Diaphragm and preparation method thereof, electrode assembly, battery and electric device

By setting up a sodium supplementation layer on the sodium secondary battery separator and using melt coextrusion technology to closely combine the sodium supplementation material with the base film, the problem of sodium loss in the sodium secondary battery is solved, and the circulation performance and capacity maintenance of the battery are improved Rate.

CN119009368APending Publication Date: 2024-11-22CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310551997.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There is a problem of sodium loss during the circulation of sodium secondary batteries, which affects battery performance.

Method used

Design a separator, including a base film and a sodium supplement layer arranged on the base film side. The sodium supplement layer consists of sodium supplement material and polymer. The sodium supplement layer is closely combined with the base film through melt coextrusion technology to improve the sodium supplementation layer. The firmness and ion conduction ability of the sodium layer.

Benefits of technology

It effectively improves the sodium supplement effect of sodium secondary batteries, improves the circulation performance and capacity retention rate of the battery, reduces the shedding of sodium supplement materials during folding and curling, and reduces production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009368A_ABST
    Figure CN119009368A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a diaphragm and a preparation method thereof, an electrode assembly, a battery and an electric device. The diaphragm comprises a base membrane and a sodium supplementing layer arranged on at least one side of the base membrane, the sodium supplementing layer comprises a sodium supplementing material, and the sodium supplementing effect of the diaphragm in the sodium secondary battery is improved by arranging the sodium supplementing layer on the base membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a diaphragm and a preparation method thereof, an electrode assembly, a battery and an electrical device. Background Art

[0002] Sodium secondary batteries have great development prospects in the field of large-scale energy storage due to their abundant sodium reserves.

[0003] There is a problem of sodium loss during the cycle of sodium secondary batteries. Summary of the invention

[0004] The main object of the present invention is to provide a separator aimed at improving the performance of sodium secondary batteries.

[0005] To achieve the above object, the present invention provides a diaphragm, which includes a base film and a sodium supplement layer provided on at least one side of the base film, wherein the sodium supplement layer includes a sodium supplement material.

[0006] The sodium replenishing effect of the separator in the sodium secondary battery is improved by arranging a sodium replenishing layer on the base film.

[0007] Optionally, the sodium supplement layer further comprises a polymer, and the polymer is coated on the surface of the sodium supplement material.

[0008] The diaphragm includes a base film and a sodium-supplementing layer arranged on at least one side of the base film. The sodium-supplementing layer includes a sodium-supplementing material and a polymer coated on the surface of the sodium-supplementing material. The sodium-supplementing material is coated by the polymer so that the sodium-supplementing material in the sodium-supplementing layer is not easy to fall off from the base film, thereby improving the sodium-supplementing effect of the diaphragm in the sodium secondary battery.

[0009] Optionally, the ratio of the thickness of the sodium supplement layer to the thickness of the base film is 1:3 to 3:2.

[0010] In order to improve the sodium replenishment capacity and ion conductivity of the separator, the ratio of the thickness of the sodium replenishment layer to the thickness of the base film is 1:3 to 3:2.

[0011] Optionally, the thickness of the sodium supplement layer ranges from 1 μm to 15 μm. Optionally, the thickness of the sodium supplement layer ranges from 3 μm to 10 μm.

[0012] And / or, the thickness of the base film ranges from 5 μm to 15 μm, optionally, the thickness of the base film ranges from 5 μm to 10 μm;

[0013] And / or, the thickness of the diaphragm ranges from 6 μm to 30 μm. Optionally, the thickness of the diaphragm ranges from 8 μm to 20 μm.

[0014] In order to improve the sodium supplementation ability of the separator, the thickness of the sodium supplementation layer ranges from 1 μm to 15 μm. Optionally, the thickness of the sodium supplementation layer ranges from 3 μm to 10 μm.

[0015] In order to improve the ion conduction capability of the separator, the thickness of the base film is in a range of 5 μm to 15 μm. Optionally, the thickness of the base film is in a range of 5 μm to 10 μm.

[0016] In order to improve the sodium supplementation ability and ion conduction ability of the diaphragm, the thickness of the diaphragm ranges from 6 μm to 30 μm. Optionally, the thickness of the diaphragm ranges from 8 μm to 20 μm.

[0017] Optionally, the mass percentage of the sodium supplement material to the total mass of the sodium supplement layer is 20% to 50%. Optionally, the mass percentage of the sodium supplement material to the total mass of the sodium supplement layer is 25% to 35%.

[0018] In order to improve the ion conductivity and sodium supplementation capacity of the sodium supplementation layer, the mass percentage of the sodium supplementation material to the total mass of the sodium supplementation layer is 20% to 50%. Optionally, the mass percentage of the sodium supplementation material to the total mass of the sodium supplementation layer is 25% to 35%.

[0019] Optionally, the sodium supplement layer further includes a toughening agent, and the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 8% to 16%. Optionally, the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 10% to 15%.

[0020] In order to improve the firmness of the combination between the sodium supplement material and the polymer, and to improve the tightness of the combination between the sodium supplement layer and the base membrane layer, the sodium supplement layer also includes a toughening agent. Furthermore, in order to reduce the impact of excessive addition of the toughening agent on the diaphragm performance, the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 8% to 16%. Optionally, the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 10% to 15%.

[0021] Optionally, the sodium supplement material includes a sodium salt of a metal oxide and / or a non-metallic sodium salt.

[0022] Optionally, the sodium salt of the metal oxide includes Na 5 FeO 4 、Na 5 Fe 5 O 8 、Na 6 CoO 4 、Na 2 NiO 2 、NaCrO 2 At least one of;

[0023] And / or, the non-metallic sodium salt includes Na 2 CO 3 、Na 2 O、Na 2 S, Na 3 P, Na 3 N、Na 2 O 2 、Na 2 C 2 O 2 N 2 、Na 2 C 2 O 4 At least one of .

[0024] The sodium supplement materials in this application include but are not limited to Na 5 FeO 4 、Na 5 Fe 5 O 8 、Na 6 CoO 4 、Na 2 NiO 2 、NaCrO 2 、Na 2 CO 3 、Na 2 O、Na 2 S, Na 3 P, Na 3 N、Na 2 O 2 、Na 2 C 2 O 2 N 2 、Na 2 C 2 O 4 One or more of the sodium supplement materials can supplement the loss of sodium ions during the initial charge and discharge formation process, thereby improving the performance of the sodium secondary battery.

[0025] Optionally, the polymer includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide;

[0026] And / or, the sodium supplement layer further comprises a toughening agent, and the toughening agent comprises one or more of vinyl acetate copolymer, polyethylene octene co-elastomer, and polymer polyol;

[0027] And / or, the material of the base film includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide.

[0028] The polymer in the present application includes but is not limited to at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide.

[0029] The toughening agent in the present application includes, but is not limited to, one or more of vinyl acetate copolymer, polyethylene octene co-elastomer, and polymer polyol.

[0030] The material of the base film in the present application includes but is not limited to at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide.

[0031] Optionally, the volume average particle size Dv50 of the sodium supplementing material is in the range of 50 nm to 1 μm. Optionally, the volume average particle size Dv50 of the sodium supplementing material is in the range of 50 nm to 200 nm.

[0032] In order to improve the problem that the sodium supplement material has too large a particle size and thus blocks the micropores of the sodium supplement layer, to improve the problem that the sodium supplement material has too small a particle size and thus easily agglomerates, thus causing the uneven distribution of the sodium supplement material in the sodium supplement layer, and to facilitate the molding of the sodium supplement layer into a sodium supplement layer of appropriate thickness, the volume average particle size Dv50 of the sodium supplement material ranges from 50nm to 1μm. Optionally, the volume average particle size Dv50 of the sodium supplement material ranges from 50nm to 200nm.

[0033] Optionally, the material of the base film is the same as the material of the polymer.

[0034] Theoretically, the material of the base film and the material of the polymer can be the same or different, preferably the same, to improve the problem of inconsistent ion conduction rates between the base film and the sodium supplement layer, which affects battery performance.

[0035] Optionally, the sodium supplement layer also includes inorganic materials, and the inorganic materials include at least one of Al oxide, Al nitride, Si oxide, Si nitride, Fe oxide, Fe nitride, Fe oxyacid, Sn oxide, Ti oxide, Ti nitride, Cu oxide, Cu nitride, Mn oxide, Ge oxide, Zr oxide, Zn oxide, and Ni oxide.

[0036] In order to improve the high temperature resistance, wettability and hardness of the diaphragm, the sodium supplement layer also includes inorganic materials, including but not limited to at least one of Al oxide, Al nitride, Si oxide, Si nitride, Fe oxide, Fe nitride, Fe oxyacid, Sn oxide, Ti oxide, Ti nitride, Cu oxide, Cu nitride, Mn oxide, Ge oxide, Zr oxide, Zn oxide and Ni oxide. These inorganic materials have good wettability and can improve the wettability of the diaphragm. These inorganic materials have the characteristics of high temperature resistance and can improve the high temperature resistance of the diaphragm. These inorganic materials have a certain hardness and can act as a barrier to prevent metal dendrites from piercing the diaphragm and causing battery short circuit.

[0037] Optionally, the mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 5%. Optionally, the mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 2%.

[0038] And / or, the inorganic material includes Al 2 O 3 、SiO 2 , ZnO, Fe 2 O 3 、NiO、CuO、TiO 2 At least one of;

[0039] And / or, the volume average particle size Dv50 of the inorganic material is in the range of 0.5 μm to 50 μm. Optionally, the volume average particle size Dv50 of the inorganic material is in the range of 1 μm to 20 μm.

[0040] In order to improve the high temperature resistance, wettability and hardness of the diaphragm, the mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 5%. Optionally, the mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 2%.

[0041] The inorganic materials of this application include but are not limited to Al 2 O 3 、SiO 2 , ZnO, Fe 2 O 3 、NiO、CuO、TiO 2 The inorganic material has the characteristics of good mechanical strength, high electrochemical stability, and good wettability to the electrolyte.

[0042] In order to improve the problem of inorganic materials clogging the micropores of the sodium supplement layer, and to improve the problem of uneven distribution of inorganic materials in the sodium supplement layer caused by the easy agglomeration of inorganic materials, and to facilitate the molding of the sodium supplement layer into a sodium supplement layer of appropriate thickness, the volume average particle size Dv50 of the inorganic material ranges from 0.5μm to 50μm. Optionally, the volume average particle size Dv50 of the inorganic material ranges from 1μm to 20μm.

[0043] The present application provides a method for preparing a diaphragm, comprising:

[0044] preparing raw materials for the sodium supplementation layer;

[0045] The sodium supplement layer raw material is compounded to the base film to obtain a separator.

[0046] For example, the sodium supplement material can be prepared into a slurry and coated on the separator.

[0047] Optionally, the present application further provides a method for preparing a diaphragm, wherein in the step of preparing a raw material for a sodium supplementing layer; compounding the raw material for the sodium supplementing layer to a base film to obtain a diaphragm, the method comprises:

[0048] The sodium supplement material and the polymer are stirred and mixed to obtain a sodium supplement layer raw material;

[0049] The raw material of the sodium supplement layer and the material of the base film are respectively added into at least two extruders of the co-extrusion membrane device, and melt co-extruded, and a composite membrane base film is obtained through a cooling roller;

[0050] The composite membrane substrate is subjected to a cold drawing process to form holes, subjected to a heat treatment and a hot drawing process to form holes, and subjected to a shaping process to obtain a diaphragm.

[0051] Melt coextrusion refers to an extrusion process that uses several extruders to simultaneously supply different plastic melt streams to a compounding die to merge into a multi-layer composite product.

[0052] The sodium-supplementing layer and the base film are melt-coextruded simultaneously by co-extrusion technology, and the prepared diaphragm includes a polymer-coated sodium-supplementing material, which can improve the problem that the sodium-supplementing material is coated on the diaphragm due to insufficient adhesion, and the sodium-supplementing material falls off on the diaphragm during the folding and curling process when assembling the battery, resulting in reduced sodium-supplementing efficiency. In addition, the preparation method does not involve the use of organic solvents, thereby reducing production costs and environmental pollution.

[0053] Optionally, in the step of mixing the sodium supplementing material and the polymer to obtain the sodium supplementing layer raw material, the following steps are further included:

[0054] The sodium supplement material, polymer, toughening agent and / or inorganic material are stirred and mixed, the stirring speed is 400 r / min to 800 r / min, and the stirring time is 0.5 h to 1 h to obtain a sodium supplement layer raw material.

[0055] In the process of preparing the raw material of the sodium supplement layer, adding a toughening agent can improve the firmness of the combination between the sodium supplement material and the polymer, and improve the tightness of the combination between the sodium supplement layer and the base film layer.

[0056] Adding inorganic materials can improve the high temperature resistance, wettability and hardness of the diaphragm. Directly adding inorganic materials during the preparation of sodium supplement raw materials can produce a diaphragm with certain high temperature resistance, wettability and hardness. There is no need to use conventional coating steps to coat the slurry of inorganic materials on the surface of the base film, thus reducing the process steps.

[0057] Optionally, the step of adding the sodium supplement layer raw material and the base film material to at least two extruders of a co-extrusion membrane device, performing melt co-extrusion, and obtaining a composite film base sheet through a cooling roller includes:

[0058] The sodium supplement layer raw material and the base film material are respectively added into the two extruders of the co-extrusion diaphragm device, and melt co-extrusion is carried out under the condition that the width of the extrusion heads of the two extruders is the same and the ratio of the extrusion speed of the sodium supplement layer raw material to the extrusion speed of the base film material is 1:3 to 3:2, and a composite film substrate is obtained by passing through a cooling roller.

[0059] In order to obtain a sodium supplement layer and a base film of suitable thickness, during the extrusion process, the width of the extruder heads of the two extruders is controlled to be the same, and the ratio of the extrusion speed of the sodium supplement layer material to the extrusion speed of the base film material is 1:3 to 3:2, and melt co-extrusion is performed, and a composite film substrate is obtained through a cooling roller. The above steps are used to facilitate obtaining a separator of suitable thickness, reduce the cumbersome process caused by the secondary treatment of the positive and negative electrodes and the separator, and do not affect the structure and performance of the battery.

[0060] Optionally, the temperature of the cooling roller is 15°C to 30°C;

[0061] and / or, the thickness of the composite film substrate is 10 μm to 50 μm;

[0062] And / or, the cold drawing process is performed under the conditions of uniaxial stretching at a temperature of 15° C. to 30° C., a stretching ratio of 1 to 2 times, and a stretching speed of 0.01 m / min to 0.1 m / min;

[0063] And / or, the heat treatment condition is heating at 15°C to 30°C below the melting point of the polymer for 30min to 60min;

[0064] And / or, the conditions of the hot drawing process are uniaxial stretching at a temperature of 100° C. to 160° C., a stretching ratio of 1 to 5 times, and a stretching speed of 0.05 m / min to 0.5 m / min;

[0065] And / or, the shaping treatment conditions are: temperature 15°C to 30°C, time 0.5h to 2h.

[0066] During the preparation process of the diaphragm, the corresponding steps are made to meet the above conditions to obtain a diaphragm of suitable thickness.

[0067] The present application also provides an electrode assembly, which includes the diaphragm as described above, or includes the diaphragm obtained by the preparation method of the diaphragm as described above.

[0068] Optionally, the electrode assembly includes a positive electrode plate, and the sodium supplement layer is arranged on one side of the base film and faces the positive electrode plate.

[0069] Theoretically, there is no limitation on the setting direction of the sodium supplement layer. For example, it can be set toward the positive electrode plate or the negative electrode plate. Optionally, the sodium supplement layer is set toward the positive electrode plate. In this way, during the sodium supplement process, the sodium supplement material in the sodium supplement layer can timely replenish the sodium loss in the positive electrode plate.

[0070] The present application also provides a battery, which includes the electrode assembly as described.

[0071] The present application also provides an electrical device, which includes the battery as described above.

[0072] The diaphragm of the present application comprises a base film and a sodium supplement layer arranged on at least one side of the base film, wherein the sodium supplement layer comprises a sodium supplement material. By arranging the sodium supplement layer on the base film, the sodium supplement effect of the diaphragm in the sodium secondary battery is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0074] Figure 1 This is a scanning electron microscope image of the diaphragm of Example 1 of the present application;

[0075] Figure 2 This is a schematic diagram of the structure of a diaphragm according to an embodiment of the present application;

[0076] Figure 3 This is a schematic diagram of the structure of a diaphragm according to an embodiment of the present application;

[0077] Figure 4 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0078] Figure 5 yes Figure 4 An exploded view of a secondary battery according to an embodiment of the present application is shown;

[0079] Figure 6 is a schematic diagram of a battery module according to an embodiment of the present application;

[0080] Figure 7 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0081] Figure 8 yes Figure 7 An exploded view of a battery pack according to an embodiment of the present application is shown;

[0082] Fig. 9 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.

[0083] Description of Figure Numbers:

[0084] Label name Label name 100 Diaphragm 3 Lower box 10 Basement membrane 4 Battery Module 20 Sodium supplementation layer 5 Secondary battery 21 The first sodium supplementation layer 51 case 22 The second sodium supplementation layer 52 Electrode assembly 1 Battery Pack 53 Top cover assembly 2 Upper box

[0085] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0086] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0087] Hereinafter, the embodiments of the diaphragm and its preparation method, electrode assembly, battery and electrical device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0088] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0089] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0090] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0091] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0092] Compared with lithium secondary batteries with scarce elements such as lithium, cobalt and nickel, sodium secondary batteries have the advantages of abundant sodium resources and low raw material costs, which makes sodium secondary batteries have great development prospects in the field of energy storage.

[0093] There is a problem of sodium loss during the cycle of sodium secondary batteries.

[0094] For example, due to some irreversible reactions such as the formation of the solid electrolyte membrane (SEI membrane) on the negative electrode surface during the initial charge and discharge formation process, the positive electrode material will experience sodium ion loss, which will lead to a decrease in the energy density of the sodium secondary battery.

[0095] In order to solve the above technical problems, the present application provides a separator, aiming to improve the performance of sodium secondary batteries.

[0096] The diaphragm comprises a base film and a sodium supplement layer arranged on at least one side of the base film, and the sodium supplement layer comprises a sodium supplement material.

[0097] Diaphragm, in the structure of secondary battery, diaphragm is one of the key internal components. The performance of diaphragm determines the interface structure and internal resistance of the battery, directly affecting the battery's capacity, cycle and safety performance. Excellent performance diaphragm plays an important role in improving the comprehensive performance of the battery. The main function of the diaphragm is to separate the positive and negative electrodes of the battery to prevent the two electrodes from contacting and short-circuiting. In addition, it also has the function of allowing electrolyte ions to pass through.

[0098] The base film includes an organic microporous film, and the material of the base film includes an organic polymer material, for example, polyethylene, polypropylene, etc.

[0099] The sodium supplement layer includes a layered structure of a sodium supplement material, wherein the sodium supplement material includes a compound containing sodium element, including Na 5 FeO 4 、Na 5 Fe 5 O 8 、Na 6 CoO 4 etc. Figure 2 and Figure 3 The sodium supplement layer 20 shown in the figure is disposed on at least one side of the base film 10, that is, the sodium supplement layer 20 can be disposed on one side of the base film 10, or can be disposed on both sides of the base film 10 (such as Figure 3 As shown, the first sodium supplement layer 21 and the second sodium supplement layer 22 can be set as needed.

[0100] The sodium replenishing effect of the separator in the sodium secondary battery is improved by arranging a sodium replenishing layer on the base film.

[0101] In one embodiment, the sodium supplement layer further includes a polymer, and the polymer is coated on the surface of the sodium supplement material.

[0102] Polymer, a polymer refers to a high molecular weight compound composed of many identical, simple structural units repeatedly connected by covalent bonds, such as polyethylene, polypropylene, etc.

[0103] The polymer coated on the surface of the sodium supplement material indicates that the sodium supplement material in the sodium supplement layer is coated with the polymer, which reduces direct exposure of the sodium supplement material to the outside and improves the problem of side reactions caused by direct contact between the sodium supplement material and the electrolyte.

[0104] The sodium supplement material is coated by a polymer, so that the sodium supplement material in the sodium supplement layer is not easy to fall off from the base film, thereby improving the sodium supplement effect of the diaphragm in the sodium secondary battery.

[0105] It is understandable that the traditional sodium supplement material is obtained by adding a sodium supplement agent to the positive electrode material or coating a sodium supplement layer on the diaphragm. When the sodium supplement slurry is blended with the positive electrode active material, the following problems will occur: the sodium supplement slurry will affect the positive electrode binder PVDF (polyvinylidene fluoride), causing the slurry gel phenomenon and affecting the positive electrode coating; the sodium supplement material will leave holes in the electrode after charging, affecting the positive electrode structure and the performance of the positive electrode material. The sodium supplement layer coated on the diaphragm has insufficient adhesion and is easy to fall off.

[0106] The present application uses a polymer to coat the sodium supplement material, so that the sodium supplement material in the sodium supplement layer is not easy to fall off from the base film, thereby improving the sodium supplement effect of the diaphragm in the sodium secondary battery, and the performance of the positive electrode plate will not be affected after the sodium supplement material is consumed.

[0107] In one embodiment, the ratio of the thickness of the sodium supplement layer to the thickness of the base film is 1:3 to 3:2.

[0108] The thickness ratio refers to the ratio of the thickness of the sodium supplement layer to the thickness of the base film. For example, if the thickness of the sodium supplement layer is n1 and the thickness of the base film is n2, then the ratio of the thickness of the sodium supplement layer to the thickness of the base film is n1:n2.

[0109] In order to improve the sodium supplementation capacity and ion conduction capacity of the diaphragm, the ratio of the thickness of the sodium supplementation layer to the thickness of the base film is 1:3 to 3:2. It is understandable that the sodium supplementation layer itself also acts as an isolation membrane. The addition of sodium supplementation materials and inorganic materials in the sodium supplementation layer leads to a decrease in air permeability. When the thickness of the sodium supplementation layer and the base film is less than 1:3, the sodium supplementation capacity of the sodium supplementation layer does not meet the requirements. When it is greater than 3:2, the sodium supplementation layer is thicker, and the sodium supplementation material that is fully wrapped deep in the sodium supplementation layer cannot be decomposed and released, which further causes the diaphragm to be closed during the cycle, and the ion conduction capacity decreases rapidly. Therefore, considering the sodium supplementation capacity and ion conduction capacity of the diaphragm, the ratio of the thickness of the sodium supplementation layer to the thickness of the base film is 1:3 to 3:2.

[0110] In the above 1:3 to 3:2, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:3, 1:2, 1:1, 3:2, etc., as well as the range values ​​between any two of the above point values.

[0111] In one embodiment, the thickness of the sodium supplement layer ranges from 1 μm to 15 μm. Optionally, the thickness of the sodium supplement layer ranges from 3 μm to 10 μm.

[0112] In order to improve the sodium supplementation ability of the separator, the thickness of the sodium supplementation layer ranges from 1 μm to 15 μm. Optionally, the thickness of the sodium supplementation layer ranges from 3 μm to 10 μm.

[0113] In the above-mentioned 1μm to 15μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0114] In the above 3μm to 10μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, etc., and the range values ​​between any two of the above point values.

[0115] In one embodiment, the thickness of the base film ranges from 5 μm to 15 μm. Optionally, the thickness of the base film ranges from 5 μm to 10 μm.

[0116] In order to improve the ion conduction capability of the separator, the thickness of the base film is in a range of 5 μm to 15 μm. Optionally, the thickness of the base film is in a range of 5 μm to 10 μm.

[0117] In the above-mentioned 5μm to 15μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0118] In the above-mentioned 5μm to 10μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0119] In one embodiment, the thickness of the membrane is in a range of 6 μm to 30 μm. Optionally, the thickness of the membrane is in a range of 8 μm to 20 μm.

[0120] In order to improve the sodium supplementation ability and ion conduction ability of the diaphragm, the thickness of the diaphragm ranges from 6 μm to 30 μm. Optionally, the thickness of the diaphragm ranges from 8 μm to 20 μm.

[0121] In the above-mentioned 6μm to 30μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0122] In the above-mentioned 8μm to 20μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0123] In one embodiment, the mass percentage of the sodium supplement material to the total mass of the sodium supplement layer is 20% to 50%. Optionally, the mass percentage of the sodium supplement material to the total mass of the sodium supplement layer is 25% to 35%.

[0124] In order to improve the ion conductivity and sodium supplementation capacity of the sodium supplementation layer, the mass percentage of the sodium supplementation material to the total mass of the sodium supplementation layer is 20% to 50%. Optionally, the mass percentage of the sodium supplementation material to the total mass of the sodium supplementation layer is 25% to 35%.

[0125] In the above-mentioned 20% to 50%, the values ​​include the minimum and maximum values ​​of the range, and every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 20%, 23%, 25%, 27%, 28%, 30%, 33%, 35%, 37%, 38%, 40%, 43%, 45%, 47%, 48%, 50%, etc., and the range values ​​between any two of the above-mentioned point values.

[0126] In the above 25% to 35%, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, etc., as well as the range values ​​between any two of the above point values.

[0127] In one embodiment, the sodium supplement layer further includes a toughening agent, and the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 8% to 16%. Optionally, the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 10% to 15%.

[0128] In order to improve the firmness of the combination between the sodium supplement material and the polymer, and to improve the tightness of the combination between the sodium supplement layer and the base membrane layer, the sodium supplement layer also includes a toughening agent. Furthermore, in order to reduce the impact of excessive addition of the toughening agent on the diaphragm performance, the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 8% to 16%. Optionally, the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 10% to 15%.

[0129] In the above 8% to 16%, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, etc., and the range values ​​between any two of the above point values.

[0130] In the above 10% to 15%, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 10%, 11%, 12%, 13%, 14%, 15%, etc., and the range values ​​between any two of the above point values.

[0131] In one embodiment, the sodium supplement material includes a sodium salt of a metal oxide and / or a non-metallic sodium salt.

[0132] The sodium supplement materials in the present application include but are not limited to sodium salts of metal oxides and / or non-metallic sodium salts.

[0133] In one embodiment, the sodium salt of the metal oxide comprises Na 5 FeO 4 、Na 5 Fe 5 O 8 、Na 6 CoO 4 、Na 2 NiO 2 、NaCrO 2 At least one of; and / or, the non-metallic sodium salt comprises Na 2 CO 3 、Na 2 O、Na 2 S, Na 3 P, Na 3 N、Na 2 O 2 、Na2 C 2 O 2 N 2 、Na 2 C 2 O 4 At least one of .

[0134] The sodium supplement materials in this application include but are not limited to Na 5 FeO 4 、Na 5 Fe 5 O 8 、Na 6 CoO 4 、Na 2 NiO 2 、NaCrO 2 、Na 2 CO 3 、Na 2 O、Na 2 S, Na 3 P, Na 3 N、Na 2 O 2 、Na 2 C 2 O 2 N 2 、Na 2 C 2 O 4 One or more of the sodium supplement materials can supplement the loss of sodium ions during the initial charge and discharge formation process, thereby improving the performance of the sodium secondary battery.

[0135] In one embodiment, the polymer includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide; and / or the sodium supplement layer also includes a toughening agent, and the toughening agent includes one or more of vinyl acetate copolymer, polyethylene octene co-elastomer, and polymer polyol; and / or the material of the base film includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide.

[0136] The polymer in the present application includes but is not limited to at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide.

[0137] The toughening agent in the present application includes, but is not limited to, one or more of vinyl acetate copolymer (EVA), polyethylene octene co-elastomer (POE), and polymer polyol (POP).

[0138] The material of the base film in the present application includes but is not limited to at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide.

[0139] In one embodiment, the volume average particle size Dv50 of the sodium supplementing material is in a range of 50 nm to 1 μm. Optionally, the volume average particle size Dv50 of the sodium supplementing material is in a range of 50 nm to 200 nm.

[0140] Dv50 is the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%. Its physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%. Dv50 is also called the median diameter or median particle size. Dv50 is often used to indicate the average particle size of powders.

[0141] The volume particle size distribution Dv50 of the sodium supplement material can be tested by a method known in the art. As an example, GB / T 19077-2016 can be referred to, and a Malvern laser particle size analyzer can be used for characterization testing, such as a Malvern Mastersizer-3000 or other instrument.

[0142] In order to improve the problem that the sodium supplement material has too large a particle size and thus blocks the micropores of the sodium supplement layer, to improve the problem that the sodium supplement material has too small a particle size and thus easily agglomerates, thus causing the uneven distribution of the sodium supplement material in the sodium supplement layer, and to facilitate the molding of the sodium supplement layer into a sodium supplement layer of appropriate thickness, the volume average particle size Dv50 of the sodium supplement material ranges from 50nm to 1μm. Optionally, the volume average particle size Dv50 of the sodium supplement material ranges from 50nm to 200nm.

[0143] In the above-mentioned 50nm to 1μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 50nm, 70nm, 90nm, 100nm, 120nm, 140nm, 160nm, 180nm, 200nm, 220nm, 240nm, 260nm, 280nm, 300nm, 350nm, 400nm, 450nm, 500550nm, 600nm, 650nm, 700nm, 750nm, 800nm, 850nm, 900nm, 950nm, 1μm, etc., and the range value between any two of the above-mentioned point values.

[0144] In the above-mentioned 50nm to 200nm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 180nm, 200nm, etc., and the range values ​​between any two of the above-mentioned point values.

[0145] In one embodiment, the material of the base film is the same as the material of the polymer.

[0146] Theoretically, the material of the base film and the material of the polymer can be the same or different, preferably the same, to improve the problem of inconsistent ion conduction rates between the base film and the sodium supplement layer, which affects battery performance.

[0147] In one embodiment, the sodium supplement layer also includes inorganic materials, and the inorganic materials include at least one of Al oxide, Al nitride, Si oxide, Si nitride, Fe oxide, Fe nitride, Fe oxyacid, Sn oxide, Ti oxide, Ti nitride, Cu oxide, Cu nitride, Mn oxide, Ge oxide, Zr oxide, Zn oxide, and Ni oxide.

[0148] In order to improve the high temperature resistance, wettability and hardness of the diaphragm, the sodium supplement layer also includes inorganic materials, including but not limited to at least one of Al oxide, Al nitride, Si oxide, Si nitride, Fe oxide, Fe nitride, Fe oxyacid, Sn oxide, Ti oxide, Ti nitride, Cu oxide, Cu nitride, Mn oxide, Ge oxide, Zr oxide, Zn oxide and Ni oxide. These inorganic materials have good wettability and can improve the wettability of the diaphragm. These inorganic materials have the characteristics of high temperature resistance and can improve the high temperature resistance of the diaphragm. These inorganic materials have a certain hardness and can act as a barrier to prevent metal dendrites from piercing the diaphragm and causing battery short circuit.

[0149] In one embodiment, the mass percentage of the inorganic material to the total mass of the sodium-filling layer is 1% to 5%. Optionally, the mass percentage of the inorganic material to the total mass of the sodium-filling layer is 1% to 2%. And / or, the inorganic material includes Al 2 O 3 、SiO 2 , ZnO, Fe 2 O 3 ,NiO,CuO,TiO 2At least one of; and / or, the volume average particle size Dv50 of the inorganic material ranges from 0.5 μm to 50 μm, optionally, the volume average particle size Dv50 of the inorganic material ranges from 1 μm to 20 μm.

[0150] In order to improve the high temperature resistance, wettability and hardness of the diaphragm, the mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 5%. Optionally, the mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 2%.

[0151] The inorganic materials of this application include but are not limited to Al 2 O 3 、SiO 2 , ZnO, Fe 2 O 3 、NiO、CuO、TiO 2 The inorganic material has the characteristics of good mechanical strength, high electrochemical stability, and good wettability to the electrolyte.

[0152] In order to improve the problem of inorganic materials clogging the micropores of the sodium supplement layer, and to improve the problem of uneven distribution of inorganic materials in the sodium supplement layer caused by the easy agglomeration of inorganic materials, and to facilitate the molding of the sodium supplement layer into a sodium supplement layer of appropriate thickness, the volume average particle size Dv50 of the inorganic material ranges from 0.5μm to 50μm. Optionally, the volume average particle size Dv50 of the inorganic material ranges from 1μm to 20μm.

[0153] In the above-mentioned 0.5μm to 50μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0.5μm, 1μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0154] In the above 1μm to 20μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 5μm, 10μm, 15μm, 20μm, etc., and the range values ​​between any two of the above point values.

[0155] In the above 1% to 5%, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc., and the range values ​​between any two of the above point values.

[0156] In the above 1% to 2%, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1%, 1.2%, 1.5%, 1.7%, 2%, etc., and the range values ​​between any two of the above point values.

[0157] The present application provides a method for preparing a diaphragm, comprising: preparing a sodium-supplementing layer raw material; and compounding the sodium-supplementing layer raw material to a base film to obtain a diaphragm.

[0158] For example, the raw material of the sodium supplement layer can be made into a film separately, and then the base film and the sodium supplement layer can be laminated together; the raw material of the sodium supplement layer can also be prepared into a slurry and directly coated on the base film.

[0159] The present application also provides a method for preparing a diaphragm, in the steps of preparing a sodium-supplementing layer raw material; compounding the sodium-supplementing layer raw material to a base film to obtain a diaphragm, comprising: stirring and mixing a sodium-supplementing material and a polymer to obtain a sodium-supplementing layer raw material; respectively adding the sodium-supplementing layer raw material and the material of the base film to at least two extruders of a co-extrusion diaphragm device, performing melt co-extrusion, and obtaining a composite film substrate through a cooling roller; performing a cold drawing process on the composite film substrate to form holes, performing a heat treatment and a hot drawing process to form holes, and performing a shaping process to obtain a diaphragm.

[0160] Melt coextrusion refers to an extrusion process that uses several extruders to simultaneously supply different plastic melt streams to a compounding die to merge into a multi-layer composite product.

[0161] The sodium-supplementing layer and the base film are melt-coextruded simultaneously by co-extrusion technology, and the prepared diaphragm includes a polymer-coated sodium-supplementing material, which can improve the problem that the sodium-supplementing material is coated on the diaphragm due to insufficient adhesion, and the sodium-supplementing material falls off on the diaphragm during the folding and curling process when assembling the battery, resulting in reduced sodium-supplementing efficiency. In addition, the preparation method does not involve the use of organic solvents, thereby reducing production costs and environmental pollution.

[0162] In addition to the melt co-extrusion process, the sodium supplement layer can be made into a film separately, and then the base film and the sodium supplement layer can be laminated together; the material of the sodium supplement layer can also be prepared into a slurry and directly coated on the base film.

[0163] Through melt co-extrusion, the two layers can be tightly integrated into one, and the process is simple. Compared with the two-layer lamination and coating process that combines the base film and the sodium supplement layer together, the lamination process and the coating process are more complicated and there is a problem of loose bonding. In particular, the coating process has the problem of insufficient adhesion, which causes the sodium supplement layer to fall off, and it is easy to cause the diaphragm to be too thick.

[0164] The diaphragm of the present application is prepared by melt double-layer co-extrusion of the raw material of the sodium supplement layer and the material of the base film. The diaphragm provided by the present application will not affect the positive and negative electrode structures and performances of the sodium secondary battery while supplementing sodium ions during charging and discharging, and the preparation method is safe, simple, low-cost, and convenient for large-scale industrial production.

[0165] It can be understood that the preparation principle of the melt extrusion / stretching / heat setting method is that the polymer melt crystallizes under a high stress field to form a lamella structure perpendicular to the extrusion direction and arranged in parallel, and then the elastic material is obtained by heat treatment. After the hard elastic polymer film is stretched, the lamellae are separated and a large number of microfibers appear, thereby forming a large number of microporous structures, and then the microporous film is obtained by heat setting.

[0166] In one embodiment, the step of mixing the sodium-supplementing material and the polymer in a stirrer to obtain the raw material for the sodium-supplementing layer further includes: stirring and mixing the sodium-supplementing material, the polymer, the toughening agent and / or the inorganic material at a stirring speed of 400 r / min to 800 r / min and a stirring time of 0.5 h to 1 h to obtain the raw material for the sodium-supplementing layer.

[0167] In the process of preparing the raw material of the sodium supplement layer, adding a toughening agent can improve the firmness of the combination between the sodium supplement material and the polymer, and improve the tightness of the combination between the sodium supplement layer and the base film layer.

[0168] Adding inorganic materials can improve the high temperature resistance, wettability and hardness of the diaphragm. Directly adding inorganic materials during the preparation of sodium supplement raw materials can produce a diaphragm with certain high temperature resistance, wettability and hardness. There is no need to use conventional coating steps to coat the slurry of inorganic materials on the surface of the base film, thus reducing the process steps.

[0169] In one embodiment, the steps of adding the sodium supplement layer raw material and the base film material to at least two extruders of a co-extrusion diaphragm device respectively, performing melt co-extrusion, and obtaining a composite film substrate through a cooling roller include: adding the sodium supplement layer raw material and the base film material to the two extruders of the co-extrusion diaphragm device respectively, and performing melt co-extrusion under the condition that the extrusion heads of the two extruders have the same width and the ratio of the extrusion speed of the sodium supplement layer raw material to the extrusion speed of the base film material is 1:3 to 3:2, and obtaining a composite film substrate through a cooling roller.

[0170] It can be understood that when the ratio of the thickness of the sodium supplement layer to the thickness of the base film is 1:3, the ratio of the extrusion speed of the sodium supplement layer raw material to the extrusion speed of the base film material is 1:3, that is, the thickness ratio of the sodium supplement layer to the base film is controlled by controlling the extrusion speed.

[0171] In order to obtain a sodium supplement layer and a base film of suitable thickness, during the extrusion process, the width of the extruder heads of the two extruders is controlled to be the same, and the ratio of the extrusion speed of the sodium supplement layer material to the extrusion speed of the base film material is 1:3 to 3:2, and melt co-extrusion is performed, and a composite film substrate is obtained through a cooling roller. The above steps are used to facilitate obtaining a separator of suitable thickness, reduce the cumbersome process caused by the secondary treatment of the positive and negative electrodes and the separator, and do not affect the structure and performance of the battery.

[0172] In one embodiment, the temperature of the cooling roller is 15°C to 30°C; and / or, the thickness of the composite film substrate is 10μm to 50μm; and / or, the temperature of the cold drawing process is 15°C to 30°C, the stretching ratio is 1 to 2 times, and the stretching speed is 0.01m / min to 0.1m / min for uniaxial stretching; and / or, the heat treatment conditions are heating at 15°C to 30°C below the melting point of the polymer for 30min to 60min; and / or, the hot drawing process conditions are uniaxial stretching at a temperature of 100°C to 160°C, a stretching ratio of 1 to 5 times, and a stretching speed of 0.05m / min to 0.5m / min; and / or, the shaping treatment conditions are: temperature 15°C to 30°C, time 0.5h to 2h.

[0173] It can be understood that the heat treatment conditions are heating at 15°C to 30°C below the melting point of the polymer for 30min to 60min. Assuming the melting point of the polymer is 100°C, the heat treatment temperature is 70°C to 85°C and the heating time is 30min to 60min.

[0174] During the preparation process of the diaphragm, the corresponding steps are made to meet the above conditions to obtain a diaphragm of suitable thickness.

[0175] The present application also provides an electrode assembly, which includes the diaphragm as described above, or includes the diaphragm obtained by the preparation method of the diaphragm as described above.

[0176] In one embodiment, the electrode assembly includes a positive electrode plate, and the sodium supplement layer is disposed on one side of the base film and faces the positive electrode plate.

[0177] Theoretically, there is no limitation on the setting direction of the sodium supplement layer. For example, it can be set toward the positive electrode plate or the negative electrode plate. Optionally, the sodium supplement layer is set toward the positive electrode plate. In this way, during the sodium supplement process, the sodium supplement material in the sodium supplement layer can timely replenish the sodium loss in the positive electrode plate.

[0178] It is understandable that when a sodium supplement layer is provided on one side of the base film, an inorganic layer may be provided on the other side of the base film, and the inorganic layer includes an inorganic material and a polymer coating the inorganic material, that is, the inorganic material includes the inorganic material in the sodium supplement layer mentioned above, that is, in the process of preparing the diaphragm, the inorganic material and the polymer are stirred and mixed to obtain an inorganic layer raw material, and the inorganic layer raw material, the sodium supplement layer raw material, and the base film material are respectively added to the three extruders of the co-extrusion diaphragm device to prepare a diaphragm including a base film, a sodium supplement layer and an inorganic layer. The thickness of the inorganic layer is 1μm-5μm, for example, it can be 1μm, 2μm, 3μm, 4μm, 5μm, etc., that is, it can be any value within the range of 1μm-5μm.

[0179] In one embodiment, the present application also provides a battery, which includes the electrode assembly as described above.

[0180] Since the electrode assembly adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0181] In one embodiment, the present application further provides an electrical device, which includes the battery as described above.

[0182] Since the battery adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0183] In addition, the battery (secondary battery, battery module, battery pack) and the electric device of the present application will be described below with reference to the drawings as appropriate.

[0184] In one embodiment of the present application, a secondary battery is provided.

[0185] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. The separator is the separator improved above in this application.

[0186] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0187] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0188] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0189] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0190] In some embodiments, the positive electrode film layer may further include a conductive agent, for example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0191] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0192] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, and the negative electrode film layer includes a negative electrode active material.

[0193] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0194] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0195] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0196] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0197] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0198] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0199] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0200] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs.

[0201] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0202] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0203] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0204] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0205] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0206] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 4 The secondary battery 5 is a square structure as an example.

[0207] In some embodiments, reference Figure 5 , the outer package may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0208] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.

[0209] Figure 6 4 is an example of a battery module. Figure 6 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0210] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0211] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0212] Figure 7 and Figure 8 1 is a battery pack 1 as an example. Figure 7 and Figure 8 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0213] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0214] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0215] Fig. 9 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0216] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.

[0217] Example

[0218] Example 1

[0219] The average particle size of Na 6 CoO 4, polypropylene, and toughening agent EVA (vinyl acetate copolymer) are pre-mixed in a planetary mixer at a mass ratio of 35:50:14 at a speed of 600r / min for 40min to be uniformly stirred; the mixture and polypropylene are respectively added to a multi-layer co-extrusion diaphragm device, the width of the extruder head is controlled to be the same, so that the base film layer raw material is melt-coextruded at twice the extrusion speed of the sodium-supplemented layer mixture, and a composite film substrate with a thickness of 30μm is obtained after passing through a cooling roller at a temperature of 25°C; the composite film substrate is subjected to a unidirectional cold drawing process at a temperature of 20°C, a stretching ratio of 2, and a stretching speed of 0.08m / min, and then heated at 130°C for 40min for heat treatment, followed by unidirectional hot drawing at a temperature of 130°C, a stretching ratio of 3, and a stretching speed of 0.35m / min, and finally, after being shaped at a temperature of 23°C for 1h, a diaphragm with a sodium-supplemented layer thickness of 5μm and a base film layer thickness of 10μm is obtained.

[0220] Example 2 to Example 21

[0221] Based on Example 1, the thickness of the sodium supplement layer, the type of sodium supplement material, the particle size Dv50, the mass fraction, the material and mass fraction of the polymer, the inorganic material, and the material and thickness of the base film are adjusted to obtain Examples 2 to 21.

[0222] Embodiment 22

[0223] Will Na 6 CoO 4 , Ketjen black in a mass ratio of 85:15 as a solute, N-methylpyrrolidone (NMP) of the same mass as the solute is added to prepare a slurry, and the slurry is coated on the surface of a 10 μm polypropylene base film to form a coating with a coating thickness of 5 μm to form a diaphragm containing a sodium supplement layer. Except for the different diaphragms, the remaining steps for assembling the full battery are the same as those in Example 1.

[0224] Comparative Example 1

[0225] On the basis of Example 1, there is no sodium supplement layer on the base film, so as to obtain Comparative Example 1.

[0226] Preparation of positive electrode

[0227] Will Na 3 V 2 (PO 4 ) 2 F 3 The positive electrode active material, polyvinylidene fluoride (PVDF) and conductive agent acetylene black were dispersed and dissolved in N-methylpyrrolidone (NMP) solvent in a mass ratio of 90:5:5, and uniformly coated on an Al foil current collector as a positive electrode sheet.

[0228] Preparation of negative electrode

[0229] The active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber (SBR), and the thickener sodium hydroxymethyl cellulose (CMC) are dissolved in the solvent deionized water in a weight ratio of 96.2:0.8:0.8:1.2, and the mixture is evenly mixed to prepare a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.

[0230] Preparation of electrolyte

[0231] In an argon atmosphere glove box (H 2 O<0.1ppm, O 2 <0.1ppm), mix the organic solvent ethylene carbonate (EC) / ethyl methyl carbonate (EMC) in a volume ratio of 3 / 7, add 12.5% ​​NaPF 6 Dissolve the sodium salt in the organic solvent and stir evenly.

[0232] Preparation of sodium ion batteries

[0233] The separator, positive electrode sheet, and negative electrode sheet of Example 1 are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then wound to obtain a bare cell, and the bare cell is welded with a pole ear, and the bare cell is placed in an aluminum shell, and baked at 100°C to remove water, and then the electrolyte is injected and sealed to obtain an uncharged battery. The uncharged battery is then subjected to the processes of static, hot and cold pressing, formation, shaping, and capacity testing in sequence to obtain the sodium ion battery product of Example 1.

[0234] Test of the solidity and thermal shrinkage performance of the sodium filling layer of the diaphragm

[0235] The firmness performance test of the diaphragms of the examples and comparative examples of the present application:

[0236] Using a type I tester, the prepared diaphragm sample was placed on a copper shaft with a diameter of 2 mm, and the bending performance test was performed at a speed of 180° / s for 100 seconds. The sodium supplement layer that fell off was collected and weighed to calculate the shedding rate, which was divided into the following five levels: A, shedding rate ≤ 3%, basically no shedding; B, shedding rate between 3% and 6%; C, shedding rate between 6% and 10%; D, shedding rate between 10% and 20%; E, shedding rate greater than 20%. The experiment was conducted with reference to the standard GB / T 6742-2007 (bending test for paints and varnishes).

[0237] Thermal shrinkage performance test of the diaphragms of the present application examples and comparative examples:

[0238] With reference to the standard ISO 14616-1997 "Heat-shrinkable films of polyethylene, ethylene copolymers and mixtures thereof - Determination of shrinkage stress", the sample was cut into 15 mm × 130 mm strips using the FST-02 film heat shrinkage tester, and the heat shrinkage of the diaphragm heat-treated at 130°C for 30 minutes was tested.

[0239] Battery performance test

[0240] Battery capacity retention test

[0241] Taking Example 1 as an example, the battery capacity retention rate test process is as follows: at 25°C, the battery corresponding to Example 1 is charged to 4.3V at a constant current of 1 / 3C, then charged to a current of 0.05C at a constant voltage of 4.3V, left for 5 minutes, and then discharged to 2.8V at 1 / 3C. The obtained capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery, and record the discharge capacity Cn of the battery after the nth cycle at the same time. Then, the battery capacity retention rate Pn after each cycle is Cn / C0*100%. In this test process, the first cycle corresponds to n=1, the second cycle corresponds to n=2, and ... the 200th cycle corresponds to n=200. The battery capacity retention rate data corresponding to the embodiments and comparative examples in Tables 1 and 2 are the data measured after 200 cycles under the above test conditions, that is, the value of P200.

[0242] Table 1 Diaphragm parameter list

[0243]

[0244]

[0245] Table 2 Performance of diaphragm and corresponding sodium ion battery

[0246]

[0247]

[0248] It can be seen from the above table that the connection firmness between the sodium supplement layer and the base membrane of the diaphragm prepared by the co-extrusion diaphragm device is improved, the heat shrinkage resistance of the diaphragm is also improved, the first cycle charging capacity and discharge capacity of the sodium ion battery are also improved, and the battery 500 cycle capacity retention rate is also improved.

[0249] like Figure 1 As shown, Figure 1This is a scanning electron microscope image of the diaphragm prepared in Example 1. It can be seen from the figure that the diaphragm is formed with micropores, and the sodium-supplementing material is coated with a polymer, so that the sodium-supplementing material in the sodium-supplementing layer is not easy to fall off from the base film. The micropores formed on the diaphragm are helpful for the sodium-supplementing material to realize the transmission of sodium ions, thereby improving the sodium-supplementing effect of the diaphragm in the sodium secondary battery.

[0250] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A diaphragm, characterized in that: The diaphragm includes a base film and a sodium supplement layer provided on at least one side of the base film, and the sodium supplement layer includes a sodium supplement material.

2. The diaphragm according to claim 1, characterized in that The sodium supplement layer further comprises a polymer, and the polymer is coated on the surface of the sodium supplement material.

3. The diaphragm according to claim 1 or 2, characterized in that: The ratio of the thickness of the sodium supplement layer to the thickness of the base film is 1:3 to 3:

2.

4. The diaphragm according to any one of claims 1 to 3, characterized in that The thickness of the sodium supplement layer ranges from 1 μm to 15 μm. Optionally, the thickness of the sodium supplement layer ranges from 3 μm to 10 μm. And / or, the thickness of the base film ranges from 5 μm to 15 μm, optionally, the thickness of the base film ranges from 5 μm to 10 μm; And / or, the thickness of the diaphragm ranges from 6 μm to 30 μm. Optionally, the thickness of the diaphragm ranges from 8 μm to 20 μm.

5. The diaphragm according to any one of claims 1 to 4, characterized in that The mass percentage of the sodium supplement material to the total mass of the sodium supplement layer is 20% to 50%; optionally, the mass percentage of the sodium supplement material to the total mass of the sodium supplement layer is 25% to 35%.

6. The diaphragm according to any one of claims 1 to 5, characterized in that The sodium supplement layer also includes a toughening agent, and the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 8% to 16%; optionally, the mass percentage of the toughening agent to the total mass of the sodium supplement layer is 10% to 15%.

7. The diaphragm according to any one of claims 2 to 6, characterized in that The sodium supplement material includes sodium salt of metal oxide and / or non-metal sodium salt.

8. The diaphragm according to claim 7, characterized in that The sodium salt of the metal oxide includes at least one of Na5FeO4, Na5Fe5O8, Na6CoO4, Na2NiO2, and NaCrO2; And / or, the non-metallic sodium salt includes at least one of Na2O, Na2S, Na3P, Na3N, Na2O2, Na2C2O2N2, and Na2C2O4.

9. The diaphragm according to any one of claims 2 to 8, characterized in that The polymer includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide; And / or, the sodium supplement layer further comprises a toughening agent, and the toughening agent comprises one or more of vinyl acetate copolymer, polyethylene octene co-elastomer, and polymer polyol; And / or, the material of the base film includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polyvinylidene fluoride, polyamide, and polyimide.

10. The diaphragm according to any one of claims 1 to 9, characterized in that The volume average particle size Dv50 of the sodium supplementing material ranges from 50 nm to 1 μm; optionally, the volume average particle size Dv50 of the sodium supplementing material ranges from 50 nm to 200 nm.

11. The diaphragm according to any one of claims 2 to 10, characterized in that The material of the base film is the same as that of the polymer.

12. The diaphragm according to any one of claims 1 to 11, characterized in that The sodium supplement layer also includes inorganic materials, which include at least one of Al oxide, Al nitride, Si oxide, Si nitride, Fe oxide, Fe nitride, Fe oxyacid, Sn oxide, Ti oxide, Ti nitride, Cu oxide, Cu nitride, Mn oxide, Ge oxide, Zr oxide, Zn oxide, and Ni oxide.

13. The diaphragm according to claim 12, characterized in that The mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 5%. Optionally, the mass percentage of the inorganic material to the total mass of the sodium supplement layer is 1% to 2%. And / or, the inorganic material includes at least one of Al2O3, SiO2, ZnO, Fe2O3, NiO, CuO, and TiO2; And / or, the volume average particle size Dv50 of the inorganic material is in the range of 0.5 μm to 50 μm. Optionally, the volume average particle size Dv50 of the inorganic material is in the range of 1 μm to 20 μm.

14. A method for preparing a diaphragm according to any one of claims 1 to 13, characterized in that: include: preparing raw materials for the sodium supplementation layer; The sodium supplement layer raw material is compounded to the base film to obtain a separator.

15. The method for preparing a diaphragm according to claim 14, characterized in that: The steps of preparing a raw material for a sodium supplementing layer and compounding the raw material for the sodium supplementing layer to a base film to obtain a diaphragm include: The sodium supplement material and the polymer are stirred and mixed to obtain a sodium supplement layer raw material; The raw material of the sodium supplement layer and the material of the base film are respectively added into at least two extruders of the co-extrusion membrane device, and melt co-extruded, and a composite membrane base film is obtained through a cooling roller; The composite membrane substrate is subjected to a cold drawing process to form holes, subjected to a heat treatment and a hot drawing process to form holes, and subjected to a shaping process to obtain a diaphragm.

16. The method for preparing a diaphragm according to claim 15, characterized in that: The step of mixing the sodium supplement material and the polymer to obtain the sodium supplement layer raw material also includes: The sodium supplement material, polymer, toughening agent and / or inorganic material are stirred and mixed, the stirring speed is 400 r / min to 800 r / min, and the stirring time is 0.5 h to 1 h to obtain a sodium supplement layer raw material.

17. The method for preparing a diaphragm according to claim 15 or 16, characterized in that: The step of adding the sodium supplement layer raw material and the base film material to at least two extruders of the co-extrusion diaphragm device respectively, performing melt co-extrusion, and obtaining a composite film base sheet through a cooling roller includes: The sodium supplement layer raw material and the base film material are respectively added into the two extruders of the co-extrusion diaphragm device, and melt co-extrusion is carried out under the condition that the width of the extrusion heads of the two extruders is the same and the ratio of the extrusion speed of the sodium supplement layer raw material to the extrusion speed of the base film material is 1:3 to 3:2, and a composite film substrate is obtained by passing through a cooling roller.

18. The method for preparing a diaphragm according to any one of claims 15 to 17, characterized in that: The temperature of the cooling roller is 15°C to 30°C; and / or, the thickness of the composite film substrate is 10 μm to 50 μm; And / or, the cold drawing process is performed under the conditions of uniaxial stretching at a temperature of 15° C. to 30° C., a stretching ratio of 1 to 2 times, and a stretching speed of 0.01 m / min to 0.1 m / min; And / or, the heat treatment condition is heating at 15°C to 30°C below the melting point of the polymer for 30min to 60min; And / or, the conditions of the hot drawing process are uniaxial stretching at a temperature of 100° C. to 160° C., a stretching ratio of 1 to 5 times, and a stretching speed of 0.05 m / min to 0.5 m / min; And / or, the shaping treatment conditions are: temperature 15°C to 30°C, time 0.5h to 2h.

19. An electrode assembly, characterized in that: The electrode assembly comprises the separator according to any one of claims 1 to 13, or comprises a separator obtained by the method for preparing the separator according to any one of claims 14 to 18.

20. The electrode assembly according to claim 19, characterized in that The electrode assembly includes a positive electrode plate, and the sodium supplement layer is arranged on one side of the base film and faces the positive electrode plate.

21. A battery, characterized in that: The battery comprises the electrode assembly according to claim 19 or 20.

22. An electrical device, characterized in that: The electrical device comprises the battery as claimed in claim 21.

Citation Information

Cited By

  • Diaphragm, preparation method thereof and sodium ion battery

    CN119890613A

  • Modified diaphragm, preparation method thereof and negative-electrode-free sodium metal battery

    CN121149600A