Preparation method of polyimide powder and polyimide powder prepared by same

By using a mixed solvent of polar organic solvent and a high boiling point aromatic solvent in the preparation of polyimide powder, the problems of low imidation degree and poor mechanical properties are solved, and high imidation is achieved and excellent mechanical properties.

CN118984847APending Publication Date: 2024-11-19PI ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033171.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-11
Filing Date
2023-04-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing polyimide powder preparation methods have problems such as low degree of imidation, high water content and poor mechanical properties, and additional dehydration agents or catalysts are required, so the process efficiency is low.

Method used

Imide reaction is carried out using a mixed solvent containing polar organic solvents and high-boiling aromatic solvents, and polyimide powder is formed by high-temperature imidation, which avoids the need to add dehydrating agents or catalysts alone, and increases imide calcification and inherent viscosity.

Benefits of technology

High imidation rate and excellent intrinsic viscosity are achieved, and the mechanical properties of polyimide powder and the tensile strength, elongation, modulus and flexural strength of molded products are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005075694070000111
    Figure BDA0005075694070000111
Patent Text Reader

Abstract

Provided is a method for producing a polyimide powder having excellent intrinsic viscosity and capable of promoting imidization by controlling a polymerization reaction using a mixed solvent including a polar organic solvent and a high-boiling aromatic hydrocarbon solvent, the invention also provides the polyimide powder prepared by the preparation method of the polyimide powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for preparing a polyimide powder and the polyimide powder prepared by the method, and more specifically, to a method for preparing a polyimide powder using a mixed solvent containing a polar organic solvent and an aromatic hydrocarbon solvent with a high boiling point, and the polyimide powder prepared by the method. Background Art

[0002] With the development of advanced technology, high heat-resistant polymer materials, such as polyimide and its analogs, are indispensable materials for products that pursue miniaturization and lightweight, high performance and high reliability, and such materials are widely used in the form of films, molded parts, fibers, coatings, adhesives and composite materials and their analogs in industries such as aerospace, aviation, electronics / electrical appliances, automobiles, precision equipment and the like. Based on the chemical stability of the imide ring, polyimide has excellent mechanical strength, chemical resistance, weather resistance and heat resistance. In addition, polyimide has the advantages of easy synthesis, the possibility of being made into thin films, and the lack of cross-linking groups during curing. Due to its excellent electrical properties, polyimide has attracted much attention as a high-functional polymer material in various fields from microelectronics to optics.

[0003] Recently, in the field of displays, considerable attention has been paid to the lightweight and miniaturization of products, but the currently used glass substrates have the disadvantages of being heavy, fragile, and difficult to process continuously. In this regard, polyimide substrates having advantages such as being lightweight, flexible, and capable of continuous processing can be prepared as a substitute for glass substrates, and can also be used to form insulating films and protective coating agents for semiconductor devices, surface protective materials and base resins for flexible circuit boards and integrated circuits, and interlayer insulating films and protective films for fine circuits. In particular, when used as a coating material, a molded body of, for example, a polyimide film bonded with an adhesive or a liquid polyimide resin solution or the like can be used.

[0004] In the general method of synthesizing polyimide, firstly, a polyamic acid as a precursor is synthesized by the reaction between a dianhydride acid and a diamine, and then the polyamic acid is imidized. The synthesis of polyamic acid is completed by the ring-opening and polyaddition reaction between a diamine and a dianhydride dissolved in a solvent to prepare polyamic acid. At this time, the reaction solvent used is mainly a polar organic solvent. Polyimide is made by imidizing the synthesized polyamic acid through dehydration and ring closure reaction using a chemical or thermal method.

[0005] The chemical imidization method is to add a chemical dehydrating agent represented by anhydride, such as acetic anhydride or its analogues, and an imidization catalyst represented by tertiary amines, such as pyridine or its analogues, as precursors to a polyamic acid solution.

[0006] When the imidization reaction is performed by additionally adding the above-mentioned dehydrating agent or catalyst, there are problems of low yield and low process efficiency due to the catalyst price and the need for an additional process to remove the catalyst.

[0007] Meanwhile, the thermal imidization method is performed by applying a polyamic acid solution as a precursor to a substrate, evaporating the solvent, and heating at 250° C. to 350° C., without using a chemical dehydrating agent and a catalyst. However, the method has the disadvantage that when an amide-based solvent is used, the crystallinity is high and the polymer decomposes due to the amide exchange reaction.

[0008] In the polyimide powders prepared by these methods, if the imidization degree is low, there is a problem of water, which is a byproduct of the imidization reaction, generated in the process, thereby generating pores and reducing mechanical properties, resulting in deterioration of physical properties.

[0009] Therefore, it is necessary to research and develop a polyimide powder having excellent intrinsic viscosity, and to promote a method for preparing a polyimide powder by an imidization process that is simple and effective and does not require the addition of a separate dehydrating agent or catalyst, and can produce a molded article having excellent tensile strength and elongation. Summary of the invention

[0010] Technical issues

[0011] The embodiments of the present disclosure aim to provide a method for preparing a polyimide powder, which can promote imidization and has excellent inherent viscosity by using a mixed solvent containing a polar organic solvent and a high-boiling point aromatic hydrocarbon solvent for reaction without adding a separate dehydrating agent or catalyst, and provides a polyimide powder prepared by the method.

[0012] In addition, another embodiment of the present disclosure is to provide a method for preparing a molded article containing polyimide powder.

[0013] Furthermore, another embodiment of the present disclosure is to provide a molded product containing polyimide powder.

[0014] Technical solutions to technical problems

[0015] Hereinafter, according to the present disclosure, exemplary embodiments of the present disclosure will be described in more detail in the order of “method for preparing polyimide powder”, “polyimide powder”, “method for preparing a molded article containing polyimide powder”, and “molded article containing polyimide powder”.

[0016] Since the present disclosure can be variously modified and various embodiments can be provided, specific embodiments are shown in the drawings and described in detail. However, it should be understood that this is not intended to limit the present disclosure to specific embodiments, but to include all changes, equivalents and substitutes included in the spirit and scope of the present disclosure.

[0017] The terms in this disclosure are only used to describe specific exemplary embodiments and are not intended to limit the present disclosure. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this disclosure, terms such as "including" or "having" are intended to indicate the features, numbers, steps, operations, parts, portions, or combinations thereof described in this disclosure, and these should not be understood to exclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, parts, portions, or combinations thereof.

[0018] When an amount, concentration or other value or parameter in the present disclosure is provided as a range, a preferred range, or a list of upper preferred values ​​and lower preferred values, this should be understood to specifically disclose all ranges consisting of any upper range limit or preferred value and any lower range limit or preferred value, whether or not such range is disclosed individually.

[0019] When this disclosure refers to a numerical range, it is not intended that the range be limited to the endpoints unless otherwise specified, nor is it intended that the scope of the disclosure be limited to the specific values ​​recited when defining a range.

[0020] The term "dianhydride" as used in this disclosure is intended to include its precursors or derivatives, also referred to as "dianhydride" or "acid dianhydride". It may not be technically a dianhydride, but can still react with a diamine to form a polyamic acid, which can be converted into a polyimide.

[0021] The term "diamine" as used in this disclosure is intended to include precursors or derivatives thereof that may not technically be diamines but can still react with dianhydrides to form polyamic acids, which can be converted into polyimides.

[0022] In addition, unless otherwise defined, all terms used in the present disclosure, including technical or scientific terms, have the same meaning as those generally understood by those skilled in the art in the field to which the embodiments belong. For example, terms defined in general dictionaries should be interpreted as having meanings consistent with those in the context of the relevant technology. Unless clearly defined in the present disclosure, they should not be interpreted in an ideal or overly formal sense. The specific details of the implementation of the present disclosure will be described below.

[0023] The present disclosure provides a method for preparing polyimide powder, which uses a mixed solvent containing a polar organic solvent and a high-boiling-point aromatic hydrocarbon solvent having a boiling point of 155° C. or higher.

[0024] In one aspect, the method for preparing the polyimide powder of the present disclosure may include:

[0025] (a) dispersing a dianhydride compound and a diamine compound in a mixed solvent to prepare a polyamic acid composition; and

[0026] (b) imidizing the mixture at an elevated temperature to form a polyimide powder,

[0027] The mixed solvent includes a polar organic solvent and a high-boiling-point aromatic hydrocarbon solvent, wherein the high-boiling-point aromatic hydrocarbon solvent has a boiling point of 155° C. or higher.

[0028] In the present disclosure, the polar organic solvent may have a boiling point of 150°C or higher, preferably 160°C or higher, more preferably 170°C or higher, and even more preferably 200°C or higher, wherein the upper limit is not particularly limited, but the upper limit may be 250°C or lower.

[0029] In the present disclosure, the polar organic solvent may be N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), ethylene glycol, N-ethyl-2-pyrrolidone (NEP), dimethylolpropionic acid (DMPA) or a combination thereof and the like, preferably N-methylpyrrolidone.

[0030] The high boiling point aromatic hydrocarbon may have a boiling point of 160° C. or higher, preferably 160° C. to 250° C. The lower limit of the boiling point may be, for example, 160° C. or higher, 161° C. or higher, 162° C. or higher, 163° C. or higher, 164° C. or higher, or 165° C. or higher. In addition, the upper limit of the boiling point may be, for example, 250° C. or lower, 245° C. or lower, 240° C. or lower, 235° C. or lower, 230° C. or lower, 225° C. or lower, 220° C. or lower, 215° C. or lower, 210° C. or lower, 205° C. or lower, 200° C. or lower, 198° C. or lower, 196° C. or lower, 194° C. or lower, 192° C. or lower, 190° C. or lower, 188° C. or lower, 186° C. or lower, 184° C. or lower, 182° C. or lower, or 180° C. or lower.

[0031] In the present disclosure, the high boiling point aromatic hydrocarbons may be mesitylene, 1,2,4-trimethylbenzene, 1,2,3-trimethylbenzene, propylbenzene, 1-ethyl-2-methylbenzene and the like, preferably 1,2,4-trimethylbenzene, 1,2,3-trimethylbenzene, propylbenzene, 1-ethyl-2-methylbenzene or a combination thereof.

[0032] In the present disclosure, the mixed solvent may also include a hydrocarbon solvent, which may be n-hexane, cyclohexane, heptane, benzene, toluene, isopropylene, xylene or a combination thereof, preferably may include isopropylene or xylene, but the scope of the hydrocarbon solvent of the present disclosure is not limited thereto.

[0033] In the present disclosure, the mixed solvent may contain 5 to 50 parts by weight of a high-boiling point aromatic hydrocarbon solvent, specifically 10 to 45 parts by weight, more specifically 15 to 40 parts by weight, and even more specifically 20 to 35 parts by weight, based on 100 parts by weight, and the remaining portion may be occupied by a polar organic solvent or a hydrocarbon solvent.

[0034] In the present disclosure, the mixed solvent may contain 50 to 95 parts by weight of a polar organic solvent, specifically 55 to 90 parts by weight, more specifically 60 to 85 parts by weight, and even more specifically 65 to 80 parts by weight, based on 100 parts by weight, and the remaining portion may be occupied by aromatic solvents or hydrocarbon solvents.

[0035] In addition, the mixed solvent of the present disclosure may contain 50 to 95 parts by weight of a polar organic solvent and 5 to 50 parts by weight of a high boiling point aromatic hydrocarbon solvent, and may further contain 1 to 5 parts by weight of a hydrocarbon solvent.

[0036] In the present disclosure, the polyimide powder may be a fully aromatic polyimide, a partially alicyclic polyimide, and a fully alicyclic polyimide.

[0037] In the embodiments of the present disclosure, the dianhydride compound may be pyromellitic dianhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (sBPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (2,3,3',4'-biphenyltetracarboxylic dianhydride (sBPDA), dianhydride; a-BPDA), diphenylsulfone-3,4,3',4'-tetracarboxylic dianhydride (DSDA), bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride dianhydride;BTDA), bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenylenebis(trimellitic monoester acid anhydride), p-biphenylenebis(trimellitic monoester acid anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic dianhydride dianhydride), 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride), 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride), 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride), 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride;BPADA), 2,3,6,7-naphthalene tetracarboxylic acid dianhydride, 1,4,5,8-naphthalene tetracarboxylic acid dianhydride and 4,4'-(2,2-hexafluoroisopropylidene) phthalic acid dianhydride, and preferably pyromellitic acid dianhydride (PMDA), oxydiphthalic acid dianhydride (ODPA) or a combination thereof. The scope of the dianhydride compound disclosed in the present invention is not limited thereto, and dianhydrides used to prepare polyimides can be widely used. ;

[0038] In addition, the diamine compound may be paraphenylenediamine, metaphenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid, acid; DABA), 4,4'-diaminodiphenylether, 4,4'-oxydianiline (ODA), 3,4'-diaminodiphenylether, 4,4'-diaminodiphenylmethane (methylenedianiline), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl henyl), 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl)sulfide, 4,4'-diaminobenzanilide, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine,3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide sulfide), 4,4'-diaminodiphenylsulfide, 3,3'-diaminodiphenylsulfone, 3,4'-diaminodiphenylsulfone, 4,4'-diaminodiphenylsulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diamino 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane -aminophenyl)propane), 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane), 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane,3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene )、1,4-bis(4-aminophenyl)benzene、1,3-bis(4-aminophenoxy)benzene; TPE-R、1,4-bis(3-aminophenoxy)benzene; TPE-Q、1,3-bis(3-aminophenoxy)-4-trifluorotoluene、3,3'-diamine 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenylsulfide)benzene, 1,3-bis(4-aminophenylsulfide)benzene, 1,4-bis(4-aminophenylsulfide)benzene), 1,4-bis(4-aminophenylsulfide)benzene), 1,3-bis(3-aminophenylsulfone)benzene), 1,3-bis(4-aminophenylsulfone)benzene), 1,4-bis(4-aminophenylsulfone)benzene,1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'-bis(3-aminophenoxy)biphenyl )biphenyl), 3,3'-bis(4-aminophenoxy)biphenyl), 4,4'-bis(3-aminophenoxy)biphenyl), 4,4'-bis(4-aminophenoxy)biphenyl), bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether), bis[4-(3-aminophenoxy)phenyl]ether), bis[4-(4-aminophenoxy)phenyl]ether), bis[3-(3-aminophenoxy)phenyl]ketone), bis[3-(4-aminophenoxy)phenyl]ketone phenyl]ketone), bis[4-(3-aminophenoxy)phenyl]ketone), bis[4-(4-aminophenoxy)phenyl]ketone), bis[3-(3-aminophenoxy)phenyl]sulfide), bis[3-(4-aminophenoxy)phenyl]sulfide,Bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[3-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, ]methane (bis[4-(3-aminophenoxy)phenyl]methane), bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, [4-(3-aminophenoxy)phenyl]propane (2,2-bis[4-(3-amino)phenoxy)phenyl]propane), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane (2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane),2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane and the like, and preferably 4,4'-oxydiphenylamine (ODA). The scope of the diamine compound disclosed in the present invention is not limited thereto, and diamines used for preparing polyimide can be widely used.

[0039] In an embodiment, the polyimide powder may be prepared using pyromellitic dianhydride (PMDA) and oxydiphthalic dianhydride (ODPA) as dianhydride compounds, and using 4,4′-oxydiphenylamine (ODA) as a diamine compound.

[0040] In an embodiment, the polyamic acid composition may contain two or more types of dianhydride compounds, and may contain pyromellitic dianhydride (PMDA) therein. Specifically, 70mol% or more of pyromellitic dianhydride (PMDA) may be contained in the overall composition of the dianhydride compound. The lower limit of the ratio may be, for example, 75mol%, 78mol%, 80mol%, 82mol%, 85mol%, 87mol%, 90mol%, 92mol%, 94mol%, 95mol%, 97mol%, 99mol% or 100mol% or more, and the upper limit may be, for example, 100mol%, 99mol%, 98mol%, 97mol%, 96mol%, 95mol%, 94mol%, 93mol%, 92mol%, 91mol% or 90mol% or less.

[0041] In an embodiment, the polyamic acid composition may include two or more types of dianhydride compounds, and may include oxydiphthalic dianhydride (ODPA). Specifically, 30mol% or less of the oxydiphthalic dianhydride (ODPA) may be contained in the overall composition of dianhydride. The ratio may preferably be 20mol% or less, 19mol% or less, 18mol% or less, 17mol% or less, 16mol% or less, 15mol% or less, 14mol% or less, 13mol% or less, 12mol% or less, 11mol% or less, 10mol% or less, 8mol% or less, 6mol% or less, 4mol% or less, 2mol% or less or may be 0mol%.

[0042] In an embodiment, the polyamic acid composition may include at least one diamine compound, and preferably may include 4,4'-oxydiphenylamine (ODA). Specifically, 4,4'-oxydiphenylamine (ODA) may be contained in a ratio of 70 mol% or more in the overall composition of the diamine monomer. The lower limit of the ratio may be, for example, 70 mol% or more, 71 mol% or more, 72 mol% or more, 73 mol% or more, 74 mol% or more, 75 mol% or more, 76 mol% or more, 77 mol% or more, 78 mol% or more, 80 mol% or more, 82 mol% or more, 85 mol% or more, 87 mol% or more, 90 mol% or more, 92 mol% or more, 94 mol% or more, 95 mol% or more, 97 mol% or more, 99 mol% or more, 100 mol%, and the upper limit may be, for example, 100 mol% or less, 99 mol% or less, 98 mol% or less, 97 mol% or less, 96 mol% or less, 95 mol% or less, 94 mol% or less, 93 mol% or less, 92 mol% or less, 91 mol% or less, 90 mol% or less.

[0043] In the present disclosure, in step (a), the molar ratio of the diamine compound to the dianhydride compound may be 0.5 to 2 equivalents. The molar ratio may specifically be 0.8 to 1.5 equivalents. When the molar ratio is less than 0.5 equivalents or more than 2 equivalents, the polyimide finally formed has a very small molecular weight, so there is a problem that the physical and chemical properties of the polyimide are very poor.

[0044] In addition, the mixture in step (a) may include polyamic acid formed by polymerization of a dianhydride compound and a diamine compound.

[0045] In addition, step (a) can be performed in various ways, for example, each compound is dispersed in a solvent (or a mixed solvent) and then each reactant is introduced into a reaction vessel, and another method may be to first introduce the solvent (or a mixed solvent) into the reaction vessel and then introduce each compound therein. In addition, step (a) may be performed by a method in which each compound is first introduced into a reaction vessel and then the solvent (or a mixed solvent) is introduced therein, or may be performed by a combination of the above methods.

[0046] In the present disclosure, the amount of the mixed solvent can be 5 to 50 times, 7 to 40 times and 10 to 30 times the weight of the dianhydride compound as a reactant, and the amount of the mixed solvent can be appropriately adjusted according to the amount of the dianhydride compound and the diamine compound used in the reaction.

[0047] Meanwhile, step (a) may be performed at a temperature ranging from 10° C. to 95° C. When the temperature is lower than 10° C., the reaction may not proceed, and when the temperature is higher than 95° C., a separate additional heat source supply or a condenser or the like may be required, or an additional process may be required.

[0048] In addition, step (a) can be performed for 5 minutes to 5 days, specifically, for 1 hour to 2 days. When step (a) is performed for less than 5 minutes, there may be a problem of insufficient reaction, and when step (a) is performed for more than 5 days, there may be a problem of rapid cost increase.

[0049] In the present disclosure, step (b) may be performed at a high temperature in the temperature range of 150° C. to 450° C. Specifically, step (b) may be performed in the temperature range of 180° C. to 350° C. When step (b) is performed at a temperature below 150° C., imidization may not occur, and when step (b) is performed at a temperature above 450° C., thermal decomposition of the monomer (or compound) or the polymer itself may occur.

[0050] In the present disclosure, step (b) may be performed for 5 minutes to 5 days, specifically 10 minutes to 2 days, more specifically 30 minutes to 1 day, and even more specifically 1 hour to 5 hours. When step (b) is performed for less than 5 minutes, imidization may not occur, and when step (b) is performed for more than 5 days, hydrolysis or thermal decomposition of the polymer may occur.

[0051] Meanwhile, in step (b), the heating may be performed by one or a combination of two or more selected from the group consisting of heat treatment, hot air treatment, corona treatment, high frequency treatment, ultraviolet treatment, infrared treatment and laser treatment.

[0052] In step (b), the solid content of the polyimide powder is 1% to 25% by weight, specifically 1% to 20% by weight, more specifically 2% to 18% by weight, and even more specifically 3% to 15% by weight.

[0053] In addition, the method for preparing the polyimide powder of the present disclosure may further include step (c), washing, filtering and drying the polyimide powder.

[0054] The filtration can be performed by one or a combination of two or more selected from the group consisting of gravity filtration, reduced pressure filtration, vacuum filtration, pressure filtration, compression filtration, centrifugal filtration, microfiltration, ultrafiltration and reverse osmosis. In particular, reduced pressure filtration can be preferably used.

[0055] In addition, drying can be performed by one or a combination of two or more selected from the group consisting of natural drying, pressurized drying, hot air drying, spray drying, film drying, vacuum drying, freeze drying, spray freeze drying, electromagnetic wave drying, and flash drying. In particular, drying can be preferably performed at a temperature of 50° C. or higher under vacuum.

[0056] In the present disclosure, the imidization reaction performed in step (b) may have an imidization rate of 97% to 100%, preferably 98% to 100%, more preferably 99% to 100%, and most preferably 100%.

[0057] In the preparation method of the polyimide powder of the present disclosure, when the imidization reaction is carried out in a mixed solvent including a polar organic solvent and a high-boiling aromatic hydrocarbon solvent having a boiling point of 155° C. or higher, the high-boiling aromatic hydrocarbon solvent can simultaneously act as a dehydrating agent to promote the imidization of the polyamic acid without the need to additionally add a separate catalyst or dehydrating agent. In addition, since the powder is precipitated by imidization at a temperature of about 150° C. to 160° C., sufficient imidization can be performed to maintain excellent physical properties, such as increased intrinsic viscosity, etc.

[0058] In another aspect, the present disclosure provides a polyimide powder prepared according to the method for preparing the polyimide powder.

[0059] The polyimide powder has a high intrinsic viscosity of 1.0 dL / g or more, and thus has an advantage of being easy to perform post-processing such as molding while maintaining excellent mechanical properties.

[0060] In an embodiment, the intrinsic viscosity of the polyimide powder of the present disclosure may be 1.0 dL / g to 1.5 dL / g, specifically 1.0 dL / g to 1.3 dL / g, more specifically 1.0 dL / g to 1.2 dL / g, and even more specifically 1.1 dL / g to 1.15 dL / g. When the intrinsic viscosity of the polyimide powder is lower than 1.0 dL / g, the molded product (or molded body) molded from the polyimide powder will have a problem of weakened strength and difficult post-processing.

[0061] In another aspect of the present disclosure, the present disclosure provides a method for preparing a polyimide molded article, comprising: (1) molding the polyimide powder prepared according to the above-mentioned method for preparing the polyimide powder; and (2) sintering.

[0062] In the molding step of step (1), compression molding, injection molding, blow molding, rotational molding, extrusion molding, thermoforming, slush molding, spinning, and the like can be used.

[0063] In another aspect, the present disclosure provides a polyimide molded article prepared according to the method for preparing the polyimide molded article.

[0064] In the present disclosure, the polyimide molded article may have a tensile strength of 85 MPa or greater, preferably 90 MPa or greater, more preferably 95 MPa or greater, even more preferably 100 MPa or greater, and even more preferably 110 MPa or greater, wherein the upper limit of the range of the tensile strength is not particularly limited, but may be 200 MPa or less.

[0065] In addition, the polyimide molded article may have an elongation of 7% or more, preferably 8% or more, more preferably 9% or more, and even more preferably 10% or more, wherein the upper limit of the elongation is not particularly limited, but may be 40% or less, 30% or less, or 20% or less.

[0066] In addition, the polyimide molded article may have a modulus of 1.5 GPa or more, preferably 2.0 GPa or more, more preferably 2.5 GPa or more, and even more preferably 3.0 GPa or more.

[0067] In addition, the polyimide molded article may have a flexural strength of 150 MPa or greater, preferably 155 MPa or greater, more preferably 160 MPa or greater, and even more preferably 170 MPa or greater, wherein the upper limit of the flexural strength is not particularly limited, but may be 300 MPa or less.

[0068] In the present disclosure, the molded article may be referred to as a molded body. The prepared molded article may be in various forms, such as films, adhesives, tapes, multilayer films and the like, and may be used in a wide range of industries, such as aerospace, aviation, electronics / electrical appliances, semiconductors, displays, liquid crystal alignment films, automobiles, precision devices, packaging, medical materials, separators, fuel cells, secondary batteries and the like. The physical properties and characteristics of the molded article made from the polyimide powder of the present invention may be widely used in any suitable products or fields.

[0069] In addition, the molded product including the polyimide powder prepared by the method for preparing the polyimide powder according to the present disclosure has the advantages of simultaneously improving the tensile strength, elongation, modulus and flexural strength, and can be used in various fields requiring these physical properties.

[0070] Beneficial Effects

[0071] According to the method for preparing polyimide powder disclosed in the present invention, imidization is promoted by reacting in a mixed solvent including a polar organic solvent and a high-boiling-point aromatic hydrocarbon solvent, and no separate dehydrating agent or catalyst needs to be added, thereby making it possible to prepare polyimide powder having high intrinsic viscosity and high imidization rate through a simple and effective process, and the molded product prepared using the polyimide powder can have excellent tensile strength, elongation, modulus and flexural strength. DETAILED DESCRIPTION

[0072] The following examples may enhance the understanding of the present disclosure. These examples are only provided for a simpler understanding of the present disclosure, but the content of the present disclosure is not limited by the following examples.

[0073] <Example>

[0074] Example 1. Preparation of polyimide powder using high boiling point aromatic solvent

[0075] Example 1-1. (1) Preparation of polyimide powder

[0076] A dianhydride compound, namely, pyromellitic anhydride (PMDA) (80 mol%) and oxydiphthalic anhydride (ODPA) (20 mol%), and a diamine compound, namely, 4,4'-oxydiphenylamine (100 mol%), are dispersed in a mixed solvent of N-methylpyrrolidone and 1,2,3-trimethylbenzene (1,2,3-trimethylbenzene) (boiling point of 176° C.) in a ratio of 70:30 (v / v%) to prepare a polyamic acid composition, wherein N-methylpyrrolidone is a polar solvent and 1,2,3-trimethylbenzene is a high boiling point aromatic solvent.

[0077] The mixture was transferred to a 500 mL reaction vessel equipped with a stirrer, a nitrogen injector, and a temperature controller, and then the air in the reaction vessel was replaced with nitrogen, and then the mixture was stirred in a high temperature reactor at 180° C. for 6 hours to form a polyimide powder.

[0078] The suspension of the polyimide powder was filtered under reduced pressure and washed with distilled water to obtain an undried polyimide powder, which was then dried in a vacuum oven at 60° C. for 24 hours to obtain a polyimide powder.

[0079] Example 1-2. (2) Preparation of polyimide powder

[0080] A dianhydride compound, namely, pyromellitic dianhydride (PMDA) (80 mol%) and oxydiphthalic dianhydride (ODPA) (20 mol%), and a diamine compound, namely, 4,4'-oxydiphenylamine (100 mol%), are dispersed in a mixed solvent of N-methyl pyrrolidone and 1,2,4-trimethylbenzene (1,2,4-trimethylbenzene) (boiling point of 169° C.) in a ratio of 70:30 (v / v%) to prepare a mixture, wherein N-methyl pyrrolidone is a polar solvent and 1,2,4-trimethylbenzene is a high boiling point aromatic solvent.

[0081] The mixture was transferred to a 500 mL reaction container equipped with a stirrer, a nitrogen injector, and a temperature controller, the air in the reaction container was replaced with nitrogen, and then the mixture was stirred in a high temperature reactor at 180° C. for 6 hours to form a polyimide powder.

[0082] The suspension of the polyimide powder was filtered under reduced pressure and washed with distilled water to obtain an undried polyimide powder, which was then dried in a vacuum oven at 60° C. for 24 hours to obtain a polyimide powder.

[0083] Example 2. Preparation of a molded product of polyimide powder

[0084] Example 2-1 and Example 2-2. Preparation of polyimide molded products

[0085] The polyimide powders prepared in Example 1-1 and Example 1-2 were weighed into molds for evaluating physical properties, respectively, and then heated to 450° C. while applying a pressure of 10,000 Psi or more using a hot press to prepare molded products.

[0086] Comparative Example 1. Preparation of polyimide powder using low boiling point aromatic hydrocarbon solvent

[0087] Comparative Example 1-1. Preparation of polyimide powder

[0088] A polyimide powder was prepared in the same manner as in Example 1 except that a low boiling point aromatic solvent, xylene (boiling point: 139° C.), was used instead of a high boiling point aromatic solvent.

[0089] Comparative Example 1-2. Preparation of polyimide powder

[0090] A polyimide powder was prepared in the same manner as in Example 1 except that toluene (boiling point: 111° C.), a low boiling point aromatic solvent, was used instead of the high boiling point aromatic solvent.

[0091] Comparative Example 1-3. Preparation of polyimide powder

[0092] A polyimide powder was prepared in the same manner as in Example 1 except for the high boiling point aromatic hydrocarbon solvent.

[0093] Comparative Example 2. Preparation of molded products using polyimide powder prepared using low-boiling point aromatic hydrocarbon solvents

[0094] Comparative Examples 2-1 to 2-3. Preparation of polyimide molded products

[0095] The polyimide powders prepared in Comparative Examples 1-1 to 1-3 were weighed into molds for evaluating physical properties, respectively, and then heated to 450°C while applying a pressure of 10,000 Psi or greater using a hot press to prepare molded products of Comparative Examples 2-1, 2-2, and 2-3, respectively.

[0096] Table 1 below summarizes the components and contents of the dianhydride compound and the diamine compound and the components of the mixed solvent used in preparing the polyimide powder in Example 1-1, Example 1-2, Comparative Example 1-1, Comparative Example 1-2 and Comparative Example 1-3.

[0097] [Table 1]

[0098]

[0099] <Experimental Example> Analysis of the physical and chemical properties of polyimide powder and molded products

[0100] Experimental Example 1. Imidization rate

[0101] In order to measure the imidization rate, the polyimide powder was prepared into a granular form, and then the imidization rate was measured, compared and calculated using Nicolet iZ20 FT IR (ATR) (infrared spectrometer) of Thermo Fisher Scientific Inc., where 1390 cm -1 / 1490cm -1 The value of is set as 100% standard value of a 100% imidization-treated polyimide film.

[0102] Experimental Example 2. Intrinsic Viscosity

[0103] The polyimide powders (0.1 g) prepared according to the examples and comparative examples were dissolved in 20 mL of N,N′-dimethylacetamide, and the viscosity thereof was measured using an Ubbelohde viscometer in a thermostat maintained at 30° C.

[0104] The imidization ratio and intrinsic viscosity of the polyimide powder analyzed according to Experimental Examples 1 and 2 are shown in Table 2 below.

[0105] [Table 2]

[0106] Example 1-1 Example 1-2 Comparative Example 1-1 Comparative Example 1-2 Comparative Examples 1-3 Imidization rate (%) >100 >100 95 96 90 Intrinsic viscosity (dL / g) 1.12 1.11 0.95 0.93 0.86

[0107] Experimental Example 3. Tensile Strength

[0108] The tensile strength of the samples was measured using a universal testing machine (UTM) (Instron 5564 manufactured by Instron Corp., Massachusetts, USA) according to ASTM D1708 standard.

[0109] Experimental Example 4. Elongation

[0110] The elongation was measured on the molded bodies prepared in Examples and Comparative Examples and cut into a width of 10 mm and a length of 40 mm using Instron 5564UTM equipment in accordance with ASTM D-882 standard.

[0111] Experimental Example 5. Bending Strength

[0112] Flexural strength was measured using UTM according to ASTM D-882.

[0113] The physical property results of the polyimide molded products analyzed according to Experimental Examples 3 to 5 are shown in Table 3 below.

[0114] [Table 3]

[0115] Example 2-1 Example 2-2 Comparative Example 2-1 Comparative Example 2-2 Comparative Example 2-3 Tensile strength(MPa) 114 112 83 92 73 Elongation(%) 12 10 6.9 5.6 4.5 Flexural strength(MPa) 174 171 143 142 121

[0116] Experimental Example 6. Modulus (elastic modulus)

[0117] The polyimide molded bodies (width 15 mm) prepared in the examples and comparative examples were measured using an Instron 5564 UTM device according to ASTM D-882 standard (grip speed = 200 mm / min).

[0118] The modulus of the polyimide molded article analyzed according to Experimental Example 6 is shown in Table 4 below.

[0119] [Table 4]

[0120] Example 2-1 Example 2-2 Modulus(GPa) 2.3 2.2

[0121] The embodiment of the present disclosure using a high boiling aromatic solvent having a boiling point of 155°C or higher for imidization reaction reaches 100% imidization rate and exhibits an excellent intrinsic viscosity of 1.0 dL / g or higher. In addition, the molded product prepared using the polyimide powder according to the present disclosure has a tensile strength of 110 MPa or more, an elongation of 10% or more, and a flexural strength of 170 MPa or more, which is significantly better than the molded product of the comparative example. In addition, it is found that the molded product prepared using the polyimide powder according to the present disclosure has excellent rigidity because its modulus is 1.5 GPa or more. Comparative Examples 1-1, 1-2, and 1-3 without aromatic solvents, which use low boiling aromatic solvents with a boiling point lower than 155°C for imidization reaction, show an imidization rate lower than that of the embodiment, and the polyimide powder molded product prepared according to the comparative example has a tensile strength, elongation, and flexural strength significantly lower than that of the embodiment, and the polyimide powder molded product is not suitable for application in actual products.

[0122] In the present disclosure, detailed descriptions of contents that can be fully understood and inferred by those skilled in the art of the present disclosure are omitted. In addition to the specific exemplary embodiments described in the present disclosure, various changes and modifications can be made within the scope of not changing the technical spirit or necessary configuration of the present disclosure. Therefore, the present disclosure can also be implemented in a manner different from this specific description and explanation, which can be understood by those skilled in the art.

Claims

1. A method for preparing polyimide powder, comprising: (a) preparing a polyamic acid composition by dispersing a dianhydride compound and a diamine compound in a mixed solvent; and (b) imidizing the mixture at an elevated temperature to form a polyimide powder, The mixed solvent comprises a polar organic solvent and a high boiling point aromatic hydrocarbon solvent, wherein the high boiling point aromatic hydrocarbon solvent has a boiling point of 155° C. or higher.

2. The preparation method according to claim 1, wherein the polar organic solvent has a boiling point of 150°C or higher.

3. The preparation method according to claim 1, wherein the polar organic solvent comprises at least one selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), ethylene glycol, N-ethyl-2-pyrrolidone (NEP) and dimethylolpropionic acid (DMPA).

4. The preparation method according to claim 1, wherein the high boiling point aromatic solvent further comprises at least one selected from the group consisting of mesitylene, 1,2,4-trimethylbenzene, 1,2,3-trimethylbenzene, propylbenzene and 1-ethyl-2-methylbenzene.

5. The preparation method according to claim 1, wherein the high boiling point aromatic hydrocarbon solvent comprises a high boiling point aromatic hydrocarbon solvent having a boiling point of 160°C or higher.

6. The preparation method according to claim 1, wherein the mixed solvent further comprises a hydrocarbon solvent.

7. The preparation method according to claim 6, wherein the hydrocarbon solvent comprises at least one selected from the group consisting of n-hexane, cyclohexane, heptane, benzene, toluene, isopropylene and xylene.

8. The preparation method according to claim 1, wherein the mixed solvent is calculated as 100 parts by weight, the polar organic solvent is 50 to 95 parts by weight, and the high boiling point aromatic hydrocarbon solvent is 5 to 50 parts by weight. 9 . The preparation method according to claim 1 , wherein the polyimide powder is any one selected from the group consisting of wholly aromatic polyimide, partially alicyclic polyimide and wholly alicyclic polyimide.

10. The preparation method according to claim 1, wherein the dianhydride compound is selected from the group consisting of pyromellitic dianhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (sBPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), diphenyl sulfone-3,4,3',4-tetracarboxylic dianhydride (DSDA), bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), bis(3,4-dicarboxyphenyl)methane Dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenylene bis(trimellitic acid monoester anhydride), p-biphenylene bis(trimellitic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic acid anhydride and 4,4'-(2,2-hexafluoroisopropylidene)phthalic acid dianhydride The diamine compound is selected from the group consisting of p-phenylenediamine, m-phenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (DABA), 4,4'-oxydiphenylamine (ODA), 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (methylenedianiline), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4 ,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl)sulfide, 4,4'-diaminobenzanilide, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4-dichlorobenzophenone, 3,3'-Diamino-4,4-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(3-aminophenoxy)benzene (TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluorotoluene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-bis(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenyl sulfide)benzene, 1,3-bis(4-aminophenyl sulfide)benzene, 1,4-bis(4-aminophenyl sulfide)benzene, 1,3-bis(3-aminophenyl sulfone)benzene, 1,3-bis(4-aminophenyl sulfone)benzene, 1,4-bis(4-aminophenyl sulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl] Benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[3-(3-aminophenoxy)phenyl]ketone, bis[3-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]ketone , bis[4-(4-aminophenoxy)phenyl]ketone, bis[3-(3-aminophenoxy)phenyl]sulfide, bis[3-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[3-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[3-(3-diaminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,At least one of the group consisting of 2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.

11. The preparation method according to claim 1, further comprising: (c) washing, filtering and drying the polyimide powder. 12 . The preparation method according to claim 1 , wherein in the imidization, the imidization rate is 97% to 100%.

13. A polyimide powder prepared by the method for preparing a polyimide powder according to any one of claims 1 to 12. 14 . The polyimide powder of claim 13 , wherein the polyimide powder has an intrinsic viscosity of 1.0 dL / g to 1.5 dL / g.

15. A method for preparing a polyimide molded product, comprising: (1) molding a polyimide powder prepared by the method for preparing a polyimide powder according to any one of claims 1 to 12; and (2) Sintering 16. A polyimide molded product prepared according to the preparation method according to claim 15.

17. The polyimide molded article as claimed in claim 16, wherein the polyimide molded article has a tensile strength of 85 MPa or greater; an elongation of 7% or greater; a modulus of 1.5 GPa or greater; and a flexural strength of 150 MPa or greater.