Decorative plaster material with antibacterial function and application thereof
By adding specific components such as antibacterial and adsorbents to the decorative stucco materials, the antibacterial and mechanical properties are improved, and the shortcomings of traditional stucco materials in antibacterial, antifouling and anti-compression bending are solved, and the further improvement is achieved High health, safety and service life.
Patent Information
- Application Number
- CN202411078335.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional decorative stucco materials have shortcomings in antibacterial and soil-resistant properties, compressive strength and bending strength, and it is difficult to effectively inhibit the growth of bacteria and mold in a wet or closed environment, affecting health and safety.
Antibacterial stucco materials containing silicon-aluminum powder, kaolin, quartz powder, diatomaceous earth, high-strength semi-water gypsum, calcium carbonate, reinforcement, retarder, carboxymethylcellulose, antibacterial agent and adsorbent, through specific The component ratio and preparation method improve the antibacterial and mechanical properties of the material.
It provides long-term antibacterial effect and maintains high compressive strength and bending strength within 28 days, significantly improving the health, safety and service life of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coatings, and in particular relates to a decorative plaster material with antibacterial function and application thereof. Background Art
[0002] The antibacterial function in interior decoration is particularly important. It can effectively reduce the harm of harmful substances such as bacteria and viruses to the human body, protect our health, and make our lives more secure and comfortable. Therefore, integrating antibacterial function into interior decoration and closely integrating it with healthy life has become a major trend in modern home design.
[0003] In the current decorative materials market, plaster decorative materials are widely used in indoor and outdoor decoration due to their good plasticity and aesthetics. However, with the improvement of people's living standards and the enhancement of health and environmental awareness, the problems and shortcomings of this type of traditional materials in terms of antibacterial and anti-pollution are becoming increasingly prominent. On the one hand, due to technical limitations, it is difficult for traditional decorative plaster materials to have long-lasting and effective antibacterial properties, which makes it easy for bacteria and mold to grow in a humid or closed environment, posing a potential threat to people's health. On the other hand, in terms of compressive strength and flexural strength, it is also relatively weak. Therefore, how to improve the antibacterial and anti-fouling properties, compressive strength and flexural strength of traditional decorative plaster materials has become an important challenge currently faced. Summary of the invention
[0004] The object of the present invention is to provide a decorative plaster material with antibacterial function and application thereof, so as to solve the problems raised in the above background technology.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: On the one hand, the present invention provides a decorative plaster material with antibacterial function, which comprises the following components: silica alumina powder, kaolin, quartz powder, diatomaceous earth, high-strength semi-hydrate gypsum, calcium carbonate, reinforcing agent, retarder, carboxymethyl cellulose, antibacterial agent, and adsorbent.
[0006] As a further improvement, the decorative plaster material with antibacterial function contains the following components in parts by mass: 10-25 parts of silica aluminum powder, 20-40 parts of kaolin, 5-12 parts of quartz powder, 10-15 parts of diatomaceous earth, 30-50 parts of high-strength semi-hydrate gypsum, 5-20 parts of calcium carbonate, 0.5-2 parts of reinforcing agent, 0.1-0.5 parts of retarder, 0.5-1 parts of carboxymethyl cellulose, 2-10 parts of antibacterial agent, and 0.1-2 parts of adsorbent.
[0007] As a further improvement, the adsorbent is prepared by reacting lignin sulfonic acid and N-ethylaniline.
[0008] As a further improvement, the method for preparing the adsorbent comprises the following steps:
[0009] (1.1) Mix lignin sulfonic acid and hydrochloric acid solution and stir until dissolved, add N-ethylaniline, continue to mix evenly and let stand for treatment;
[0010] (1.2) Mix the initiator and hydrochloric acid solution evenly and let it stand for treatment;
[0011] (1.3) The substance in step (1.2) is added dropwise into step (1.1) while stirring to fully react. After the reaction is completed, the mixture is filtered, washed, and dried to obtain an adsorbent.
[0012] As a further improvement, the antibacterial agent is a silver nitrate antibacterial agent and a quaternary ammonium salt antibacterial agent.
[0013] As a further improvement, the quaternary ammonium salt antibacterial agent is prepared by reacting succinic acid, diethylenetriamine and benzyl chloride.
[0014] As a further improvement, the preparation method of the quaternary ammonium salt antibacterial agent comprises the following steps:
[0015] (2.1) Succinic acid, diethylenetriamine and toluene are placed in a reactor, and then reacted at 130-180° C. for 2-6 hours, then heated to 185-200° C. for further reaction for 1-3 hours, and then kept warm for 2-6 hours, and then rotary evaporated to obtain an intermediate;
[0016] (2.2) The intermediate in step (2.1) is dissolved in anhydrous ethanol, and then benzyl chloride is added to react sufficiently, and then recrystallized and dried to obtain a quaternary ammonium salt antibacterial agent.
[0017] As a further improvement, 0.5-2 parts of a thickener are also included.
[0018] As a further improvement, the thickener is at least one of hydroxypropyl methylcellulose and hydroxyethyl cellulose.
[0019] As a further improvement, the reinforcing agent is calcium chloride.
[0020] As a further improvement, the thickener includes but is not limited to at least one of hydroxymethyl starch ether or hydroxypropyl starch ether.
[0021] On the other hand, the present invention also provides an application of a decorative plaster material with antibacterial function in exterior and interior walls of buildings.
[0022] Compared with the prior art, the beneficial effects of the present invention are: the decorative plaster material with antibacterial function provided by the present application has good antibacterial properties when placed for a long time, and has good mechanical properties such as 28d compressive strength and 28d flexural strength. DETAILED DESCRIPTION
[0023] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0024] In the following examples, except for adsorbent A and quaternary ammonium salt antibacterial agent, the other compound monomers and related reagents used can be purchased from the market, among which the retarder was purchased from Shandong Bofei Cement Technology Service Co., Ltd.
[0025] The preparation method of the adsorbent A comprises the following steps:
[0026] (1.1) Mix 2.7 g of lignin sulfonic acid and 700 mL of 2 mol / L hydrochloric acid solution and stir at room temperature until dissolved. Add 25.2 mL of N-ethylaniline and continue mixing. Place the mixture in a 0°C water bath for 0.5 h.
[0027] (1.2) Mix 46 g of ammonium persulfate and 300 mL of 2 mol / L hydrochloric acid solution and stir at room temperature until dissolved. Place the mixture in a 0°C water bath for 0.5 h.
[0028] (1.3) The substance in step (1.2) is added dropwise to step (1.1) while stirring, and the mixture is reacted in a 0°C water bath for 30 hours. After the reaction is completed, the reaction solution is filtered, washed with deionized water, and dried in a 50°C thermostat to obtain an adsorbent.
[0029] The preparation method of the quaternary ammonium salt antibacterial agent comprises the following steps:
[0030] (2.1) 30 g of succinic acid, 65 mL of diethylenetriamine and 300 mL of toluene were placed in a reactor, and then reacted at 165° C. for 5 h, then heated to 190° C. and continued to react for 2 h, then kept warm for 4 h, and then the toluene was removed by rotary evaporation to obtain an intermediate;
[0031] (2.2) The intermediate in step (2.1) was dissolved in 150 mL of anhydrous ethanol, and then 110 mL of benzyl chloride was added for sufficient reaction. The mixture was recrystallized three times with a mixed solvent (the mixed solvent was ethanol and acetone, and the volume ratio was 1:1), and then vacuum dried at 60° C. to obtain a quaternary ammonium salt antibacterial agent.
[0032] Embodiment 1:
[0033] A decorative plaster material with an antibacterial function comprises the following components in parts by mass: 12 parts of silicon aluminum powder, 30 parts of kaolin, 5 parts of quartz powder, 10 parts of diatomaceous earth, 30 parts of high-strength semi-hydrate gypsum, 12 parts of calcium carbonate, 1 part of calcium chloride, 0.2 parts of a retarder, 1 part of carboxymethyl cellulose, 3 parts of a quaternary ammonium salt antibacterial agent, 1 part of a silver nitrate antibacterial agent, and 0.5 parts of an adsorbent A.
[0034] Embodiment 2:
[0035] A decorative plaster material with antibacterial function, comprising the following components in parts by mass: 15 parts of silicon aluminum powder, 40 parts of kaolin, 10 parts of quartz powder, 10 parts of diatomaceous earth, 35 parts of high-strength semi-hydrate gypsum, 10 parts of calcium carbonate, 0.8 parts of calcium chloride, 0.4 parts of retarder, 0.5 parts of carboxymethyl cellulose, 2 parts of quaternary ammonium salt antibacterial agent, 3 parts of silver nitrate antibacterial agent, and 1 part of adsorbent A.
[0036] Embodiment 3:
[0037] A decorative plaster material with antibacterial function, comprising the following components in parts by mass: 12 parts of silicon aluminum powder, 25 parts of kaolin, 8 parts of quartz powder, 12 parts of diatomaceous earth, 32 parts of high-strength semi-hydrate gypsum, 15 parts of calcium carbonate, 1.5 parts of calcium chloride, 0.5 parts of retarder, 1 part of carboxymethyl cellulose, 4 parts of quaternary ammonium salt antibacterial agent, 1 part of silver nitrate antibacterial agent, and 1.5 parts of adsorbent A.
[0038] Embodiment 4:
[0039] A decorative plaster material with an antibacterial function comprises the following components in parts by mass: 12 parts of silicon aluminum powder, 30 parts of kaolin, 5 parts of quartz powder, 10 parts of diatomaceous earth, 30 parts of high-strength semi-hydrate gypsum, 12 parts of calcium carbonate, 1 part of calcium chloride, 0.2 parts of a retarder, 1 part of carboxymethyl cellulose, 4 parts of a silver nitrate antibacterial agent, and 0.5 parts of an adsorbent A.
[0040] Embodiment 5:
[0041] A decorative plaster material with antibacterial function comprises the following components in parts by mass: 12 parts of silicon aluminum powder, 30 parts of kaolin, 5 parts of quartz powder, 10 parts of diatomaceous earth, 30 parts of high-strength semi-hydrate gypsum, 12 parts of calcium carbonate, 1 part of calcium chloride, 0.2 parts of retarder, 1 part of carboxymethyl cellulose, 3 parts of quaternary ammonium salt antibacterial agent, 1 part of silver nitrate antibacterial agent, and 0.5 parts of sodium lignin sulfonate.
[0042] Comparative Example 1:
[0043] A decorative plaster material with antibacterial function, comprising the following components in parts by mass: 12 parts of silica-alumina powder, 30 parts of kaolin, 5 parts of quartz powder, 10 parts of diatomaceous earth, 30 parts of high-strength semi-hydrate gypsum, 12 parts of calcium carbonate, 1 part of calcium chloride, 0.2 parts of retarder, 1 part of carboxymethyl cellulose, 3 parts of quaternary ammonium salt antibacterial agent, and 1 part of silver nitrate antibacterial agent.
[0044] Comparative Example 2:
[0045] A decorative plaster material with antibacterial function comprises the following components in parts by mass: 12 parts of silicon aluminum powder, 30 parts of kaolin, 5 parts of quartz powder, 10 parts of diatomaceous earth, 30 parts of high-strength semi-hydrate gypsum, 12 parts of calcium carbonate, 1 part of calcium chloride, 0.2 parts of retarder, 1 part of carboxymethyl cellulose and 0.5 parts of adsorbent A.
[0046] When preparing the decorative plaster materials with antibacterial function required in Examples 1 to 5, the following production process is adopted:
[0047] A premixture is prepared by mixing silica-alumina powder, kaolin, quartz powder, diatomaceous earth, high-strength hemihydrate gypsum, calcium carbonate, calcium chloride, retarder, carboxymethyl cellulose, antibacterial agent and adsorbent in the required mass of the formula, and then the premixture is placed for 30 days, and then 40% wt of water is added to the premixture and mixed evenly. The stirring speed during mixing is 120 r / min and the stirring time is 15 min to obtain a decorative plaster material with antibacterial function.
[0048] When preparing the decorative plaster material with antibacterial function required in Comparative Example 1, the following production process is adopted:
[0049] A premix is prepared by mixing the required mass of silica-alumina powder, kaolin, quartz powder, diatomaceous earth, high-strength semi-hydrated gypsum, calcium carbonate, calcium chloride, retarder, carboxymethyl cellulose and antibacterial agent. The premix is then placed for 30 days, and water accounting for 40% wt of the premix is added and mixed evenly. The stirring speed during mixing is 120 r / min and the stirring time is 15 min to obtain a decorative plaster material with antibacterial function.
[0050] When preparing the decorative plaster material with antibacterial function required for Comparative Example 2, the following production process is adopted:
[0051] A premixture is prepared by mixing silica-alumina powder, kaolin, quartz powder, diatomaceous earth, high-strength hemihydrate gypsum, calcium carbonate, calcium chloride, retarder, carboxymethyl cellulose and adsorbent in the required mass of the formula, and then the premixture is placed for 30 days, and water accounting for 40%wt of the premixture is added and mixed evenly. The stirring speed during mixing is 120r / min and the stirring time is 15min to obtain a decorative plaster material with antibacterial function.
[0052] The test method is as follows:
[0053] Air sterilization test:
[0054] The decorative plaster materials with antibacterial function prepared in Examples 1-5 and Comparative Examples 1-2 were coated on 1 m 3 On the inner wall of the cabinet, during the test, Staphylococcus aureus liquid was sprayed into the cabinet, and then the bacterial count in the cabinet was measured, which was the bacterial count in the air before the experiment. After standing for 8 hours, the bacterial count in the cabinet was measured again, and the number of live Staphylococcus aureus was determined by qualitative testing in accordance with GB4789.10-2010.
[0055] Compressive strength and flexural strength test: The test is carried out in accordance with GB / T50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete".
[0056]
[0057] It can be seen from the comparison between the embodiment and the comparative example that when the components of the decorative plaster material with antibacterial function contain both the antibacterial agent and the adsorbent, the decorative plaster material with antibacterial function still has a high antibacterial rate even if it is placed for a long time;
[0058] By comparing Examples 1-3 and 4-5, it can be seen that when the components of the decorative plaster material with antibacterial function contain both an antibacterial agent and an adsorbent, and the antibacterial agent is an ammonium salt antibacterial agent or a silver nitrate antibacterial agent, and the adsorbent is adsorbent A, the obtained decorative plaster material with antibacterial function is placed for a long time, and the antibacterial agent is improved, and the 28d compressive strength and the 28d flexural strength have good mechanical properties;
[0059] In summary, the decorative plaster material with antibacterial function provided by the present application has good antibacterial properties when placed for a long time, and has good mechanical properties such as 28d compressive strength and 28d flexural strength.
[0060] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A decorative plaster material with antibacterial function, characterized in that: The decorative plaster material with antibacterial function comprises the following components: silica-alumina powder, kaolin, quartz powder, diatomaceous earth, high-strength semi-hydrate gypsum, calcium carbonate, a reinforcing agent, a retarder, carboxymethyl cellulose, an antibacterial agent, and an adsorbent.
2. The decorative plaster material with antibacterial function according to claim 1, characterized in that: The decorative plaster material with antibacterial function comprises the following components in parts by mass: 10-25 parts of silicon aluminum powder, 20-40 parts of kaolin, 5-12 parts of quartz powder, 10-15 parts of diatomaceous earth, 30-50 parts of high-strength semi-hydrate gypsum, 5-20 parts of calcium carbonate, 0.5-2 parts of reinforcing agent, 0.1-0.5 parts of retarder, 0.5-1 parts of carboxymethyl cellulose, 2-10 parts of antibacterial agent and 0.1-2 parts of adsorbent.
3. The decorative plaster material with antibacterial function according to claim 1, characterized in that: The adsorbent is prepared by reacting lignin sulfonic acid and N-ethylaniline.
4. The decorative plaster material with antibacterial function according to claim 3, characterized in that: The preparation method of the adsorbent comprises the following steps: (1.1) Mix lignin sulfonic acid and hydrochloric acid solution and stir until dissolved, add N-ethylaniline, continue to mix evenly and let stand for treatment; (1.2) Mix the initiator and hydrochloric acid solution evenly and let it stand for treatment; (1.3) The substance in step (1.2) is added dropwise into step (1.1) while stirring to fully react. After the reaction is completed, the mixture is filtered, washed, and dried to obtain an adsorbent.
5. The decorative plaster material with antibacterial function according to claim 1, characterized in that: The antibacterial agent is a silver nitrate antibacterial agent and a quaternary ammonium salt antibacterial agent.
6. The decorative plaster material with antibacterial function according to claim 5, characterized in that: The quaternary ammonium salt type antibacterial agent is prepared by reacting succinic acid, diethylenetriamine and benzyl chloride.
7. The decorative plaster material with antibacterial function according to claim 6, characterized in that: The preparation method of the quaternary ammonium salt antibacterial agent comprises the following steps: (2.1) Succinic acid, diethylenetriamine and toluene are placed in a reactor, and then reacted at 130-180° C. for 2-6 hours, then heated to 185-200° C. for further reaction for 1-3 hours, and then kept warm for 2-6 hours, and then rotary evaporated to obtain an intermediate; (2.2) The intermediate in step (2.1) is dissolved in anhydrous ethanol, and then benzyl chloride is added to react sufficiently, and then recrystallized and dried to obtain a quaternary ammonium salt antibacterial agent.
8. The decorative plaster material with antibacterial function according to claim 7, characterized in that: Also contains 0.5-2 parts of thickener.
9. The decorative plaster material with antibacterial function according to claim 8, characterized in that: The thickener is at least one of hydroxypropyl methylcellulose and hydroxyethyl cellulose.
10. Use of the decorative plaster material with antibacterial function according to any one of claims 1 to 9 in exterior and interior walls of buildings.