Forging method of eccentric forge piece

By designing the step shaft blank with large middle diameter and small diameter at both ends, the lateral force is used to achieve the forming of eccentric forging, which solves the positioning, misaligned material separation and forming problems in the forming of eccentric forging, and avoids forging Defects and additional tooling investment achieve efficient forming of forgings.

CN119016654AActive Publication Date: 2024-11-26CHINA NAT ERZHONG GRP DEYANG WANHANG DIE FORGING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411371613.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-26
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

There are problems in the forming of eccentric forging parts such as positioning, mismatched material and forming, which are prone to forging defects such as cracks and folding. The prior art requires increasing forging fire and tooling investment, which is poor in economy.

Method used

The step shaft blank with a large middle diameter and small end diameter is adopted. The mold cavity is designed to have an acute angle and angle. The blank is slidingly formed in the mold cavity through lateral force to achieve misalignment and forming, avoiding additional auxiliary workpieces .

Benefits of technology

Without adding auxiliary tooling, the positioning, mismatched material distribution and forming problems of eccentric forgings are solved, and defects such as cracks and folding are avoided, and uniform forming of forgings and metal filling are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016654A_ABST
    Figure CN119016654A_ABST
Patent Text Reader

Abstract

The invention provides a forging method of an eccentric forge piece. The forging method comprises the following steps that A1, a blank is designed, specifically, the blank is designed into a stepped shaft blank with the large middle diameter and the small two-end diameter; a2, mold cavity design, wherein an included angle is formed between an upper mold cavity and a lower mold cavity; a3, forming process; a3.1, the round bar is forged into a stepped shaft blank through the drawing and rolling technology; a3.2, the mold is preheated; the upper die cavity falls down to make contact with the stepped shaft blank for forging; a3.3, an upper mold cavity firstly makes contact with the large-diameter position of the stepped shaft blank; a3.4, an acute angle formed by the upper die cavity and the lower die cavity makes contact with the small-diameter position of the ladder shaft blank, and forge piece staggered material distribution is achieved; and A3.5, the small-diameter blanks at the two ends are subjected to forging forming under the influence of the acute-angle cavity surface and the mold platform resistance. The problems of positioning, wrong material distribution and forming in the eccentric forging forming process are solved, and the forge piece does not have the risks of forging defects such as cracks and folding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of die forging manufacturing, in particular to a forging method for a long strip eccentric forging. Background Art

[0002] Forging of eccentric die forgings, the blank before die forging is usually an eccentric blank formed by free forging or a blank formed with the aid of misaligned tooling; however, the free forging of eccentric blanks is relatively complicated, and improper control can easily lead to forging defects such as cracks and folds; although the use of misaligned tooling to assist in forming can reduce the risk of cracks and folding defects in the blank, it requires an increase in forging times and tooling investment, and is less economical. Summary of the invention

[0003] The technical problem solved by the present invention is to provide a forging method for eccentric forgings, which solves the problems of positioning, misaligned material separation and forming in the forming of eccentric forgings, and the forgings have no risk of forging defects such as cracks and folding.

[0004] The technical solution adopted by the present invention to solve its technical problem is:

[0005] A forging method for an eccentric forging comprises the following steps:

[0006] A1. Billet design: The billet is designed as a stepped shaft billet with a large diameter in the middle and small diameters at both ends;

[0007] A2. Mold cavity design: The mold cavity includes an upper mold cavity and a lower mold cavity, and the upper mold cavity and the lower mold cavity form an angle, which is an acute angle;

[0008] A3. Molding process

[0009] A3.1. Heat the round bar to the forging temperature, and forge the round bar into a stepped shaft blank through the drawing and rolling process;

[0010] A3.2. Preheat the mold and spray the mold release agent evenly on the surface of the mold cavity; heat the stepped shaft blank to the forging temperature, then put the stepped shaft blank into the lower mold cavity, and the upper mold cavity falls down to contact the stepped shaft blank for forging. The stepped shaft blank is deformed under the lateral force F of the mold;

[0011] A3.3. The upper die cavity first contacts the large diameter of the step shaft blank. As the forged step shaft blank deforms, the deformed blank is fixed on the die.

[0012] A3.4. As the mold cavity is pressed, the acute angle formed by the upper mold cavity and the lower mold cavity contacts the small diameter of the ladder shaft blank. The mold cavity presses the small diameter blank to form a lateral force. Under the action of the lateral force, the small diameter blank bends and slides toward the width of the cavity while deforming, until the blank slides to the upper and lower mold platforms, realizing the staggered material separation of the forgings.

[0013] A3.5. As the pressing deformation continues, the small diameter billets at both ends are forged under the influence of the sharp-angle cavity surface and the resistance of the die platform.

[0014] In step A1, the diameter of the stepped shaft blank is a rounded transition greater than R300, and the stepped shaft blank is a multi-step shaft blank structure.

[0015] In step A2, the acute angle is 15-40°, the mold cavity is wide on the left and narrow on the right, the acute angle is on the right side of the mold cavity, and the starting position of the acute angle slope is ≥ 30 mm from the center of the cavity width.

[0016] In step A3.1, the forging temperature is 30-50°C, and the stepped shaft blank is polished to clean the oxide scale and wrinkles on the surface of the blank.

[0017] In step A3.2, the mold preheating temperature is 200-350°C, and the upper mold cavity drop forging speed is 2-10 mm / s.

[0018] In step A3.2, the lateral force F is perpendicular to the mold cavity surface, and the lateral force F is decomposed into a horizontal force F 水平 and the vertical force F 竖直 , the step shaft blank is at F 水平 Under the action of F 竖直 Under the action of , forming and widening are achieved.

[0019] The beneficial effects of the present invention are:

[0020] 1. By using a stepped shaft blank with a circular cross-section and a mold structure with an acute angle plane, without adding additional auxiliary tooling, a simple stepped shaft blank is used to solve the problems of positioning, mis-material separation, and forming in the forming of eccentric forgings, and there is no risk of forging defects such as cracks and folding in the forgings.

[0021] 2. By generating the lateral force F, the middle position of the blank is pressed and fixed by the mold cavity. Under the action of the lateral force F, the two ends of the small diameter of the blank slide toward the width of the cavity to achieve the misalignment and separation of the forgings. At the same time, during the pressing process of the forgings, the inclined upper and lower surfaces act as bridges, which helps the metal continue to flow to one side and facilitates the filling of the forgings. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a schematic diagram of an eccentric forging;

[0023] Figure 2 This is a schematic diagram of a step shaft blank;

[0024] Figure 3 is a schematic diagram of a mold profile with an acute angle;

[0025] Figure 4 for Figure 3 Schematic diagram of the enlarged angle between the upper and lower model surfaces;

[0026] Figure 5 Schematic diagram of the contact between the upper and lower dies and the blank during the pressing process;

[0027] Figure 6 for Figure 5 Schematic diagram of the cross-section structure at point A:

[0028] Figure 7 It is a schematic diagram of the force on the blank under the action of the mold surface with an acute angle;

[0029] Figure 8 is the exploded diagram of the lateral force F;

[0030] Fig. 9 It is a schematic diagram of the structure in which the upper die cavity first contacts the large diameter in the middle of the blank;

[0031] Fig.10 for Fig. 9 Transverse cross-section of

[0032] Fig.11 It is a schematic diagram of bending and sliding forming of small diameter blank;

[0033] Fig.12 This is the final forming diagram of the forging;

[0034] Fig.13 This is the analysis diagram of the deformation temperature field and strain field of the forging;

[0035] Fig.14 A side view of the mold cavity.

[0036] As shown in the figure: 1-upper die; 2-lower die; 3-angle. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0038] Example 1

[0039] like Figure 1As shown in the figure, the die structure of the eccentric die forging and the stepped shaft blank with a circular cross section, the die is divided into an upper die 1 and a lower die 2, the upper die 1 has an upper die cavity, the lower die 2 has a lower die cavity, the upper and lower die cavities in the die structure are designed with an acute angle 3, the surface of the upper and lower die cavities are deflected from the vicinity of the width center of the forging to one side of the forging according to the eccentric structure of the forging, and the angle 3 between the upper and lower mold surfaces is between 15 and 40 degrees; the circular cross-section blank is a stepped shaft with a large diameter in the middle and small diameters at both ends. When die forging, the blank is placed in the die cavity, and the blank diameter is large in the middle and small at both ends. The upper and lower mold cavities first contact the large diameter in the middle of the billet during the pressing process. As the pressing progresses, the small diameters at both ends of the billet contact the upper and lower mold surfaces with acute angles. The inclined upper and lower mold surfaces generate lateral forces on the circular billet. The middle position of the billet is pressed and fixed by the mold cavity. Under the lateral force, the two ends of the small diameter of the billet slide to the side of the cavity width to achieve the misalignment and separation of the forgings. At the same time, during the pressing process of the forgings, the inclined upper and lower mold surfaces act as bridges, which help the metal to continue to flow to one side and facilitate the forgings to be filled.

[0040] A forging method for an eccentric forging comprises the following steps:

[0041] A1. Figures 2 to 4 As shown in the figure, the blank design: before die forging, the blank is designed as a stepped shaft blank with a large diameter in the middle and small diameters at both ends. The diameter of the blank is determined according to the cross-sectional size of the forging. According to the actual size of the forging, the blank can be designed as a rough blank of a multi-step shaft;

[0042] The diameter size is determined by the size of the forging, and the larger diameter is 20mm larger than the smaller diameter.

[0043] For example, if the large diameter is Φ400mm and the small diameter is Φ300mm, the single-side drop between the large diameter and the small diameter is 50mm.

[0044] A2. Figures 5 to 6 As shown, the mold cavity design: the mold cavity includes an upper mold cavity and a lower mold cavity, and the upper mold cavity and the lower mold cavity form an angle, and the angle is an acute angle;

[0045] Cavity transition design: The small angle head end is designed with a platform that is equal to or slightly higher than the bridge, which plays the role of a bridge during the forming process and helps the forming of forgings;

[0046] A3. Forming process. The forming process is explained by taking TA15 titanium alloy forgings as an example. β is the phase transition temperature of titanium alloy;

[0047] A3.1. Heat the round bar to the forging temperature, and forge the round bar into a stepped shaft blank through the drawing and rolling process;

[0048] A3.2. Preheat the mold and spray the mold release agent evenly on the surface of the mold cavity; heat the stepped shaft blank to the forging temperature, then put the stepped shaft blank into the lower mold cavity, and the upper mold cavity falls down to contact the stepped shaft blank for forging. The stepped shaft blank deforms under the lateral force F of the mold, and the deformation is as follows: Figures 9 to 10 As shown;

[0049] A3.3, if Fig.11 As shown, the upper die cavity first contacts the large diameter of the step shaft blank, and as the forged step shaft blank is deformed, the deformed blank is fixed on the die;

[0050] A3.4. As the mold cavity is pressed, the acute angle formed by the upper mold cavity and the lower mold cavity contacts the small diameter of the ladder shaft blank. The mold cavity presses the small diameter blank to form a lateral force. Under the action of the lateral force, the small diameter blank bends and slides toward the width of the cavity while deforming, until the blank slides to the upper and lower mold platforms, realizing the staggered material separation of the forgings.

[0051] A3.5, if Fig.12 As shown in Figure 2, as the pressing deformation continues, the small-diameter billets at both ends are finally formed under the influence of the sharp-angle cavity surface and the resistance of the die platform, as shown in Figure 2. Fig.13 As shown, the forgings are deformed evenly, the temperature is controllable, and the equivalent strain is 0.25 to 0.5.

[0052] In step A1, the diameter of the stepped shaft blank is a rounded transition greater than R300, and the stepped shaft blank is a multi-step shaft blank structure.

[0053] In step A2, the acute angle is 15-40°, the mold cavity is wide on the left and narrow on the right, and the acute angle is on the right side of the mold cavity. Fig.14 As shown, the starting position of the acute angle slope is ≥ 30 mm from the center of the cavity width.

[0054] In step A3.1, the forging temperature is 30-50°C, and the stepped shaft blank is polished to clean the oxide scale and wrinkles on the surface of the blank.

[0055] The dual-state structure of the two-phase region of the forging is ensured at a forging temperature of 30-50°C while maintaining a high forging temperature, which is beneficial to the forming of the forging.

[0056] In step A3.2, the mold preheating temperature is 200-350°C, and the upper mold cavity drop forging speed is 2-10 mm / s.

[0057] The preheating temperature of 200-350℃ is used to fully preheat the mold to avoid rapid temperature drop when the forging contacts the mold cavity, which may cause cracking on the forging surface. The forging speed of 2-10mm / s is used to ensure the forming of the forging, while avoiding the influence of forging heat return caused by deformation on the microstructure and properties of the forging.

[0058] In step A3.2, if Figures 7 to 8 As shown, the lateral force F is perpendicular to the mold cavity surface, and the lateral force F is decomposed into a horizontal force F 水平 and the vertical force F 竖直 , the step shaft blank is at F 水平 Under the action of F 竖直 Under the action of , forming and widening are achieved.

[0059] The forming force range of F is 0-800MN. According to the decomposition of horizontal and vertical forces, F 水平 =F*cosα,F 竖直 =sinα.

[0060] By adopting a stepped shaft blank with a circular cross-section and a mold structure with a sharp-angled plane, without adding any additional auxiliary tooling, a simple stepped shaft blank is used to solve the problems of positioning, mis-material separation, and forming in the forming of eccentric forgings, and there is no risk of forging defects such as cracks and folding in the forgings.

[0061] By generating a lateral force F, the middle position of the blank is pressed and fixed by the mold cavity. Under the action of the lateral force F, the two ends of the small diameter of the blank slide toward the width of the cavity to achieve material separation of the forgings. At the same time, during the pressing process of the forgings, the inclined upper and lower surfaces act as bridges, which helps the metal continue to flow to one side and facilitates the filling of the forgings.

[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A forging method for an eccentric forging, characterized in that: The following steps are involved: A1. Billet design: The billet is designed as a stepped shaft billet with a large diameter in the middle and small diameters at both ends; A2. Mold cavity design: The mold cavity includes an upper mold cavity and a lower mold cavity, and the upper mold cavity and the lower mold cavity form an angle, which is an acute angle; A3. Molding process A3.

1. Heat the round bar to the forging temperature, and forge the round bar into a stepped shaft blank through the drawing and rolling process; A3.

2. Preheat the mold and spray the mold release agent evenly on the surface of the mold cavity; heat the stepped shaft blank to the forging temperature, then put the stepped shaft blank into the lower mold cavity, and the upper mold cavity falls down to contact the stepped shaft blank for forging. The stepped shaft blank is deformed under the lateral force F of the mold; A3.

3. The upper die cavity first contacts the large diameter of the step shaft blank. As the forged step shaft blank deforms, the deformed blank is fixed on the die. A3.

4. As the mold cavity is pressed, the acute angle formed by the upper mold cavity and the lower mold cavity contacts the small diameter of the ladder shaft blank. The mold cavity presses the small diameter blank to form a lateral force. Under the action of the lateral force, the small diameter blank bends and slides toward the width of the cavity while deforming, until the blank slides to the upper and lower mold platforms, realizing the staggered material separation of the forgings. A3.

5. As the pressing deformation continues, the small diameter billets at both ends are forged under the influence of the sharp-angle cavity surface and the resistance of the die platform.

2. The forging method of an eccentric forging according to claim 1, characterized in that: In step A1, the diameter of the stepped shaft blank is a rounded transition greater than R300, and the stepped shaft blank is a multi-step shaft blank structure.

3. The forging method of an eccentric forging according to claim 1, characterized in that: In step A2, the acute angle is 15-40°, the mold cavity is wide on the left and narrow on the right, the acute angle is on the right side of the mold cavity, and the starting position of the acute angle slope is ≥ 30 mm from the center of the cavity width.

4. The forging method of an eccentric forging according to claim 1, characterized in that: In step A3.1, the forging temperature is 30-50°C, and the stepped shaft blank is polished to clean the oxide scale and wrinkles on the surface of the blank. The forging method of an eccentric forging as described in claim 1 is characterized in that: in step A3.2, the mold preheating temperature is 200-350°C, and the drop forging speed of the upper mold cavity is 2-10mm / s.

5. The forging method of an eccentric forging according to claim 1, characterized in that: In step A3.2, the lateral force F is perpendicular to the mold cavity surface, and the lateral force F is decomposed into a horizontal force F 水平 and the vertical force F 竖直 , the step shaft blank is at F 水平 Under the action of F 竖直 Under the action of , forming and widening are achieved.

Citation Information

Patent Citations

  • Oval integrally-forged eccentric gas-lift mandrel for oil and gas field

    CN202531124U

  • Finishing forging die of eccentric shaft and forging and pressing die comprising finishing forging die

    CN217647414U

  • Eccentric shaft pre-forging die capable of conveniently utilizing waste heat for finish forging

    CN218192357U

  • Method of forging heavy articles

    EP0059038A2

  • Manufacturing method of eccentric shaft for compressor by automatic cold forging process

    KR1020160147327A