention, an aluminum metal layer 30 is provided on the aluminum oxide layer 20.

[0055] Further, in the aluminum oxide film provided by the present invention, the oxide filter layer includes 80% to 90% aluminum oxide and 20% to 10% aluminum. With this structure, the anti-oxidation ability of the aluminum layer can be improved, and the bonding force between the aluminum metal layer 30 and the aluminum oxide layer 20 can be improved. Further, in the aluminum oxide film provided by the present invention, the aluminum metal layer 30 includes 80% to 90% aluminum and 20% to 10% aluminum oxide. With this structure, the bonding force between the aluminum metal layer 30 and the aluminum oxide layer 20 can be improved.

[0056] Furthermore, in the aluminum oxide film provided by the present invention, the dyne value of the outer surface of the aluminum oxide layer 20 is 44 to 46. This is conducive to further improving the bonding force between the aluminum metal layer 30 and the aluminum oxide layer 20.

[0057] like Figure 2 As shown, the present invention also provides a composite positive electrode current collector, comprising the aluminum oxide film provided by the present invention as above, and a metal aluminum layer 40 is arranged on the surface of the aluminum oxide film. Further, the composite positive electrode current collector provided by the present invention, the aluminum oxide film includes a support layer 10, and the upper surface and the lower surface of the support layer 10 are both provided with an aluminum oxide layer 20, and the density of the metal aluminum layer 40 is greater than the density of the aluminum oxide layer 20. Under the same volume conditions, the quality of the metal aluminum layer of the present application is higher, which can improve the flow capacity of the metal aluminum layer, and thus the current resistance is higher. The present application is provided with a slurry coating area specially used for coating active slurry and a welding area for welding the pole ear on the composite current collector, wherein the aluminum metal density of the welding area is greater than the aluminum metal density of the slurry coating area, so that the flow capacity of the welding area can be increased, and the welding strength of the pole ear can be improved. Furthermore, the density of aluminum oxide in the tab welding area is lower than that of aluminum metal in the tab welding area, while the aluminum metal density in the tab welding area is greater than that in the coating area. This has the advantage that since the aluminum metal density in the tab welding area is greater than that of aluminum oxide, it is convenient to conduct the aluminum metal in the tab welding area, which is beneficial to improve the battery energy density, improve the welding capacity, and also improve the current gathering capacity here.

[0058] Further, in the composite positive electrode current collector provided by the present invention, the support layer 10 is a film made of polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber or polycarbonate material, and the thickness of the support layer 10 is 3um-8um. Preferably, the density of the aluminum oxide layer 20 is 2 to 4 times the density of the support layer 10. This is conducive to preventing foreign substances from entering the support layer 10.

[0059] Furthermore, in the aluminum oxide film provided by the present invention, the aluminum oxide content in the aluminum metal layer 30 is less than the aluminum content in the aluminum oxide layer 20. In this way, in the composite current collector, the weight of the composite current collector can be reduced and the battery energy density can be improved. Further, in the aluminum oxide film provided by the present invention, in the aluminum oxide layer 20, the aluminum oxide content is N, the aluminum content is M, and in the aluminum metal layer 30, the aluminum metal content is K, and the aluminum oxide content is I, then (K*M)>(I*N). In this way, in the composite current collector, the conductivity of the entire composite current collector can be made better and have better convergence capacity.

[0060] Furthermore, in the present invention, a PP (polypropylene) film is preferably used as the support layer 10, because it is more acid- and alkali-resistant, and can greatly improve the service life of the current collector of the present invention together with the coating structure of the present invention. The PP film of the present invention is preferably 3um-8um, which can reduce the mass of the current collector of the present invention and improve the energy density of the battery.

[0061] like Figure 3 As shown, the present invention provides a vacuum evaporation device for manufacturing the above-mentioned aluminum oxide film, including a vacuum chamber 101, wherein an evaporation boat 102, a pay-off roller 103, a guide roller 107, a bending roller 108, a water-cooled roller 109, a tension roller 112 and a winding roller 118 are arranged in the vacuum chamber 101, the pay-off roller 103 is arranged below the winding roller 118, and a film is mounted on the pay-off roller 103. The film paid out by the pay-off roller 103 passes through the guide roller 107, the bending roller 108, the water-cooled roller 109, the tension roller 112 in sequence, and is finally wound up by the winding roller 118. The bending roller 108 and the guide roller 107 are located above the evaporation boat 102, and an OD (optical density) transmittance detector is arranged between the tension roller 112 and the water-cooled roller 109. The winding roller 118 is used to wind up the film, and the unwinding roller 103 is used to unwind the film. The unwinding roller 103 and the winding roller 118 are located on the same side in the vacuum chamber 101, which is convenient for taking and placing the film. The present invention is convenient for better evaporation of the film, and an OD transmittance detector 111 is installed in the vacuum evaporation equipment, so that the thickness of aluminum oxide can be detected online.

[0062] Optical density (OD) is defined as a characterization of the material's ability to block light. It is the logarithm of the ratio of incident light to transmitted light, or the logarithm of the inverse of light transmittance. The calculation formula is OD = log10 (incident light / transmitted light) or OD = log10 (1 / transmittance) 12. In fields such as biology, medicine, and chemistry, OD values ​​are used to evaluate the degree to which light penetrates a substance1. Transmittance refers to the ability of light to penetrate a medium, which is the percentage of the luminous flux passing through a transparent or translucent body to its incident luminous flux2. It indicates the efficiency of a material in transmitting light. Simply put, optical density (OD) indicates the degree of light absorption by a substance, while transmittance indicates the efficiency of light passing through a substance. There is an inverse relationship between the two, that is, the greater the optical density, the smaller the transmittance; the smaller the optical density, the greater the transmittance. Through OD detection of aluminum oxide film, the transmittance is obtained through the OD value.

[0063] Furthermore, in the vacuum evaporation equipment provided by the present invention, a front mirror roller 110 is further provided in the vacuum chamber 101, and the front mirror roller 110 is provided between the water-cooled roller 109 and the tension roller 112, and the film rolled out from the water-cooled roller 109 passes through the front mirror roller 110 and the tension roller 112 in sequence. The tension roller 112 is conducive to maintaining the tension of the film.

[0064] Furthermore, in the vacuum evaporation equipment provided by the present invention, the OD transmittance detector 111 is disposed between the front mirror roller 110 and the tension roller 112. The OD transmittance detector 111 is used to detect the transmittance of the film.

[0065] Furthermore, in the vacuum evaporation device provided by the present invention, a rear mirror roller 113 is further provided in the vacuum chamber 101, and the rear mirror roller 113 is provided between the tension roller 112 and the winding roller 118, and the film between the tension roller 112 and the winding roller 118 passes through the rear mirror roller 113. The mirror roller plays the role of supporting the film on the one hand, and can also play the role of flattening the film at the same time. When the film is flattened, the film is not easily scratched due to its smooth surface.

[0066] Furthermore, in the vacuum evaporation equipment provided by the present invention, a pay-out roller group is further provided in the vacuum chamber 101, and the pay-out roller group is provided between the pay-out roller 103 and the guide roller 107, and the film between the pay-out roller 103 and the guide roller 107 passes through the pre-pay-out roller group. The provision of the pay-out roller group is conducive to keeping the film surface of the film flat during unwinding.

[0067] Furthermore, in the vacuum evaporation equipment provided by the present invention, a front retracting roller group is further provided in the vacuum chamber 101, and the front retracting roller group is provided between the rear mirror roller 113 and the winding roller 118, and the film between the rear mirror roller 113 and the winding roller 118 passes through the front retracting roller group. The provision of the front retracting roller group is conducive to keeping the film surface of the film flat when unwinding.

[0068] Furthermore, in the vacuum evaporation equipment provided by the present invention, the pay-out roller group includes a first roller 104, a second roller 105 and a third roller 106, and the front rewinding roller group includes a fourth roller 114, a fifth roller 115, a sixth roller 116 and a seventh roller 117. The film paid out by the pay-out roller 103 successively bypasses the lower sides of the first roller 104, the second roller 105 and the third roller 106, and then successively bypasses the upper side of the guide roller 107, the upper side of the water-cooled roller 109, the lower side of the front mirror roller 110, the upper side of the tension roller 112, the lower side of the rear mirror roller 113, and then passes successively through the lower side of the fourth roller 114, the upper side of the fifth roller 115, the upper side of the sixth roller 116 and the upper side of the seventh roller 117, and is finally rewound by the rewinding roller 118. The first roller 104, the second roller 105 and the third roller 106 of the present invention are not in a straight line, and the fifth roller 115, the sixth roller 116 and the seventh roller 117 are not in a straight line. The roller diameter of the water-cooled roller 109 is larger than the roller diameter of the tension roller 112, the roller diameter of the tension roller 112 is larger than the roller diameter of the guide roller 107, the bending roller 108 is located below or to the lower right of the water-cooled roller 109, and the front mirror roller 110 is located to the upper right of the water-cooled roller 109, so that the contact area between the film and the water-cooled roller 109 is larger.

[0069] The present invention also provides a device for producing the above-mentioned composite current collector. To produce the above-mentioned composite current collector, the above-mentioned aluminum oxide film is placed in a vacuum evaporation device and coated in a crucible manner, that is, the evaporation boat 102 in the above-mentioned vacuum coating equipment for producing the aluminum oxide film is replaced with a crucible. The advantage of this is that a thicker metallic aluminum can be formed on the aluminum oxide film at one time, thereby improving the coating efficiency.

[0070] In summary, the present invention provides an aluminum oxide film and a composite positive electrode current collector, wherein the aluminum oxide film provided by the present invention includes a support layer, the upper surface and the lower surface of the support layer are both provided with an aluminum oxide layer, the transmittance of the support layer is 80% to 98%, and the thickness of the aluminum oxide layer on the support layer is 30nm to 60nm. In the present invention, the support layer (film) has two upper and lower surfaces in the thickness direction, and aluminum oxide layers are provided on the upper and lower surfaces to form an aluminum oxide film. The inventor found that a support layer with a transmittance of 80%-98% is used, and then an aluminum oxide with a thickness of 30nm-60nm is formed on the support layer, so that the aluminum oxide film is easier to accurately identify the holes when it is detected by CCD (Charge-Coupled Device), avoiding the subsequent layer processing causing too many and too large holes in the finished product, affecting the qualified rate of the final finished product, and the present invention is conducive to the subsequent judgment of the product holes, and is conducive to screening out unqualified products, thereby improving the production quality.

[0071] The composite positive electrode current collector provided by the present invention comprises the aluminum oxide film provided by the present invention as above, and a metal aluminum layer is arranged on the surface of the aluminum oxide film. Further, the composite positive electrode current collector provided by the present invention comprises a support layer, and the upper and lower surfaces of the support layer are both provided with an aluminum oxide layer, and the density of the metal aluminum layer is greater than the density of the aluminum oxide layer. Under the condition of the same volume, the composite current collector of the present application has a larger mass and a higher current resistance.

[0072] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. An aluminum oxide film, characterized in that: It comprises a supporting layer, wherein the upper surface and the lower surface of the supporting layer are both provided with an aluminum oxide layer, the transmittance of the supporting layer is 80% to 98%, and the thickness of the aluminum oxide layer on the supporting layer is 30nm to 60nm.

2. The aluminum oxide film according to claim 1, characterized in that: An aluminum metal layer is disposed on the aluminum oxide layer.

3. The aluminum oxide film according to claim 2, characterized in that: The oxide filter layer comprises 80% to 90% of aluminum oxide and 20% to 10% of aluminum.

4. The aluminum oxide film according to claim 3, characterized in that: The aluminum metal layer includes 80% to 90% aluminum and 20% to 10% aluminum oxide.

5. The aluminum oxide film according to claim 4, characterized in that: The aluminum oxide content in the aluminum metal layer is less than the aluminum content in the aluminum oxide layer.

6. The aluminum oxide film according to claim 5, characterized in that: In the aluminum oxide layer, the content of aluminum oxide is N, and the content of aluminum is M. In the aluminum metal layer, the content of aluminum metal is K, and the content of aluminum oxide is I. Then (K*M)>(I*N).

7. The aluminum oxide film according to any one of claims 2 to 6, characterized in that: The dyne value of the outer surface of the aluminum oxide layer is 44-46.

8. A composite positive electrode current collector, characterized in that: It comprises the aluminum oxide film as described in any one of claims 1 to 7, wherein a metal aluminum layer is arranged on the surface of the aluminum oxide film.

9. The composite positive electrode current collector according to claim 8, characterized in that: The aluminum oxide film comprises a supporting layer, the upper surface and the lower surface of the supporting layer are both provided with an aluminum oxide layer, and the density of the metal aluminum layer is greater than the density of the aluminum oxide layer.

10. The composite positive electrode current collector according to any one of claims 8 to 9, characterized in that: The support layer is a film made of polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber or polycarbonate material. The thickness of the support layer is 3um-8um, and the density of the aluminum oxide layer is 2 to 4 times the density of the support layer.