Preparation method and application of full-spectrum response type photocatalyst
By preparing the full spectrum responsive photocatalyst Ca(OH)2@NaNb1-xFexO3-v, the problems of low solar energy utilization rate and high photogenerated electron-hole recombination rate of NaNbO3 photocatalyst are solved, and high efficiency is achieved for uranium-containing wastewater The treatment improves catalytic activity and resistance.
Patent Information
- Application Number
- CN202411346003.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-26
Smart Images

Figure CN119016059A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a spectrally responsive photocatalyst, belonging to the technical field of photocatalysis. Background Art
[0002] Uranium resources are the foundation of the development of the nuclear industry. With the rapid development of the nuclear energy industry, the demand for uranium used as nuclear fuel has also increased dramatically. Nuclear energy development and utilization, nuclear fuel processing, nuclear waste disposal and other activities have generated a large amount of uranium-containing radioactive wastewater. The efficient treatment of uranium-containing radioactive wastewater has always received great attention. Photocatalytic reduction technology has attracted much attention in the photocatalytic reduction of U(VI) due to its advantages such as cleanliness, no secondary pollution, low energy consumption, and normal temperature and pressure. Sodium niobate (NaNbO3) has a typical perovskite structure (ABO3) and has attracted widespread attention due to its excellent physical properties (such as high photoelectric and nonlinear optical coefficients, etc.), especially as a photocatalyst for its non-toxic and stable advantages, and is applied in the field of semiconductor heterogeneous catalysis. However, the band gap of NaNbO3 is about 3.2eV, the light absorption range is narrow, and the utilization rate of solar energy is low; on the other hand, when NaNbO3 is used as a photocatalyst, the photogenerated electron-hole recombination rate is very high, which makes the light quantum efficiency low, resulting in low photocatalytic activity of single NaNbO3, and its use is limited. Therefore, how to broaden the visible light response range of NaNbO3, promote the effective separation of photogenerated electrons and holes, and enhance its photocatalytic reduction activity is a key issue that needs to be solved urgently. Summary of the invention
[0003] The purpose of the present invention is to overcome the technical problems of low utilization rate of solar energy, easy recombination of photogenerated carriers and low catalytic activity of existing NaNbO3 photocatalysts during use, and to provide a preparation method and application of a full-spectrum responsive photocatalyst. The present invention broadens the response range of the photocatalyst to the solar spectrum, improves its quantum yield in the visible spectrum, effectively suppresses the recombination rate of photogenerated electrons and holes, improves the photocatalytic performance of the material, and has good acid and alkali resistance, thermal stability and resistance to ion interference, and the preparation method is simple, energy consumption and cost are low.
[0004] The preparation method of a full-spectrum responsive photocatalyst of the present invention is carried out according to the following steps:
[0005] 1. Add ferric nitrate and calcium nitrate into deionized water at a molar ratio of 1:(0-2.5), stir and dissolve to obtain a mixed solution I;
[0006] 2. Add NaOH solution dropwise to the mixed solution I and ensure that no precipitation is generated, and mix and react for 20 to 30 minutes to obtain a mixed solution II;
[0007] 3. Add niobium oxide (Nb2O5) to the mixed solution II and stir for 50 to 60 minutes to obtain a mixed solution III; transfer the mixed solution III to a hydrothermal reactor, place the reactor in a constant temperature drying oven at 140 to 180°C and heat to react for 4 to 6 hours; after the reaction is completed, cool to room temperature, separate the solid phase, wash the solid phase with deionized water, dry it, and obtain a full-spectrum responsive photocatalyst, grind it into powder, and seal it for storage.
[0008] Furthermore, the concentration of ferric nitrate in solution I described in step 1 is 0.06-0.2 mmol / mL.
[0009] Furthermore, the concentration of NaOH in step 2 is 12 mol / L.
[0010] Furthermore, the amount of niobium oxide in step three and the amount of iron nitrate in step one is 1:(0.05-6.0).
[0011] Furthermore, the reaction temperature in step 3 is 160° C. and the reaction time is 4 h.
[0012] Furthermore, the drying temperature in step three is 60-80° C., and the drying time is 6-8 hours.
[0013] The chemical formula of the full-spectrum responsive photocatalyst prepared by the above method is Ca(OH)2@NaNb 1-x Fe x O 3-v , where 0.2≤x<1.0 and V represents an oxygen vacancy.
[0014] The application of the full-spectrum responsive photocatalyst prepared by the above method is to use the full-spectrum responsive photocatalyst for the treatment of uranium-containing wastewater, wherein the uranium-containing wastewater contains U(VI).
[0015] The method for treating uranium-containing wastewater using a full-spectrum responsive photocatalyst is as follows: adding the full-spectrum responsive photocatalyst to the uranium-containing wastewater at a concentration of 0.2 to 0.3 g / L, adjusting the pH to 3.0 to 6.0, stirring for 20 to 30 minutes under sunlight irradiation, separating the full-spectrum responsive photocatalyst, and completing the treatment of uranium-containing wastewater. Photocatalytic reduction of U(VI) is carried out under sunlight irradiation, and soluble U(VI) is photocatalytically reduced to insoluble U(IV) and precipitated in the form of UO2.
[0016] The regeneration method of the full-spectrum responsive photocatalyst is: after the full-spectrum responsive photocatalyst adsorbed with uranium is oxidized in the air for 24 to 48 hours, it is eluted with a 0.1 mol / L NaHCO3 solution to remove the UO2 deposited on the photocatalyst, and then washed with water and dried to complete the regeneration of the full-spectrum responsive photocatalyst.
[0017] The preparation method of the present invention has low cost, simple process, environmentally friendly and non-toxic materials, easy-to-control reaction conditions, and no need to add any surfactant. The prepared composite photocatalytic material has a full spectrum response range, low photogenerated electron-hole recombination rate, and strong photocatalytic reduction activity. The composite material has a hexadecahedral morphology and abundant oxygen vacancies, and the photocatalytic reduction performance of U(VI) in the solution is greatly improved. More than 93.68% of U(VI) is rapidly reduced to insoluble U(IV) within 30 minutes under sunlight irradiation, and the theoretical reduction capacity is 826.45 mg·g -1 The reduction capacity of U(VI) under sunlight is 16 times that of single NaNbO3, and it still has strong reduction capacity after being recycled for 5 times. The full-spectrum responsive photocatalyst synthesized by the present invention can be used in the field of uranium-containing wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 FT-IR images of the full-spectrum responsive photocatalysts prepared in Comparison 1 and Examples 1 to 7;
[0019] Figure 2 The UV diffuse reflectance images of NNO prepared in Comparative Example 1 and the full-spectrum responsive photocatalysts prepared in Examples 1 to 4;
[0020] Figure 3 The UV diffuse reflectance graphs of the full-spectrum responsive photocatalysts prepared by NNO in Comparative Example 1 and Examples 1, 5, 6, and 7;
[0021] Figure 4 UV diffuse reflectance and band gap diagram of NNO in Comparative Example 1 and full spectrum responsive photocatalyst in Example 1;
[0022] Figure 5 The fluorescence spectra of NNO in Comparative Example 1 and the materials in Examples 1 to 4 are shown;
[0023] Figure 6 The photoluminescence spectra of NNO in comparative example 1 and the full-spectrum responsive photocatalysts in examples 1, 5, 6, and 7;
[0024] Figure 7 The photoluminescence spectra of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1;
[0025] Figure 8It is the oxygen vacancy test diagram of NNO in comparative example 1 and the full spectrum responsive photocatalyst in examples 1, 4, 5 and 6;
[0026] Fig. 9 It is the transient photocurrent diagram of NNO in comparative example 1 and CH-8@NNFO-4 in example 1;
[0027] Fig.10 Electrochemical impedance diagrams of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1;
[0028] Fig.11 SEM, TEM and EDS images of NNO prepared in Comparative Example 1;
[0029] Fig.12 The SEM, TEM and EDS images of CH-8@NNFO-4 prepared in Example 1;
[0030] Fig.13 FT-IR images of NNO prepared in Comparative Example 1 and CH-8@NNFO-4 prepared in Example 1;
[0031] Fig.14 XRD spectra of NNO prepared in Comparative Example 1 and CH-8@NNFO-4 in Example 1;
[0032] Fig.15 The thermal stability diagram of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1;
[0033] Fig.16 It is a specific surface area diagram of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1;
[0034] Fig.17 It is a photocatalytic reduction effect diagram of U(VI) by NNO in Comparative Example 1, CH-8@NNFO-4 in Example 1 under dark environment and sunlight irradiation conditions, and NNFO-4 in Example 2 under sunlight irradiation;
[0035] Fig.18 This is a diagram showing the effect of temperature and time on the photocatalytic reduction of U(VI) by CH-8@NNFO-4 under sunlight in Example 1;
[0036] Fig.19 This is a diagram showing the effect of pH on the photocatalytic reduction of U(VI) by CH-8@NNFO-4 under sunlight in Example 1;
[0037] Fig. 20 This is a diagram showing the effect of different anions and cations on the photocatalytic reduction of U(VI) by CH-8@NNFO-4 under sunlight in Example 1;
[0038] Fig.21 In order to add AgNO3 capture agent electron (e - ) conditions, the electron capture result of CH-8@NNFO-4 in Example 1 under sunlight irradiation in the photocatalytic reduction of U(VI);
[0039] Fig. 22 In order to capture superoxide radicals (·O2 - ) conditions, the CH-8@NNFO-4 of Example 1 captured superoxide radicals in the photocatalytic reduction of U(VI) under sunlight irradiation;
[0040] Fig.23 To capture holes (h + ) conditions, the hole capture result of CH-8@NNFO-4 in Example 1 under sunlight irradiation in photocatalytic reduction of U(VI);
[0041] Fig.24 This is a graph showing the capture results of hydroxyl radicals in the photocatalytic reduction of U(VI) by CH-8@NNFO-4 of Example 1 under sunlight irradiation with the addition of isopropyl alcohol (IPA);
[0042] Fig.25 This is the XPS characterization result of the material after the photocatalytic reduction of U(VI) by CH-8@NNFO-4 in Example 1 under sunlight irradiation;
[0043] Fig.26 This is a graph showing the number of cycles of CH-8@NNFO-4 in Example 1 in the photocatalytic reduction of U(VI) under sunlight. DETAILED DESCRIPTION
[0044] Use the following examples to verify the beneficial effects of the present invention:
[0045] Example 1: The preparation method of the full-spectrum responsive photocatalyst of Example 1 is carried out according to the following steps:
[0046] 1. Add 4.0mmol of Fe(NO3)3·9H2O and 8.0mmol of Ca(NO3)2·4H2O into 30mL of deionized water, stir and dissolve to obtain a mixed solution I;
[0047] 2. Add 12 mmol / L NaOH solution to the mixed solution I and ensure that no precipitation is produced, and mix and react for 30 minutes to obtain a mixed solution II.
[0048] 3. Add 1.0mmol of niobium oxide to the mixed solution II and stir for 60min to obtain a mixed solution III; transfer the mixed solution III to a 100mL hydrothermal reactor, place the reactor in a 160℃ constant temperature drying oven and heat for 4h; after the reaction is completed, cool to room temperature, separate the solid phase, wash the solid phase with deionized water 5 times, and then place it in an oven at 80℃ to dry for 6h to obtain a full-spectrum responsive photocatalyst, grind it into powder and seal it for storage. The full-spectrum responsive photocatalyst prepared in this embodiment 1 is recorded as Ca(OH)2@NaNb 1-x Fe x O 3-v , referred to as CH-8@NNFO-4.
[0049] Example 2: The difference between this example and Example 1 is that the amount of Ca(NO3)2·4H2O in step 1 is 0.0 mmol, and the other steps and parameters are the same as those in Example 1. The obtained full-spectrum responsive photocatalyst is recorded as NaNb 1-x Fe x O 3-v , referred to as NNFO-4.
[0050] Example 3: The difference between this example and Example 1 is that the amount of Ca(NO3)2·4H2O in step 1 is 6.0 mmol, and the other steps and parameters are the same as those in Example 1. The obtained full-spectrum responsive photocatalyst is recorded as min-Ca(OH)2@NaNb 1- x Fe x O 3-v , referred to as CH-6@NNFO-4.
[0051] Example 4: The difference between this example and Example 1 is that the amount of Ca(NO3)2·4H2O in step 1 is 10.0 mmol, and the other steps and parameters are the same as those in Example 1. The obtained full-spectrum responsive photocatalyst is recorded as max-Ca(OH)2@NaNb 1- x Fe x O 3-v , referred to as CH-10@NNFO-4.
[0052] Example 5: The difference between this example and Example 1 is that the amount of Ca(NO3)2·4H2O is 8.0mmol, the amount of Fe(NO3)3·9H2O is 0.0mmol, and the other steps and parameters are the same as those in Example 1. The obtained full-spectrum responsive photocatalyst is recorded as Ca(OH)2@NaNbO 3-v , referred to as CH-8@NNO.
[0053] Example 6: The difference between this example and Example 1 is that the amount of Ca(NO3)2·4H2O is 8.0mmol, the amount of Fe(NO3)3·9H2O is 2.0mmol, and the other steps and parameters are the same as those in Example 1. The obtained full-spectrum responsive photocatalyst is recorded as Ca(OH)2@NaNb 1-x Fe x O 3-v -min, referred to as CH-8@NNFO-2.
[0054] Example 7: The difference between this example and Example 1 is that the amount of Ca(NO3)2·4H2O is 8.0mmol, the amount of Fe(NO3)3·9H2O is 6mmol, and the other steps and parameters are the same as those in Example 1. The obtained full-spectrum responsive photocatalyst is recorded as Ca(OH)2@NaNb 1-x Fe x O 3-v -max, referred to as CH-8@NNFO-6.
[0055] Comparative Example 1: This comparative example uses a one-step hydrothermal method to synthesize NaNbO3. The specific preparation steps are as follows:
[0056] 1. Dissolve 0.33 mol NaOH in about 30 mL of deionized water and stir to dissolve to obtain a NaOH solution;
[0057] 2. Add 1.0 mmol of Nb2O5 to the NaOH solution and stir for 60 min to disperse the turbid liquid to obtain a mixed solution;
[0058] 3. Transfer the mixed solution into a 100mL hydrothermal reactor, and place the reactor in a constant temperature drying oven at 160°C for 4 hours. After the reaction is completed, cool to room temperature, separate the solid phase, wash it with deionized water 5 times, and then place it in an oven at 80°C to dry for 6 hours to obtain NaNbO3, referred to as NNO, which is ground into powder and sealed for storage.
[0059] Figure 1 For comparison 1 and the FT-IR images of the full spectrum responsive photocatalysts prepared in Examples 1 to 7, Figure 1 It can be seen that the change of Fe and Ca content in the synthesized photocatalytic material will not affect the crystal form of the material, indicating that the material has good crystallinity.
[0060] Figure 2 The UV diffuse reflectance images of NNO prepared in Comparative Example 1 and the full-spectrum responsive photocatalysts prepared in Examples 1 to 4 are shown in FIG. Figure 3 The UV diffuse reflectance graphs of the full-spectrum responsive photocatalysts prepared by NNO in Comparative Example 1 and Examples 1, 5, 6, and 7 are shown in FIG. Figure 2 and Figure 3 It can be seen that the light absorption band of the single NNO prepared in Comparative Example 1 is around 400nm, that is, it only responds to ultraviolet light, while the light absorption range of CH-8@NNFO-4 prepared in Example 1 extends from the ultraviolet region to the visible light region and the near-infrared region, which is obviously wider than the absorption range of the materials prepared in other examples to sunlight. Figure 4 The UV diffuse reflectance and band gap diagrams of NNO in Comparative Example 1 and the full spectrum responsive photocatalyst in Example 1 are shown in FIG. Figure 4 It can be seen that the band gap width decreases from 2.83 eV of NNO to 0.95 eV of CH-8@NNFO-4, which is beneficial to the utilization of visible light by the material.
[0061] Figure 5 The fluorescence spectra of NNO in Comparative Example 1 and the full-spectrum responsive photocatalysts in Examples 1-4 are shown in FIG. Figure 6 The photoluminescence spectra of NNO in comparative example 1 and the full-spectrum responsive photocatalysts in examples 1, 5, 6, and 7 are shown in FIG. Figure 7 The photoluminescence spectra of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1 are shown in Table 1. Figure 5 to Figure 7 It can be seen that the PL emission peak intensity of NNO alone is the highest, while the PL emission peak of CH-8@NNFO-4 is the lowest among all samples, indicating that the photogenerated electron-hole recombination rate in CH-8@NNFO-4 is low, which is beneficial to enhance the photocatalytic performance.
[0062] Figure 8 The oxygen vacancy test diagram of NNO in comparative example 1 and the full spectrum responsive photocatalyst in examples 1, 4, 5, and 6 is shown in FIG. Figure 8 The electron spin resonance signal of CH-8@NNFO-4 is significantly stronger than that of other materials, indicating that CH-8@NNFO-4 has a higher concentration of oxygen vacancies. Oxygen vacancies are conducive to the effective separation of photogenerated electrons and holes, thereby enhancing the photocatalytic performance.
[0063] Fig. 9 The transient photocurrent diagram of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1 is shown in FIG. Fig. 9 It can be seen that both NNO and CH-8@NNFO-4 can generate photocurrent under visible light irradiation, but the photocurrent generated by CH-8@NNFO-4 is significantly stronger than that of NNO, indicating that CH-8@NNFO-4 has a higher separation efficiency of photogenerated electrons and holes.
[0064] Fig.10 The electrochemical impedance diagram of NNO in comparative example 1 and CH-8@NNFO-4 in example 1 is shown in Fig.10The Nyquist arc radius of CH-8@NNFO-4 is smaller than that of NNO, indicating that the interfacial photogenerated charge transfer resistance in CH-8@NNFO-4 is small, which is conducive to the separation and transfer of photogenerated electrons and holes, and thus beneficial to enhance its photocatalytic activity.
[0065] The morphology and composition of the NNO prepared in Comparative Example 1 and the full-spectrum responsive photocatalysts prepared in Examples 1 to 5 were characterized. Fig.11 The SEM, TEM and EDS images of NNO prepared in Comparative Example 1 are shown in FIG. Fig.12 The SEM, TEM and EDS images of CH-8@NNFO-4 prepared in Example 1; Fig.11 It can be seen that NNO is tetrahedral with a lattice spacing of 0.41nm, corresponding to the (161) face of NNO. It is mainly composed of Na, Nb, O and C, with no other components. Fig.12 It can be seen that CH-8@NNFO-4 is a hexadecahedron with Ca(OH)2 and Ca2FeNbO6 deposited on the surface. The lattice spacing of 0.26 nm corresponds to the Ca(OH)2(012) plane, and the lattice spacing of 0.29 nm corresponds to the Ca2FeNbO6(114) plane.
[0066] Fig.13 FT-IR images of NNO prepared in Comparative Example 1 and CH-8@NNFO-4 prepared in Example 1. Fig.13 It can be seen that in the infrared spectrum of NNO, at 900cm -1 The peak near the bending vibration of Nb-O is 3600cm -1 The OH bond stretching vibration peak appears near the surface, mainly the OH bond in calcium hydroxide (Ca(OH)2), 1000-1200cm -1 The bending vibration peak at is mainly NaNb 1-x Fe x O 3-v Nb-O and O-Fe-O bonds in.
[0067] Fig.14 The XRD spectra of NNO prepared in Comparative Example 1 and CH-8@NNFO-4 in Example 1 are shown in Table 1. Fig.14 It can be seen that compared with the Ca(OH)2 and NNO standard cards, CH-8@NNFO-4 has better crystallinity and the crystal form has not changed.
[0068] Fig.15 The thermal stability diagram of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1 is shown in FIG. Fig.15 It can be seen that CH-8@NNFO-4 has good thermal stability.
[0069] Fig.16 The specific surface area diagram of NNO in Comparative Example 1 and CH-8@NNFO-4 in Example 1 is shown in FIG. Fig.16 It can be seen that the specific surface area of single NNO is 1.8896m 2 / g, while the specific surface area of CH-8@NNFO-4 is 161.6443m 2 / g, which is much larger than that of NNO. The large specific surface area of CH-8@NNFO-4 is beneficial to the adsorption of U(VI).
[0070] Application example 1: Photocatalytic reduction U(VI) performance test:
[0071] In order to evaluate the photocatalytic reduction U(VI) performance of the prepared photocatalytic material, the photocatalytic reduction experiment of U(VI) was carried out on the photocatalytic materials prepared in Comparative Example 1, Example 1 and Implementation 2 under sunlight irradiation without adding any protective agent or sacrificial agent. The specific process is as follows:
[0072] In 50 ml of a solution with a U(VI) concentration of 10 mg / L, a photocatalytic material was added at a solid-liquid ratio of 0.2 g / L, and the pH was adjusted to 4.0. The U(VI) reduction experiment was performed in a dark environment and under sunlight. The photocatalytic reduction effects of NNO in Comparative Example 1, CH-8@NNFO-4 in Example 1 under dark environment and sunlight, and NNFO-4 in Example 2 under sunlight are shown in Figure 2. Fig.17 As shown, from Fig.17 It can be seen that NNO has almost no reduction ability for U(VI) under dark conditions and sunlight conditions, and the photocatalytic reduction ability of NNFO-4 for U(VI) under sunlight is about 40%. Although CH-8@NNFO-4 has good reduction performance for U(VI) under dark conditions, the reaction rate is slow. Under sunlight, CH-8@NNFO-4 has a faster reduction rate for U(VI), and the removal rate reaches more than 93% within 30 minutes. The effect of temperature and time on the photocatalytic reduction of U(VI) by CH-8@NNFO-4 under sunlight in Example 1 is shown in the figure. Fig.18 As shown, from Fig.18 It can be seen that the reduction rate reaction of CH-8@NNFO-4 to U(VI) is not affected by temperature.
[0073] In 50 ml of a solution with a U(VI) concentration of 10 mg / L, CH-8@NNFO-4 in Example 1 was added at a solid-liquid ratio of 0.2 g / L, and the pH was adjusted to 2.0-6.0, and a U(VI) reduction experiment was conducted under sunlight. The effect of pH on the photocatalytic reduction of U(VI) by CH-8@NNFO-4 in Example 1 under sunlight is shown in Figure 2. Fig.19 As shown, from Fig.19 It can be seen that CH-8@NNFO-4 has good acid resistance and has little effect on the photocatalytic reduction of U(VI) performance after pH>3.0.
[0074] In 50 ml of a solution with a U(VI) concentration of 10 mg / L, CH-8@NNFO-4 prepared in Example 1 was added at a solid-liquid ratio of 0.2 g / L, and the pH was adjusted to 4.0. Different anions and cations (Na + , K + , Ca 2+ Mg 2+ 、SO4 2+ 、NO3 - 、F - 、CO3 2- , HA, NOT), and the reduction experiment of U(VI) was carried out under sunlight. 1-x Fe x O 3-v The photocatalytic reduction of U(VI) under sunlight is affected by different anions and cations. Fig. 20 As shown, from Fig. 20 It can be seen that except for F - and CO3 2- Except for the significant influence on the photocatalytic reduction performance, other anions and cations have almost no effect on the photocatalytic reduction of U(VI), indicating that the CH-8@NNFO-4 photocatalytic material has good anti-interference ability to anions and cations.
[0075] Application Example 2: Test on the influence of active species on photocatalytic reduction performance
[0076] In order to verify the active species that play a major role in the photocatalytic reduction process, active species capture research was carried out. In 50ml of a solution with a U(VI) concentration of 10mg / L, CH-8@NNFO-4 prepared in Example 1 was added at a solid-liquid ratio of 0.2g / L, the pH was adjusted to 4.0, and the U(VI) reduction experiment was carried out under sunlight. The other conditions were the same as those in Application Example 1. AgNO3 electron capture agents (e - ), benzoquinone (p-BQ) captures superoxide radicals (·O2 -), methanol (CH3OH) captures holes (h + ) and isopropyl alcohol (IPA) to capture hydroxyl radicals (·OH). - ) conditions, the electron capture results of CH-8@NNFO-4 in Example 1 under sunlight irradiation in the photocatalytic reduction of U(VI) are shown in the figure below. Fig.21 As shown, from Fig.21 It can be seen that the addition of AgNO3 capture agent electrons (e - )The reducing ability of the material to U(VI) decreases with the increase of AgNO3 concentration. When the AgNO3 concentration is 5mmol / L, the material completely loses the ability to reduce U(VI), indicating that photogenerated electrons are the main reducing active species.
[0077] After adding benzoquinone (p-BQ) to capture superoxide radicals (·O2 - ) under the conditions of Example 1, the capture results of superoxide radicals in the photocatalytic reduction of U(VI) by CH-8@NNFO-4 under sunlight are as follows: Fig. 22 As shown, from Fig. 22 It can be seen that the addition of benzoquinone captures superoxide radicals (·O2 - ), the reduction ability of the material to U(VI) gradually decreased, indicating that superoxide radicals are also active species involved in the reduction of U(VI).
[0078] When methanol (CH3OH) is added to capture holes (h + ) under the conditions of Example 1, the hole capture results of the photocatalytic reduction of U(VI) by CH-8@NNFO-4 under sunlight are as follows: Fig.23 As shown, from Fig.23 It can be seen that adding methanol to capture holes (h + ), the reduction rate and reduction ability of the material to U(VI) were effectively promoted, indicating that holes would recombine with electrons, thereby reducing the reduction ability to U(VI).
[0079] The capture results of hydroxyl radicals in U(VI) by photocatalytic reduction of CH-8@NNFO-4 in Example 1 under sunlight irradiation are as follows: Fig.24 As shown, from Fig.24 It can be seen that the addition of isopropanol to capture hydroxyl radicals (·OH) can improve the reduction rate and reduction ability of the material to U(VI). This is mainly because hydroxyl radicals (·OH) will react with holes, reducing the recombination of photogenerated electrons and holes, ensuring that there are enough electrons in the system to reduce U(VI).
[0080] Fig.25The XPS characterization results of the material after the photocatalytic reduction of U(VI) by CH-8@NNFO-4 in Example 1 under sunlight irradiation are shown in Figure 1. Fig.25 It can be seen that most of the U(VI) was reduced to U(IV), and a small amount of U(VI) was present and removed from the wastewater by adsorption.
[0081] Application Example 3: Photocatalytic material recycling performance test
[0082] After the CH-8@NNFO-4 of Example 1 photocatalytically reduces U(VI) under sunlight, it is filtered out, oxidized in air for 24 hours, and then eluted with a 0.1 mol / L NaHCO3 solution to remove UO2 deposited on the photocatalyst. It is then washed with water and dried for recycling performance verification. The results of the recycling times of the CH-8@NNFO-4 of Example 1 in the photocatalytic reduction of U(VI) under sunlight are as follows: Fig.26 As shown, from Fig.26 It can be seen that after 5 cycles, the removal rate of U(VI) is still 88.77%, indicating that the material has good reusability.
Claims
1. A method for preparing a full-spectrum responsive photocatalyst, characterized in that The method proceeds as follows:
1. Add ferric nitrate and calcium nitrate into deionized water at a molar ratio of 1:(0-2.5), stir and dissolve to obtain a mixed solution I; 2. Add NaOH solution dropwise to the mixed solution I and ensure that no precipitation is generated, and mix and react for 20 to 30 minutes to obtain a mixed solution II; 3. Add niobium oxide to the mixed solution II and stir for 50 to 60 minutes to obtain a mixed solution III; transfer the mixed solution III to a hydrothermal reactor, and place the reactor in a constant temperature drying oven at 140 to 180°C for heating reaction for 4 to 6 hours; after the reaction is completed, cool to room temperature, separate the solid phase, and then wash the solid phase with deionized water and dry to obtain a full-spectrum responsive photocatalyst.
2. The method for preparing a full-spectrum responsive photocatalyst according to claim 1, characterized in that: The concentration of ferric nitrate in the mixed solution I described in step 1 is 0.06-0.2 mmol / mL.
3. The method for preparing a full-spectrum responsive photocatalyst according to claim 1, characterized in that: The concentration of NaOH described in step 2 is 12 mol / L.
4. The method for preparing a full-spectrum responsive photocatalyst according to claim 1, characterized in that: The amount of niobium oxide in step 3 and the amount of iron nitrate in step 1 is 1:(0.05-6.0).
5. The method for preparing a full-spectrum responsive photocatalyst according to claim 1, characterized in that: The reaction temperature in step 3 is 160° C. and the reaction time is 4 h.
6. The method for preparing a full-spectrum responsive photocatalyst according to claim 1, characterized in that: The drying temperature described in step 3 is 60-80°C and the drying time is 6-8h.
7. Application of the full-spectrum responsive photocatalyst prepared by the method of claim 1, characterized in that: The application is to use a full-spectrum responsive photocatalyst for the treatment of uranium-containing wastewater, wherein the uranium-containing wastewater contains U(VI).
8. The use of the full-spectrum responsive photocatalyst according to claim 7, characterized in that: The method for treating uranium-containing wastewater using a full-spectrum responsive photocatalyst is as follows: adding the full-spectrum responsive photocatalyst to the uranium-containing wastewater at a concentration of 0.2 to 0.3 g / L, adjusting the pH to 3.0 to 6.0, stirring for 20 to 30 minutes under sunlight, separating the full-spectrum responsive photocatalyst, and completing the treatment of the uranium-containing wastewater.
9. The use of the full-spectrum responsive photocatalyst according to claim 7, characterized in that: The regeneration method of the full-spectrum responsive photocatalyst is: after the full-spectrum responsive photocatalyst adsorbed with uranium is oxidized in the air for 24 to 48 hours, it is eluted with a 0.1 mol / L NaHCO3 solution to remove the UO2 deposited on the photocatalyst, and then washed with water and dried to complete the regeneration of the full-spectrum responsive photocatalyst.