Method for preparing high-strength and high-ignition-point palm shell physical columnar activated carbon
By soaking the palm shell in sodium carbonate solution and carbonizing it in water vapor atmosphere, and mixing it with starch and distilled plant tar for granulation and molding, the problem of preparing high-strength and high-ignition activated carbon in palm shell is solved, and efficient utilization is achieved Renewable resources improve product performance and environmental protection.
Patent Information
- Application Number
- CN202411089940.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
It is difficult for the prior art to effectively use palm shells to prepare physical columnar activated carbon with high strength and high ignition points, and most of the binders on the market are non-renewable resources, resulting in waste of resources.
After soaking the palm shell raw material in sodium carbonate solution, carbonizing, crushing, and mixing it with starch and distilled plant tar, it is granulated and secondary molded. High-strength, high-ignition and high-ignition point palm shell physics are prepared by activation of water vapor. columnar activated carbon.
High-strength, high-ignition activated carbon prepared by palm shells is realized, and the renewable resource plant tar is utilized, which improves the performance and environmental protection of the product.
Smart Images

Figure BDA0004986243720000081
Abstract
Description
Technical Field
[0001] The invention relates to the fields of environmental protection technology and activated carbon processing technology, and in particular to a method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon. Background Art
[0002] Plant-based physical columnar activated carbon generally uses coconut shell and bamboo-based raw materials; among them, coconut shell raw materials have the best performance, but the price is relatively high; bamboo-based raw materials have high potassium content, which directly affects the ignition point of physical columnar activated carbon, making its ignition point 320-350℃. Due to the characteristics of wood raw materials, the physical columnar activated carbon prepared has low strength and light specific gravity and cannot be used.
[0003] Since palm shells are classified as by-products in the palm fruit processing chain, their output is huge, and the main target products in the processing process are crude palm oil and palm oil. Since palm shells themselves are not of high value, they have long been abandoned as waste in the palm fruit processing chain, and some palm kernel shells are only used as an alternative energy source for thermal coal. Due to the variety of palm shells and the uneven thickness of the shell walls, a large amount of white ash needs to be added to the palm fruit in the process of making palm oil. Most of the white ash adheres to the palm shells. If columnar activated carbon is directly prepared without treatment, the strength of the product will be reduced and the ash content will be too high. At present, there is no successful case of physical columnar activated carbon made from palm shells on the market. The present invention can successfully make palm shells into physical columnar activated carbon, and its carbon tetrachloride adsorption rate is ≥60%, strength is ≥97%, and ignition point is >400℃.
[0004] In addition, the binders used in the physical columnar activated carbon on the market are mostly coal tar and coal pitch, which are non-renewable resources. However, biomass raw materials such as bamboo, wood, and fruit shells will produce a large amount of plant tar during the carbonization process. The tar has a strong odor and is not used in large quantities, resulting in a serious surplus of resources. If it can be utilized, it will be a good renewable resource. However, plant tar has a low viscosity. If it is directly used as a binder for columnar activated carbon, the strength of the prepared columnar activated carbon is low. There are very few physical columnar activated carbon products on the market that use plant tar as a binder. Summary of the invention
[0005] In view of this, the purpose of the present invention is to propose a method for preparing high-strength, high-ignition-point palm shell physical method columnar activated carbon, which is reliable in implementation, has a wide source of raw materials, is environmentally friendly and has good product performance.
[0006] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:
[0007] A method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon, comprising:
[0008] After the palm shell raw material is screened, it is soaked in sodium carbonate solution and then filtered, and then soaked in water and filtered, and the water soaking treatment is repeated for a preset number of times to obtain a washing material; after the washing material is dried, it is carbonized and kept warm for a preset time in a water vapor atmosphere to obtain a carbonized material; after the carbonized material is coarsely crushed, screened, and pulverized, a carbonized material powder is obtained, and then the carbonized material powder is mixed with starch and distilled plant tar, and then water is added for kneading, and then it is formed into a columnar material, and then the columnar material is carbonized and activated in a water vapor atmosphere to obtain a high-strength, high-ignition-point palm shell physical method columnar activated carbon.
[0009] As a possible implementation manner, further, in the present invention, the palm shell raw material is passed through a 3-mesh sieve, and the palm shell raw material with a mesh size larger than 3 mesh is alternately soaked in a sodium carbonate solution and water.
[0010] As a possible implementation mode, further, the mass concentration of the sodium carbonate solution described in this scheme is 1-10%, and the time for soaking the palm shell raw material with the sodium carbonate solution and water is 1 hour / time; wherein, after the palm shell raw material is soaked in the sodium carbonate solution and filtered, the number of times of soaking in water and filtering is repeated 4 times; the moisture content of the washing material after drying is controlled within 15%.
[0011] As a possible implementation mode, further, after drying, the washed material of this scheme is carbonized and kept warm at an ambient temperature of 450-650° C. for 10-120 minutes in a steam atmosphere to obtain a carbonized material.
[0012] As a possible implementation mode, further, the carbonized material of this scheme is coarsely crushed by a double-roll crusher with a spacing of 3 to 6 mm, and then sieved to obtain carbonized material with a particle size greater than 1.5 mm, which is then pulverized to obtain carbonized material powder.
[0013] As a possible implementation manner, further, the amount of starch added in this solution is 1-4% of the weight of the carbonized material powder, and the amount of distilled plant tar added is 25-40% of the weight of the carbonized material powder.
[0014] As a preferred implementation option, preferably, the distilled plant tar described in this scheme is a tar by-product produced during the carbonization process of bamboo, wood, fruit shells, etc., which is obtained by low-temperature distillation at a distillation temperature of 160-240°C.
[0015] As a possible implementation method, further, in this scheme, after the carbonized material powder is mixed with starch and distilled plant tar, water is added for kneading, the mixture is first granulated by an oil press to form a φ6-10mm columnar material, and then the mixture is granulated and formed into a φ2-5mm columnar material. Finally, the columnar material is carbonized and activated in a water vapor atmosphere to obtain a high-strength, high-ignition-point palm shell physical method columnar activated carbon.
[0016] As a preferred implementation option, preferably, the carbonization temperature of the columnar material in this scheme is 450-650°C, and the insulation is 10-60 minutes, and the ambient temperature for water vapor atmosphere activation is 850-950°C, and the insulation is 30-120 minutes.
[0017] As a preferred implementation option, preferably, this solution includes the following steps:
[0018] (1) Raw material screening: The palm shell raw material is passed through a 3-mesh sieve to obtain coarse and thick particles of palm shell raw material larger than 3 mesh;
[0019] (2) soaking and washing: soaking the palm shell raw material obtained by screening in step (1) in a sodium carbonate solution with a mass concentration of 1 to 10% for 1 hour and then filtering it; then soaking it in water for 1 hour and then filtering it, and then repeating the water soaking and filtering, and the number of repetitions is greater than 4 times to obtain a washed material;
[0020] (3) Drying and carbonization: After drying the washed material until the moisture content is less than 15%, place it in a steam atmosphere and carbonize it at 450-650°C for 10-120 minutes to obtain a carbonized material;
[0021] (4) Crushing and screening: The carbonized material is coarsely crushed using a double-roll crusher with a spacing of 3-6 mm, and then screened to obtain carbonized material with a particle size greater than 1.5 mm, which is then crushed to obtain carbonized material powder;
[0022] (5) Granulation: After the carbonized material powder is uniformly mixed with starch and distilled plant tar, an appropriate amount of water is added for kneading, and then granulated by a hydraulic press to form a columnar material of φ6-10 mm, and then granulated again to form a columnar material of φ2-5 mm, wherein the amount of starch added is 1-4% of the weight of the carbonized material powder, and the amount of distilled plant tar added is 25-40% of the weight of the carbonized material powder;
[0023] (6) Carbonization and activation: The columnar material is carbonized and activated in a water vapor atmosphere to obtain a palm shell physical method columnar activated carbon with high strength and high ignition point. The carbonization temperature of the columnar material is 450-650°C, and the temperature is kept for 10-60 minutes. The ambient temperature of the water vapor atmosphere activation is 850-950°C, and the temperature is kept for 30-120 minutes.
[0024] In this solution, thin palm shells in the raw materials can be removed when the raw materials are screened.
[0025] By adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0026] (1) This scheme uses palm shell as raw material, and it can use palm shell after oil extraction. The white ash attached to the surface of the palm shell after oil extraction is wrapped and adhered by grease and is difficult to remove. If treated with strong alkali, strong acid, etc., it will destroy the physical properties of the palm shell material itself, and the residual alkali and acid will corrode the equipment and affect the granulation strength in the subsequent process. Therefore, this scheme uses sodium carbonate solution for soaking. The sodium carbonate solution can wash away the white ash and grease of the palm shell after oil extraction, which affect the strength of the prepared columnar activated carbon, but does not destroy the physical properties of the palm shell material. Its residue does not affect the product indicators of the columnar activated carbon and is non-corrosive to the equipment.
[0027] (2) In the present scheme, during the carbonization treatment, since the palm shell is carbonized in a water vapor atmosphere, the palm shell carbonized material has a stronger affinity with the binder. At the same time, the carbonized material is coarsely crushed, and the mechanical action of the crushing is utilized to peel off and screen out the impurities and fine powder on the surface of the carbonized material that affect the strength of the columnar activated carbon.
[0028] (3) The distilled plant tar used in this scheme is distilled at low temperature, which can remove most of the light components with pungent odors and increase the viscosity of the plant tar. As a binder for columnar activated carbon, the production process has less odor and the strength of the prepared columnar activated carbon is higher. In addition, the higher the distillation temperature, the higher the specific gravity of the prepared columnar activated carbon.
[0029] (4) This scheme adopts secondary granulation technology to prepare columnar activated carbon, which can improve the strength and specific gravity of the columnar activated carbon. DETAILED DESCRIPTION
[0030] The present invention will be further described in detail below in conjunction with the embodiments. It is particularly noted that the following embodiments are only used to illustrate the present invention, but are not intended to limit the scope of the present invention. Similarly, the following embodiments are only partial embodiments of the present invention rather than all embodiments, and all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] This embodiment provides a method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon, which comprises the following steps:
[0033] (1) Raw material screening: The palm shell raw material is passed through a 3-mesh sieve to obtain coarse and thick particles of palm shell raw material larger than 3 mesh;
[0034] (2) soaking and washing: soaking the palm shell raw material obtained by screening in step (1) in a sodium carbonate solution with a mass concentration of 5% for 1 hour and then filtering it; then soaking it in water for 1 hour and then filtering it, and then repeating the water soaking and filtering, and repeating the process 4 times to obtain a washed material;
[0035] (3) Drying and carbonization: After drying the washed material until the moisture content is less than 15%, it is placed in a steam atmosphere and carbonized at 500°C for 20 minutes to obtain a carbonized material;
[0036] (4) Crushing and screening: The carbonized material is coarsely crushed using a double-roll crusher with a spacing of 3-6 mm, and then screened to obtain carbonized material with a particle size greater than 1.5 mm, which is then crushed to obtain carbonized material powder;
[0037] (5) Granulation: After the carbonized material powder is uniformly mixed with starch and distilled plant tar, an appropriate amount of water is added and kneaded, and then granulated by a hydraulic press to form a φ9 mm columnar material, and then granulated again to form a φ4 mm columnar material, wherein the starch is added in an amount of 2% by weight of the carbonized material powder, and the distilled plant tar is obtained by low-temperature distillation at 200° C., and its addition amount is 33% by weight of the carbonized material powder;
[0038] (6) Carbonization and activation: The columnar material is carbonized and activated in a water vapor atmosphere to obtain a palm shell physical method columnar activated carbon with high strength and high ignition point. The carbonization temperature of the columnar material is 500°C and kept warm for 20 minutes. The ambient temperature of the water vapor atmosphere activation is 900°C and kept warm for 60 minutes.
[0039] Among them, the palm shell physical method columnar activated carbon prepared in this embodiment has no obvious signs of powdering on its surface after activation.
[0040] Example 2
[0041] This embodiment provides a method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon, which comprises the following steps:
[0042] (1) Raw material screening: The palm shell raw material is passed through a 3-mesh sieve to obtain coarse and thick particles of palm shell raw material larger than 3 mesh;
[0043] (2) soaking and washing: soaking the palm shell raw material obtained by screening in step (1) in a sodium carbonate solution with a mass concentration of 1% for 1 hour and then filtering it; then soaking it in water for 1 hour and then filtering it, and then repeating the water soaking and filtering, and repeating the process 4 times to obtain a washed material;
[0044] (3) Drying and carbonization: After drying the washed material until the moisture content is less than 15%, it is placed in a steam atmosphere and carbonized at 450°C for 120 minutes to obtain a carbonized material;
[0045] (4) Crushing and screening: crushing the carbonized material with a double-roll crusher with a spacing of 3-6 mm, then screening to obtain carbonized material with a particle size greater than 1.5 mm, and then crushing it to obtain carbonized material powder;
[0046] (5) Granulation: After the carbonized material powder is uniformly mixed with starch and distilled plant tar, an appropriate amount of water is added and kneaded, and then granulated by a hydraulic press to form a φ10 mm columnar material, and then granulated again to form a φ5 mm columnar material, wherein the starch is added in an amount of 4% by weight of the carbonized material powder, and the distilled plant tar is obtained by low-temperature distillation at 240° C., and its addition amount is 25% by weight of the carbonized material powder;
[0047] (6) Carbonization and activation: The columnar material is carbonized and activated in a water vapor atmosphere to obtain a palm shell physical method columnar activated carbon with high strength and high ignition point. The carbonization temperature of the columnar material is 450°C and kept warm for 60 minutes. The ambient temperature of the water vapor atmosphere activation is 850°C and kept warm for 120 minutes.
[0048] Among them, the palm shell physical method columnar activated carbon prepared in this embodiment has no obvious signs of powdering on its surface after activation.
[0049] Example 3
[0050] This embodiment provides a method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon, which comprises the following steps:
[0051] (1) Raw material screening: The palm shell raw material is passed through a 3-mesh sieve to obtain coarse and thick particles of palm shell raw material larger than 3 mesh;
[0052] (2) soaking and washing: soaking the palm shell raw material obtained by screening in step (1) in a sodium carbonate solution with a mass concentration of 10% for 1 hour and then filtering it; then soaking it in water for 1 hour and then filtering it, and then repeating the water soaking and filtering, and repeating the process 4 times to obtain a washed material;
[0053] (3) Drying and carbonization: After drying the washed material until the moisture content is less than 15%, it is placed in a steam atmosphere and carbonized at 650°C for 10 minutes to obtain a carbonized material;
[0054] (4) Crushing and screening: The carbonized material is coarsely crushed using a double-roll crusher with a spacing of 3-6 mm, and then screened to obtain carbonized material with a particle size greater than 1.5 mm, which is then crushed to obtain carbonized material powder;
[0055] (5) Granulation: After the carbonized material powder is uniformly mixed with starch and distilled plant tar, an appropriate amount of water is added for kneading, and then granulated by a hydraulic press to form a φ6 mm columnar material, and then granulated again to form a φ2 mm columnar material, wherein the starch is added in an amount of 1% by weight of the carbonized material powder, and the distilled plant tar is obtained by low-temperature distillation at 160° C., and its addition amount is 40% by weight of the carbonized material powder;
[0056] (6) Carbonization and activation: The columnar material is carbonized and activated in a water vapor atmosphere to obtain a palm shell physical method columnar activated carbon with high strength and high ignition point. The carbonization temperature of the columnar material is 650°C and kept warm for 10 minutes. The ambient temperature of the water vapor atmosphere activation is 950°C and kept warm for 30 minutes.
[0057] Among them, the palm shell physical method columnar activated carbon prepared in this embodiment has no obvious signs of powdering on its surface after activation.
[0058] Comparative Example
[0059] This comparative example provides a method for preparing palm shell physical method columnar activated carbon, which comprises the following steps:
[0060] (1) Raw material screening: The palm shell raw material is passed through a 3-mesh sieve to obtain coarse and thick particles of palm shell raw material larger than 3 mesh;
[0061] (2) Drying and carbonization: placing the palm shell raw material in a steam atmosphere and carbonizing and keeping the temperature at 500°C for 20 min to obtain a carbonized material;
[0062] (3) Crushing and screening: The carbonized material is coarsely crushed by a double-roll crusher with a spacing of 3-6 mm, and then screened to obtain carbonized material with a particle size greater than 1.5 mm, which is then crushed to obtain carbonized material powder;
[0063] (4) Granulation: After the carbonized material powder is uniformly mixed with starch and distilled plant tar, an appropriate amount of water is added for kneading, and then granulated by a hydraulic press to form a φ9 mm columnar material, and then granulated again to form a φ4 mm columnar material, wherein the starch is added in an amount of 2% by weight of the carbonized material powder, and the distilled plant tar is obtained by low-temperature distillation at 200° C., and its addition amount is 33% by weight of the carbonized material powder;
[0064] (5) Carbonization and activation: The columnar material is carbonized and activated in a water vapor atmosphere to obtain a palm shell physical method columnar activated carbon with high strength and high ignition point. The carbonization temperature of the columnar material is 500°C and kept warm for 20 minutes. The ambient temperature of the water vapor atmosphere activation is 900°C and kept warm for 60 minutes.
[0065] Among them, the palm shell physical method columnar activated carbon prepared in this comparative example has obvious and serious surface powder removal after activation.
[0066] Comparison test
[0067] In order to facilitate the performance testing and comparison of the palm shell physical method columnar activated carbon obtained in the embodiment and comparative example of this scheme. According to the "Test Method for Wood Activated Carbon - Determination of Carbon Tetrachloride Adsorption Rate (Activity)" (GB / T 12496.5-1999), "Test Method for Wood Activated Carbon - Determination of Apparent Density" (GB / T12496.1-1999), "Test Method for Activated Carbon Ignition Point" (GB / T 20450-2006), "Test Method for Coal Granular Activated Carbon - Determination of Strength" (GB / T 7702.3-2008), the columnar activated carbon obtained in Examples 1, 2, 3 and the comparative example was tested for carbon tetrachloride adsorption rate, particle strength, ignition point and apparent density, and the results are as follows:
[0068]
[0069] Note: The higher the activation degree of columnar activated carbon (the higher the carbon tetrachloride adsorption rate), the lower the strength and specific gravity. If the activation degree of the comparative example is increased to a carbon tetrachloride adsorption rate of 60%, the strength will be less than 85.34%.
[0070] From the above comparison, it can be seen that the columnar activated carbon prepared by this scheme has excellent strength and high ignition point.
[0071] The above descriptions are only some embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any equivalent device or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon, characterized in that: It includes: After screening the palm shell raw material, soaking it in a sodium carbonate solution and then filtering it, then soaking it in water and filtering it, and the water soaking treatment is repeated for a preset number of times to obtain a washing material; After the washing material is dried, it is carbonized and kept warm for a preset time in a steam atmosphere to obtain a carbonized material; the carbonized material is coarsely crushed, screened and pulverized to obtain a carbonized material powder; the carbonized material powder is then mixed with starch and distilled plant tar, and water is added for kneading, followed by molding to obtain a columnar material; finally, the columnar material is carbonized and activated in a steam atmosphere to obtain a high-strength, high-ignition-point palm shell physical method columnar activated carbon.
2. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 1, characterized in that: The palm shell raw material was passed through a 3-mesh sieve, and the palm shell raw material larger than 3 mesh was alternately soaked with sodium carbonate solution and water.
3. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 1, characterized in that: The mass concentration of the sodium carbonate solution is 1-10%, and the time for soaking the palm shell raw material in the sodium carbonate solution and water is 1 hour / time; wherein, after the palm shell raw material is soaked in the sodium carbonate solution and filtered, the number of times of soaking in water and filtering is repeated 4 times; the moisture content of the washed material after drying is controlled within 15%.
4. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 1, characterized in that: After the washed material is dried, it is carbonized and kept warm at an ambient temperature of 450-650° C. for 10-120 minutes in a water vapor atmosphere to obtain a carbonized material.
5. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 1, characterized in that: The carbonized material is coarsely crushed by a double-roll crusher with a spacing of 3 to 6 mm, and then sieved to obtain carbonized material with a particle size greater than 1.5 mm, which is then pulverized to obtain carbonized material powder.
6. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 1, characterized in that: The added amount of the starch is 1-4% of the weight of the carbonized material powder, and the added amount of the distilled plant tar is 25-40% of the weight of the carbonized material powder.
7. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 6, characterized in that: The distilled plant tar is a tar byproduct produced during the carbonization process of bamboo, wood, fruit shells, etc. It is produced by low-temperature distillation at a distillation temperature of 160-240°C.
8. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 1, characterized in that: After the carbonized material powder is mixed with starch and distilled plant tar, water is added for kneading, and the mixture is first granulated into φ6-10mm columnar material by an oil press, and then granulated and molded into φ2-5mm columnar material. After carbonization and activation in a water vapor atmosphere, high-strength and high-ignition-point palm shell physical method columnar activated carbon is obtained.
9. The method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to claim 8, characterized in that: The carbonization temperature of the columnar material is 450-650°C, and the temperature is kept for 10-60 minutes. The ambient temperature for activation in a steam atmosphere is 850-950°C, and the temperature is kept for 30-120 minutes.
10. A method for preparing high-strength and high-ignition-point palm shell physical method columnar activated carbon according to any one of claims 1 to 9, characterized in that: It includes the following steps: (1) Raw material screening: The palm shell raw material is passed through a 3-mesh sieve to obtain coarse and thick particles of palm shell raw material larger than 3 mesh; (2) soaking and washing: soaking the palm shell raw material after screening in step (1) in a sodium carbonate solution with a mass concentration of 1 to 10% for 1 hour and then filtering it; then soaking it in water for 1 hour and then filtering it, and then repeating the water soaking and filtering, and the number of repetitions is greater than 4 times to obtain a washed material; (3) Drying and carbonization: After drying the washed material until the moisture content is less than 15%, place it in a steam atmosphere and carbonize it at 450-650°C for 10-120 minutes to obtain a carbonized material; (4) Crushing and screening: The carbonized material is coarsely crushed by a double-roll crusher with a spacing of 3-6 mm, and then screened to obtain carbonized material with a particle size greater than 1.5 mm, which is then crushed to obtain carbonized material powder; (5) Granulation: After the carbonized material powder is uniformly mixed with starch and distilled plant tar, an appropriate amount of water is added for kneading, and then granulated by a hydraulic press to form a columnar material of φ6-10 mm, and then granulated again to form a columnar material of φ2-5 mm, wherein the amount of starch added is 1-4% of the weight of the carbonized material powder, and the amount of distilled plant tar added is 25-40% of the weight of the carbonized material powder; (6) Carbonization and activation: The columnar material is carbonized and activated in a water vapor atmosphere to obtain a palm shell physical method columnar activated carbon with high strength and high ignition point. The carbonization temperature of the columnar material is 450-650°C, and the temperature is kept for 10-60 minutes. The ambient temperature of the water vapor atmosphere activation is 850-950°C, and the temperature is kept for 30-120 minutes.
Citation Information
Patent Citations
Granular activated carbon, and manufacturing method for same
CN104995136A
Preparation method of active carbon with large specific surface area
CN107140634A
Method for green preparation of molded activated carbon from agricultural processing residues
CN114620725A
Production method of high-ignition-point plant-based columnar activated carbon
CN117247009A
Preparation method of sodium ion negative electrode material and sodium ion negative electrode plate
CN117727899A