Zirconium-cerium double-metal modified MOF-808 as well as preparation method and application thereof

By doping lanthanide metal Ce in MOF-808, the rapid one-pot hydrothermal method is used to synthesize zirconium cerium bimetal modified MOF-808, the problem of poor photocatalytic performance of MOF-808 is solved, and the pollution of water is significantly improved The adsorption and photocatalytic removal of substances have achieved more efficient contaminant treatment.

CN118994622APending Publication Date: 2024-11-22BEIJING INST OF TECH TANGSHAN RES INST +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411254102.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing MOF-808 materials have poor photocatalytic performance and are difficult to effectively treat emerging pollutants, such as PPCPs in water bodies, and their defective structure affects the adsorption performance.

Method used

By doping lanthanide metal Ce in MOF-808, the synthesis of zirconium cerium bimetal modified MOF-808 is carried out by using a fast one-pot hydrothermal method to preserve adsorption and photocatalytic performance, and is used to adsorption and light of pollutants in water bodies. Catalytic removal.

Benefits of technology

The adsorption and photocatalytic removal rates of clobate and ibuprofen were significantly improved. Compared with undoped MOF-808, the adsorption removal rates were increased by 31.08% and 62.50%, and the photocatalytic removal rates were increased to 44.37% and 98.89%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994622A_ABST
    Figure CN118994622A_ABST
Patent Text Reader

Abstract

The invention discloses zirconium-cerium double-metal modified MOF-808 as well as a preparation method and application thereof, and relates to the technical field of MOF-808. According to the invention, Ce is doped on the basis of MOF-808 by adopting a rapid one-pot hydrothermal method to synthesize MOF-808 (Zr / Ce), and the MOF-808 (Zr / Ce) is used for adsorption and photocatalytic removal of emerging pollutants PPCPs in a water body. Compared with the MOF-808 (Zr), the MOF-808 (Zr / Ce) has the advantages that the adsorption removal rate of the MOF-808 (Zr / Ce) to the clofibric acid is increased from 1.76% to 31.08%, and the photocatalytic removal rate is increased from% to 44.37%; the adsorption removal rate of ibuprofen is increased from 2.34% to 62.50%, and the photocatalytic removal rate is increased from 40% to 98.89%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of MOF-808 materials, and in particular to a zirconium-cerium bimetallic modified MOF-808 and a preparation method and application thereof. Background Art

[0002] Metal organic frameworks (MOFs) are a new type of crystalline porous materials that have been widely explored as a highly versatile platform for functional applications in many research fields. Due to their high specific surface area and porosity, MOFs are widely used in many fields. Among the known MOF materials, zirconium-oxygen metal organic frameworks (Zr-MOFs) are often used in water environment treatment problems due to their precisely controllable pore structure and excellent thermal and chemical stability.

[0003] Zr-MOFs have a strong tolerance for structural defects of missing linkers. The ideal coordination number of Zr-MOFs ligands is 12, and a decrease in the coordination number (to 6 or 8) can form intrinsic defects in MOFs. In addition, by changing the number or type of linkers, the defects of Zr-MOFs can be rationally controlled to obtain large pore volumes and specific surface areas. Zr-MOFs can maintain their crystalline structure even in the presence of a large number of defects. MOF-808 is a zirconium-based MOF similar to UiO-66, in which each cluster is connected by 6 trimer linkers, while the other coordination of Zr ions is saturated by bridging formic acid molecules. These formic acid molecules can be removed by simple solvent washing or heat treatment, leaving two coordination vacancies on each metal site, occupied by a -OH group and an unstable H2O molecule, respectively. These properties provide great possibilities for MOF-808 to tolerate ligands of different topological structures and functions. Due to the electrostatic interaction, hydrogen bonding and Lewis acid-base interaction between MOF-808 and various pollutants, it has excellent adsorption performance, but its photocatalytic performance is poor. Summary of the invention

[0004] The present invention provides a zirconium-cerium bimetallic modified MOF-808 and a preparation method and application thereof, wherein lanthanide metal Ce is doped into the MOF-808 structure, aiming to retain the adsorption performance of MOF-808 while improving its catalytic performance.

[0005] In a first aspect, the present invention provides a method for preparing a zirconium-cerium bimetallic modified MOF-808 material, comprising the following steps: S1. Weigh trimesic acid and add it into N,N-dimethylformamide, perform ultrasonication until it is completely dissolved, and obtain a mixed solution A; S2, completely dissolving the zirconium salt and the cerium salt in ultrapure water respectively; S3, taking two metal salt solutions and quickly adding them to the mixed solution A, then adding formic acid, and mixing evenly to obtain a mixed solution B; S4. The mixed solution B is subjected to a heating treatment, then cooled to room temperature, centrifuged, and the separated solid product is washed with N,N-dimethylformamide and ethanol in succession, and activated by vacuum heating to obtain the final product.

[0006] Furthermore, the zirconium salt is ZrO(NO3)2, the cerium salt is Ce(NH4)2(NO3)6, the usage ratio of ZrO(NO3)2 to ultrapure water is 12.32g:100mL, and the usage ratio of Ce(NH4)2(NO3)6 to ultrapure water is 29.22g:100mL.

[0007] Furthermore, the usage ratio of trimesic acid to N,N-dimethylformamide in S1 is 67.2 mg:1.6 mL, to obtain a mixed solution A; S3 adds 0.2-1.2 mL of zirconium salt solution and 0-1.0 mL of cerium salt solution to the mixed solution A, and then adds 4.12 mL of formic acid.

[0008] Furthermore, the ultrasound time in S1 was 10 to 20 min.

[0009] Furthermore, the S4 heating temperature is 100°C, the holding time is 20 min; the centrifugal speed is 1000 r / min, and the centrifugal time is 30 min.

[0010] Furthermore, when S4 is cleaned, it is first cleaned with N,N-dimethylformamide by stirring for 3 days, and then cleaned with ethanol by stirring for 3 days.

[0011] In a second aspect, the present invention provides a zirconium-cerium bimetallic modified MOF-808 material obtained by the above method.

[0012] In a third aspect, the present invention provides an application of a zirconium-cerium bimetallic modified MOF-808 material in treating organic pollutants in sewage, especially in the adsorption and photocatalytic treatment of clofibric acid (CA) and ibuprofen (IBU).

[0013] Compared with the prior art, the present invention has at least the following beneficial effects: The present invention adopts a rapid one-pot hydrothermal method to dope Ce on the basis of MOF-808 to synthesize MOF-808 (Zr / Ce), and uses it for the adsorption and photocatalytic removal of emerging pollutants PPCPs in water bodies. First, a rapid one-pot hydrothermal method is used to statically synthesize MOF-808 (Zr / Ce) within 20 minutes. Material structure characterization shows that compared with MOF-808 (Zr), MOF-808 (Zr / Ce) retains the basic morphology of MOF-808, and Ce is successfully doped into MOF-808; compared with MOF-808 (Zr), the adsorption and removal rate of clofibric acid by MOF-808 (Zr / Ce=0.55) is increased from 1.76% to 31.08%, and the photocatalytic removal rate is increased from % to 44.37%; the adsorption and removal rate of ibuprofen is increased from 2.34% to 62.50%, and the photocatalytic removal rate is increased from 40% to 98.89%. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 The PXRD diffraction patterns of the products of Examples 1-3 and Comparative Examples provided by the present invention; Figure 2 The product photos of Examples 1-3 and Comparative Examples provided by the present invention, the samples from left to right are MOF-808 (Zr), MOF-808 (Zr / Ce=4.71), MOF-808 (Zr / Ce=1.88), MOF-808 (Zr / Ce=0.55); Figure 3 The SEM image of the comparative example product provided by the present invention; Figure 4 The SEM image of the product of Example 3 provided by the present invention; Figure 5 The adsorption and photocatalytic curves of clofibric acid by the products of Examples 1-3 and Comparative Examples provided by the present invention; Figure 6 The adsorption and photocatalytic curves of ibuprofen by the products of Examples 1-3 and Comparative Examples provided by the present invention; Figure 7 The bar graph is a graph showing the removal rates of clofibric acid and ibuprofen by the products of Example 3 and the comparative example provided by the present invention. DETAILED DESCRIPTION

[0015] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific implementation methods, but the present invention is not limited thereto. Example 1

[0016] Weigh 67.2 mg of H3BTC, add 1.6 mL of DMF, and sonicate for 15 min to completely dissolve it, which is mixed solution A. Weigh 12.32 g of ZrO(NO3)2 and 29.22 g of Ce(NH4)2(NO3)6 and completely dissolve them in two 100 mL portions of ultrapure water to obtain ZrO(NO3)2 solution and Ce(NH4)2(NO3)6 solution.

[0017] Then, 1.0 mL of ZrO(NO3)2 solution and 0.2 mL of Ce(NH4)2(NO3)6 solution were quickly added to the mixed solution A, and then 4.12 mL of formic acid was added. The completely mixed solution was transferred into an oven and kept at 100 °C for 20 min. After that, it was cooled to room temperature and centrifuged at 1000 r / min for 30 min. It was stirred and washed with DMF and ethanol for 6 days. The solid product after washing and separation was placed in a 70 °C vacuum oven and reacted for 12 h to obtain activated MOF-808 (Zr / Ce=4.71). Example 2

[0018] The difference from Example 1 is that 0.6 mL of ZrO(NO3)2 solution and 0.6 mL of Ce(NH4)2(NO3)6 solution are quickly added to the mixed solution A. The rest is the same as Example 1. The final product is recorded as MOF-808 (Zr / Ce=1.88). Example 3

[0019] The difference from Example 1 is that 0.2 mL ZrO(NO3)2 solution and 1.0 mL Ce(NH4)2(NO3)6 solution are quickly added to the mixed solution A. The rest is the same as Example 1. The final product is recorded as MOF-808 (Zr / Ce=0.55).

[0020] Comparative Example The difference from Example 1 is that only 1.2 mL of ZrO(NO3)2 solution is quickly added to the mixed solution A, and the rest is the same as Example 1. The final product is recorded as MOF-808 (Zr).

[0021] The products of Examples 1-3 and the comparative example were subjected to powder X-ray diffraction detection, and the results were as follows: Figure 1 The characteristic peaks corresponding to the (222) and (311) crystal planes of MOF-808 appear between 8° and 9°. As the Ce content increases, the corresponding diffraction peaks shift to the left. This is because Ce ions have a higher ionic radius (Ce 3+ :1.143 Å > Ce 4+ :0.97Å > Zr 4+: 0.84 Å for a coordination number of 8), the successful incorporation of Ce leads to unit cell expansion, resulting in a larger lattice parameter, which indicates that Ce is successfully doped and maintains the original crystalline structure of MOF-808.

[0022] In order to clearly observe the color change of the synthesized powder, the products of Examples 1-3 and the comparative example were evenly distributed in an acetone solution and photographed. The results are as follows: Figure 2 As shown, MOF-808 (Zr) appears white, and the modified MOF-808 (Zr / Ce) appears orange, and the color becomes darker with the increase of cerium dosage.

[0023] The products obtained in the comparative example and embodiment 3 were observed by scanning electron microscope respectively. Figure 3 and Figure 4 As shown. MOF-808 (Zr) has a clear and obvious octahedral structure, which is evenly distributed and has a relatively uniform size. The particle size of MOF-808 (Zr / Ce=0.55) becomes smaller with the addition of Ce metal and gradually becomes spherical, but the material still maintains the basic structure of MOF-808. The above results all show that the synthesized material has been successfully doped with Ce and maintains the basic morphology of the original MOF-808.

[0024] Adsorption and photocatalytic behavior detection: Wastewater A: Contains 400 μg·L of organic pollutant clofibric acid (CA) -1, (Prepared by adding drugs to ultrapure water); Wastewater B: Contains 400 μg·L of organic pollutant ibuprofen (IBU) -1 ; At room temperature, 40 mL of sewage A was taken in four portions, 2 mg of the product of Example 1 was added to the first portion, 2 mg of the product of Example 2 was added to the second portion, 2 mg of the product of Example 3 was added to the third portion, and 2 mg of the product of the comparative example was added to the last portion. The pH value of the solution was 6.5-7.0. The four portions were subjected to adsorption tests under dark conditions for 120 min. After reaching adsorption saturation, a xenon lamp (current 20 A, light power density 158.2 mW / cm 2 ) Simulate sunlight, with a light distance of 10 cm, and conduct photocatalytic tests.

[0025] Wastewater B was also subjected to adsorption and photocatalytic tests according to the above operation steps and dosage. The results are as follows Figures 5 to 7 shown.

[0026] like Figure 5 and Figure 6As shown in the figure, during the adsorption and photocatalytic process, the two drugs can reach adsorption saturation equilibrium within 50 minutes, both of which show a fast adsorption rate. Among them, MOF-808 (Zr) has poor adsorption capacity for both drugs, and the adsorption removal rate is less than 5%. MOF-808 (Zr / Ce=0.55) has different degrees of improvement in the adsorption and removal performance of CA and IBU, especially the adsorption and removal effect of IBU has been greatly improved. In the photocatalytic process, MOF-808 (Zr) has no photocatalytic ability for CA and IBU pollutants. MOF-808 (Zr / Ce=0.55) has different photocatalytic degradation capabilities for both drugs, and has better degradation performance for IBU, degrading 97.32% within 30 minutes.

[0027] like Figure 7 As shown, within 2 h of photocatalysis after adsorption equilibrium, the degradation rate of CA by MOF-808 (Zr / Ce=0.55) reached 44.37%, and the degradation rate of IBU reached 98.89%.

[0028] Finally, it should be noted that the above are only preferred embodiments of the present invention. Of course, those skilled in the art can make changes and modifications to the present invention. If these modifications and variations fall within the scope of the claims of the present invention and their equivalent technologies, they should be considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing a zirconium-cerium bimetallic modified MOF-808 material, characterized in that: The steps include: S1. Weigh trimesic acid and add it into N,N-dimethylformamide, perform ultrasonication until it is completely dissolved, and obtain a mixed solution A; S2. Dissolving zirconium salt and cerium salt completely into ultrapure water respectively; S3, taking two metal salt solutions and quickly adding them to the mixed solution A, then adding formic acid, and mixing evenly to obtain a mixed solution B; S4, heating the mixed solution B at 100°C for 20 minutes; The mixture was then cooled to room temperature and centrifuged, and the separated solid product was washed with N,N-dimethylformamide and ethanol in succession, and activated by vacuum heating to obtain the final product.

2. The method for preparing the zirconium-cerium bimetallic modified MOF-808 material according to claim 1, characterized in that: The zirconium salt used is ZrO(NO3)2, the cerium salt used is Ce(NH4)2(NO3)6, the dosage ratio of ZrO(NO3)2 to ultrapure water is 12.32g:100mL, and the dosage ratio of Ce(NH4)2(NO3)6 to ultrapure water is 29.22g:100mL.

3. The method for preparing the zirconium-cerium bimetallic modified MOF-808 material according to claim 2, characterized in that: The dosage ratio of trimesic acid to N,N-dimethylformamide in S1 is 67.2 mg:1.6 mL, and a mixed solution A is obtained; S3: 0.2-1.2 mL of zirconium salt solution and 0-1.0 mL of cerium salt solution are added to the mixed solution A, and then 4.12 mL of formic acid is added.

4. The method for preparing the zirconium-cerium bimetallic modified MOF-808 material according to claim 1, characterized in that: The ultrasound time in S1 is 10~20min.

5. The method for preparing the zirconium-cerium bimetallic modified MOF-808 material according to claim 1, characterized in that: The centrifugal speed of S4 was 1000 r / min and the centrifugal time was 30 min.

6. The method for preparing the zirconium-cerium bimetallic modified MOF-808 material according to claim 1, characterized in that: When cleaning S4, first use N,N-dimethylformamide for stirring cleaning for 3 days, and then use ethanol for stirring cleaning for 3 days.

7. The preparation method of the zirconium-cerium bimetallic modified MOF-808 material according to any one of claims 1 to 6 obtains the zirconium-cerium bimetallic modified MOF-808 material.

8. Application of the zirconium-cerium bimetallic modified MOF-808 material according to claim 7 in treating organic pollutants in sewage.

Citation Information

Patent Citations

  • Application of TCPP coordinated MOF material in antibiotic-containing sewage

    CN115991515A

  • Metal organic frameworks for removal of elemental impurities in pharmaceutical products

    US20210354107A1