Manufacturing method of artificial steel microcracks

Through pressure control of the steel surface cutting and bending tester, the microcracks on the steel surface are simulated, and the problem of large differences between artificial microcracks and real microcracks in the prior art is solved, and more appropriate microcrack morphology and expansion characteristics are achieved. Better research ideas.

CN119017025AActive Publication Date: 2024-11-26ZENITH STEEL GROUP CORP CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411370702.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-26
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

In the prior art, the method of artificially producing microcracks on the surface of steel cannot accurately simulate real microcracks, making it difficult to determine the real cause of microcracks. The obtained artificial microcracks are quite different from real microcracks and cannot be effectively used in steel products. Research on surface quality and mechanical properties.

Method used

By selecting the steel continuous casting billet, cutting and sampling, and opening grooves on the columnar crystal sample, applying pressure and reverse compression using a bending tester, the opening and expansion of cracks are controlled, ensuring that the opening of artificial microcracks is less than 100μm, and simulation The morphology and expansion characteristics of real microcracks.

Benefits of technology

The opening of artificial microcracks is less than 100μm, and the expansion is smaller internal cracks, which is more in line with the microcrack morphology of the real formed on the steel surface, providing better research ideas for the source and control of microcracks on the surface of steel products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017025A_ABST
    Figure CN119017025A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of manufacturing of artificial steel microcracks, in particular to a manufacturing method of artificial steel microcracks. According to a conventional method for artificially manufacturing micro-cracks on the surface of steel, the obtained artificial micro-cracks are greatly different from real micro-cracks on the surface of a steel product, and it is difficult to know the real cause of the micro-cracks of the steel product by comparing the artificial micro-cracks with the real micro-cracks on the surface of the steel product. In order to solve the problems, the manufacturing method of the artificial steel microcrack is provided, cutting sampling is conducted on a columnar crystal area of a steel continuous casting billet, fracturing and reverse pressing are conducted, the opening of the obtained artificial microcrack is smaller than 100 micrometers, finer internal cracks are expanded, the artificial microcrack better fits the shape of the microcrack actually formed on the surface of the steel, and therefore the artificial steel microcrack is obtained. And a better research thought is provided for the source and control scheme of the steel product surface microcracks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of artificial steel microcrack production, and in particular to a method for producing artificial steel microcracks. Background Art

[0002] The production process of steel products includes continuous casting of molten steel, heating of ingots, rolling and other links. After the steel solidifies, surface cracks will appear on its surface due to various reasons (such as inappropriate mold protection slag, poor secondary cooling, excessive straightening force, inappropriate billet heating temperature, rolling scratches, etc.). Steel products with surface cracks will not disappear in the subsequent series of processing processes such as forging, extrusion, and drawing, which will cause great harm to the surface quality, service life, mechanical properties and other aspects of the final steel products. Therefore, it is very necessary to control the surface cracks of steel products.

[0003] In order to better control the surface cracks of steel products, we must first study how the surface cracks are generated and at what stage they start to form. At present, the research on the origin of microcracks on the surface of steel is usually based on production experience to observe the morphology of microcracks on the surface of the product, and roughly infer the cause of microcracks based on the degree of decarburization around the microcracks. However, this method often leads to misjudgment and cannot quickly and accurately solve the problem.

[0004] To know at which stage of steel product production the microcracks appear, a more detailed analysis and judgment is needed. The microcracks generated in steel at different production stages are simulated, and the artificial crack samples are cast under the same casting process conditions. After the casting process is completed, the surface crack morphology of the final steel product is carefully compared, and it is easy to know at which production stage the microcracks on the surface of the steel product are generated. This method can significantly reduce the misjudgment of the cause of microcracks and provide the most basic theoretical guidance for the origin of microcracks on the surface of steel products.

[0005] At present, the conventional method of artificially creating microcracks on the surface of steel is to use a wire cutting machine or a cutting machine to cut out crack-like defects on the surface of steel. Although this method is simple, it has many problems, such as large crack opening (wire cutting is usually greater than 400μm, while real cracks are usually less than 100μm), too straight cracks, no further crack expansion, and thus no smaller internal cracks can be obtained. The artificial microcracks obtained by the above conventional method are quite different from the real microcracks on the surface of steel products. It is difficult to learn the real cause of the microcracks on the surface of steel products by comparing with the real microcracks on the surface of steel products. Summary of the invention

[0006] The problem in the prior art is that the conventional method of artificially creating microcracks on the surface of steel products has a large difference between the artificial microcracks obtained and the real microcracks on the surface of steel products, and it is difficult to find out the real cause of the microcracks in steel products by comparing them with the real microcracks on the surface of steel products. In view of the above problem, the present invention provides a method for making artificial steel microcracks, which comprises the following steps:

[0007] (1) Selecting steel continuous casting billets;

[0008] (2) cutting and sampling in the columnar crystal region of the steel continuous casting billet to obtain a plurality of rectangular columnar crystal specimen strips;

[0009] (3) The columnar crystal sample strip has two faces perpendicular to the growth direction of the columnar crystals. A groove is cut on one of the two faces. The face with the groove is recorded as face a, and the other face is recorded as face b (face b is parallel to face a). The length of the groove is equal to the width of face a, and the axis of the groove is parallel to the side length of face a in the width direction.

[0010] (4) Place the columnar crystal sample strip horizontally on the experimental platform, with the a side facing downward and the b side facing upward, and apply a vertical downward force to the b side for fracturing;

[0011] (5) The columnar crystal specimen strip is rotated 90° along the a-plane, and a vertical downward force is applied to the b-plane again for reverse pressing.

[0012] Preferably, the steel continuous casting billet is a square billet or a rectangular billet. In a square billet or a rectangular billet, the columnar crystals are relatively located in horizontal and vertical positions. If it is a circular billet, the columnar crystals are distributed along the radial direction of the circle. When cutting a long strip of a columnar crystal sample, it is easy to cause cracks to extend along the radial direction of the columnar crystals, and it is easy to obtain skew cracks.

[0013] Preferably, the cross-sectional size of the steel continuous casting billet is ≥100×100 mm.

[0014] Preferably, the thickness, width and length of the columnar crystal sample strip are 10-15mm, 10-15mm and 100-150mm respectively. The size of the columnar crystal sample strip is more convenient for the subsequent bending test machine to perform fracturing experiments. When the thickness and width of the columnar crystal sample strip are less than 10mm, the crack extension can easily penetrate the sample, and the sample can be easily burned during the subsequent high-temperature heating process, causing the test failure; when the thickness and width of the columnar crystal sample strip are greater than 15mm, the sample is wasted a lot, and it is too large to be convenient for processing; when the length of the columnar crystal sample strip is less than 100mm, it cannot be placed at both ends of the bending machine pad; when the length of the columnar crystal sample strip is greater than 150mm, the sample is wasted a lot, and it is too large to be convenient for processing. The shape of the columnar crystal sample strip is a regular rectangular parallelepiped, so that the obtained artificial microcracks are convenient for sample preparation and analysis directly in the direction perpendicular to the crack. If the shape of the columnar crystal sample strip is cylindrical or other irregular shapes, it will not only affect the production of cracks, but also require further cutting and processing for subsequent sample observation.

[0015] Preferably, the depth of the groove is 0.5-1mm. The purpose of wire cutting grooving is to prefabricate an artificial defect on the a-plane of the columnar crystal sample strip, so that the crack can expand along the largest surface defect (i.e., the defect of the cutting machine grooving) during the bending process of the bending machine; the control of the grooving depth is to control the expansion depth of the crack; when the grooving depth is less than 0.5mm, it is not conducive to the expansion of the crack, and the sample may not crack immediately and bend, and then the sample breaks; when the grooving depth is greater than 1mm, after the sample is fracturing and reverse pressing, the crack obtained does not fit the morphology of the actual microcracks, and the subsequent test process cannot accurately simulate the changes in the microscopic morphology of the surface cracks of the real microcracks on the steel surface during the subsequent processing, such as decarburization behavior, oxidation behavior, etc., and the grooving is too deep, which can easily cause the expansion crack to penetrate the sample, resulting in sample fracture. Therefore, the optimal depth of wire cutting grooving is 0.5mm-1mm.

[0016] Preferably, during fracturing, the vertical downward pressure is applied by the bending arm of the bending tester, the pressure is 150-180KN, and the pressing displacement is 0.2-0.5mm. Combined with the sample size selection machine equipment capacity, when the bending tester pressure is less than 150KN, it will cause the pressing displacement to be less than 0.2mm, resulting in too small cracks in the sample; and when the pressure is greater than 180KN, it is easy to cause the pressing displacement to be greater than 0.5mm, resulting in brittle fracture of the sample and inability to control the depth of the crack. Therefore, the optimal pressure is 150KN-180KN, and the pressing displacement is 0.2-0.5mm.

[0017] Preferably, during reverse pressing, the vertical downward pressure is applied by the bending arm of the bending tester, the pressure is 200-250KN, and the pressing displacement is 0.3-0.6mm. Reverse pressing is mainly used to tighten the wide cracks that have expanded and control the crack gap to meet the actual crack width. When the pressure is less than 200KN and the combined pressing displacement is less than 0.3mm, the requirement of crack opening less than 100μm cannot be guaranteed; when the pressure is greater than 250KN and the combined pressing displacement is greater than 0.6mm, the sample is easily pressed into a dent, and bulging deformation occurs on both sides of the sample, and it is easy to cause the crack to produce secondary expansion cracks along the vertical direction of the main crack, resulting in a significant change in the overall morphology of the crack.

[0018] The present invention has the following beneficial effects:

[0019] The artificial microcracks obtained by the method of the present invention have an opening less than 100 μm and extend with smaller internal cracks, which are more consistent with the microcrack morphology actually formed on the surface of steel materials, and provide better research ideas for the sources and control solutions of microcracks on the surface of steel products. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 : Schematic diagram of the process of making artificial microcracks according to Example 1 of the present invention.

[0021] Figure 2 : Artificial microcracks obtained on the steel surface in Example 1.

[0022] Figure 3 : Artificial microcracks obtained on the steel surface in Comparative Example 1.

[0023] Figure 4 : Artificial microcracks obtained on the steel surface in Comparative Example 2.

[0024] Figure 5 : Artificial microcracks obtained on the steel surface in Comparative Example 3.

[0025] Figure 6 : Artificial microcracks obtained on the steel surface in Comparative Example 4.

[0026] Figure 7 : Artificial microcracks obtained on the steel surface in Comparative Example 5.

[0027] Figure 8 : Artificial microcracks obtained on the steel surface in Comparative Example 6.

[0028] Fig. 9 : Artificial microcracks obtained on the steel surface in Comparative Example 7.

[0029] Fig.10 : Artificial microcracks obtained on the steel surface in Comparative Example 8.

[0030] Fig.11: Artificial microcracks obtained on the steel surface in Comparative Example 9. DETAILED DESCRIPTION

[0031] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0032] Example 1

[0033] Take 40Cr steel as an example to make artificial micro cracks. The method of making artificial steel micro cracks is as follows:

[0034] (1) The cross-sectional dimensions of the 40Cr steel billet are 140 × 140 mm. At a distance of 35 mm from the surface of the billet (just in the columnar crystal area, the growth direction of the columnar crystal is as shown in the specification Figure 1 As shown, along the four sides of the cross section of the steel billet pointing to the inside of the cross section, the growth direction of the columnar crystal is perpendicular to the axis of the extension direction of the steel billet), and downwardly cut along the horizontal direction perpendicular to the end face of the steel billet to obtain a steel sheet with a thickness of d=11mm, and then the obtained steel sheet is divided into a number of columnar crystal sample strips along its width direction, and each columnar crystal sample strip is a cuboid with a thickness, width, and length of 11mm, 11mm, and 140mm respectively;

[0035] (2) Take a long strip of columnar crystal sample, which has two faces perpendicular to the growth direction of the columnar crystals. A groove is cut on one of the faces. The face with the groove is recorded as face a, and the other face is recorded as face b. The length of the groove is equal to the width of face a, the axis of the groove is parallel to the side length of face a in the width direction, and the depth of the groove is 0.6 mm;

[0036] (3) placing the columnar crystal sample strip obtained in step (2) horizontally on the experimental platform, with the a side facing downward and the b side facing upward, and applying a vertical downward force on the b side using a bending tester for fracturing, the pressure is 160 kN, and the downward displacement is controlled to be 0.3 mm;

[0037] (4) The columnar crystal sample strip was rotated 90° clockwise along the a surface, and a bending test machine was used to apply a vertical downward force on the b surface for reverse pressing. The pressure was 220 kN, and the pressing displacement was controlled to be 0.5 mm.

[0038] Example 1 The microcracks obtained on the steel surface are as shown in the attached specification. Figure 2 As shown, the opening width of the microcrack is 56 μm, and it extends with finer internal cracks.

[0039] Comparative Example 1 is the same as Example 1, except that in Comparative Example 1, a steel sheet with a thickness of d = 11 mm is obtained by cutting downward in a horizontal direction perpendicular to the end face of the steel billet at a position 70 mm away from the surface of the steel billet. The microcracks on the surface of the steel obtained in Comparative Example 1 are shown in the attached manual. Figure 3 The image shows that the crack opening width of Comparative Example 1 is 63 μm, but the crack is a non-vertical oblique crack, which is not convenient for studying the characteristics of the crack at different depths and interferes with the subsequent high-temperature oxidation treatment.

[0040] Comparative Example 2 is the same as Example 1, except that no grooves are provided on the surface of the columnar crystal sample strip in Comparative Example 2. In order to press cracks out of the sample, a pressure of 300KN is required to be set and the displacement is pressed down. The morphology of the steel surface obtained in Comparative Example 2 is shown in the attached manual. Figure 4 As shown in the image, the crack opening width is 68μm, and the crack is also a vertical crack, but the crack runs through the entire sample. Subsequent tests have the problem of high-temperature oxidation at both ends at the same time, which not only interferes with the test results, but also makes the sample very easy to break.

[0041] Comparative Example 3 is the same as Example 1, except that the depth of the groove on the a-side of the columnar crystal sample strip in Comparative Example 3 is 5 mm. The microcracks on the surface of the steel obtained in Comparative Example 3 are shown in the attached manual. Figure 5 The image shows that the crack opening width is 59μm, and the crack is also a vertical crack, but the crack runs through the entire specimen. Subsequent tests have the problem of high-temperature oxidation at both ends at the same time, which not only interferes with the test results, but also makes the specimen very easy to break.

[0042] Comparative Example 5 is the same as Example 1, except that the pressure in step (3) of Comparative Example 5 is 100 KN and the pressing displacement is 0.1 mm. The microcracks on the surface of the steel obtained in Comparative Example 5 are shown in the attached specification. Figure 6 The image shows that the crack opening width is 70 μm and the crack is also vertical, but the crack depth is too shallow to study the morphological changes of the crack at different depths in the entire crack extension direction.

[0043] Comparative Example 6 is the same as Example 1, except that the pressure in step (3) of Comparative Example 6 is 200 KN and the pressing displacement is 0.7 mm. The microcracks on the surface of the steel obtained in Comparative Example 6 are shown in the attached specification. Figure 7 The image shows that the crack opening width is 66μm and the crack is also vertical, but the crack runs through the entire specimen. Subsequent tests have the problem of high-temperature oxidation at both ends at the same time, which not only interferes with the test results, but also makes the specimen very easy to break.

[0044] Comparative Example 7 is the same as Example 1, except that the pressure in step (4) of Comparative Example 7 is 160 KN and the displacement is 0.25 mm. The microcracks on the surface of the steel obtained in Comparative Example 7 are shown in the attached specification. Figure 8 The image shows that the crack opening width is 231μm, which does not conform to the typical characteristic of an actual crack of ≤100μm. In subsequent high-temperature oxidation tests, the crack opening is prone to severe oxidation due to the large opening, and cannot be compared with the actual situation.

[0045] Comparative Example 8 is the same as Example 1, except that the pressure in step (4) of Comparative Example 8 is 300 KN and the displacement is 0.8 mm. The microcracks on the surface of the steel obtained in Comparative Example 8 are shown in the attached specification. Fig. 9 The image shows that the crack opening width is 89 μm, but there are branch cracks near the main trunk of the vertical crack, which is not convenient for single factor analysis of the crack morphology characteristics in the subsequent high temperature oxidation test.

[0046] Comparative Example 9 is the same as Example 1, except that the reverse pressing in step (4) is not performed in Comparative Example 9. The microcracks on the surface of the steel obtained in Comparative Example 9 are shown in the attached specification. Fig.10 The image shows that the crack opening width is 731μm, which does not meet the typical characteristics of an actual crack of ≤100μm. In the subsequent high-temperature oxidation test, the crack opening will be too severely oxidized due to the large opening, and it is impossible to compare with the actual situation. Therefore, the result of the artificial prefabricated crack is not good.

[0047] Comparative Example 10

[0048] (1) The cross-sectional dimensions of the 40Cr steel billet are 140×140 mm. At a position 35 mm away from the surface of the billet, a steel sheet with a thickness of d=11 mm is cut downward in a horizontal direction perpendicular to the end face of the billet. The obtained steel sheet is then divided into a number of columnar crystal sample strips along its width direction. Each columnar crystal sample strip is a cuboid with a thickness of 11 mm, a width of 11 mm, and a length of 140 mm, respectively.

[0049] (2) Take a long strip of columnar crystal sample, which has two faces perpendicular to the growth direction of the columnar crystals. A groove is cut on one of the faces. The face with the groove is recorded as face a, and the other face is recorded as face b. The length of the groove is equal to the width of face a, the axis of the groove is parallel to the side length of face a in the width direction, and the depth of the groove is 8 mm. The microcracks on the surface of the steel obtained in Comparative Example 10 are as shown in the attached manual. Fig.11 The image shows that the opening is 436 μm, which does not have the typical characteristics of a crack.

[0050] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for producing artificial steel microcracks, characterized in that: The following steps are involved: (1) Selecting steel continuous casting billets; (2) cutting and sampling in the columnar crystal region of the steel continuous casting billet to obtain a plurality of rectangular columnar crystal specimen strips; (3) The columnar crystal sample strip has two faces perpendicular to the growth direction of the columnar crystals. A groove is provided on one of the faces. The face with the groove is recorded as face a, and the other face is recorded as face b. The length of the groove is equal to the width of face a, and the axis of the groove is parallel to the side length of face a in the width direction. (4) Place the columnar crystal sample strip horizontally on the experimental platform, with the a side facing downward and the b side facing upward, and apply a vertical downward force to the b side for fracturing; (5) The columnar crystal specimen strip is rotated 90° along the a-plane, and a vertical downward force is applied to the b-plane again for reverse pressing.

2. The method for producing artificial steel microcracks according to claim 1, characterized in that: The continuous casting billet of steel is square billet or rectangular billet.

3. The method for producing artificial steel microcracks according to claim 1, characterized in that: The cross-sectional dimensions of the steel continuous casting ingot shall be ≥100×100mm.

4. The method for producing artificial steel microcracks according to claim 1, characterized in that: The thickness, width and length of the columnar crystal sample strip are 10-15mm, 10-15mm and 100-150mm respectively.

5. The method for producing artificial steel microcracks according to claim 1, characterized in that: The depth of the groove is 0.5-1 mm.

6. The method for producing artificial steel microcracks according to claim 1, characterized in that: During fracturing, pressure is applied vertically downward on the b surface, the pressure is 150-180KN, and the downward displacement is 0.2-0.5mm.

7. The method for producing artificial steel microcracks according to claim 1, characterized in that: During reverse pressing, pressure is applied vertically downward on surface b, the pressure is 200-250KN, and the pressing displacement is 0.3-0.6mm.

Citation Information

Patent Citations

  • Preparation method of metal material plate-shaped fatigue specimen with penetrated short cracks

    CN109142000A

  • Manufacturing method of internal crack defect testing plate for non-destructive testing teaching

    CN111195807A

  • Isometric crystal formation control process for furnace roll manufacturing

    CN113414356A

  • Method for preparing sample with surface cracks

    CN113514291A

  • Method for characterizing fracture toughness of PBX explosive for prefabricating superfine cracks based on femtosecond laser

    CN118706633A