Method for improving morphology and crystallinity of titanium-doped iron phosphate crystal grains through hydrothermal method

The introduction of titanium doped elements under high temperature and high pressure conditions by hydrothermal method has solved the problem of orderly damage to the crystal structure and low utilization rate of doped elements in doped lithium iron phosphate batteries, and improved the crystallinity of iron phosphate and iron phosphate. Improve battery performance.

CN119018867APending Publication Date: 2024-11-26ZHEJIANG YOUSHAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411428032.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, in the doped lithium iron phosphate battery, the introduction of doped elements leads to orderly damage of the crystal structure, small grains, low iron-phosphorus ratio and low utilization rate of doped elements, affecting the battery performance.

Method used

The hydrothermal method is used to introduce titanium doped elements during the conversion of ammonium ferric phosphate through high-temperature and high-pressure environment, which increases the conversion temperature and pressure, promotes the crystallinity and iron-phosphorus ratio of iron phosphate, and increases the grain size and utilization rate of doped elements. .

Benefits of technology

The high-iron-phosphorus ratio, high crystallinity and high incorporation rate of iron phosphate are achieved, and the electrochemical performance and battery performance of lithium iron phosphate batteries are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018867A_ABST
    Figure CN119018867A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving morphology and crystallinity of titanium-doped iron phosphate crystal grains through a hydrothermal method. The method comprises the following steps: S1, preparing raw materials: preparing an ammonium phosphate solution, a phosphoric acid solution, a titanium dioxide ferrous solution and hydrogen peroxide for later use; s2, synthesizing: adding an ammonium phosphate solution, a titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, and reacting to obtain slurry; carrying out suction filtration and washing on the slurry to obtain a yellow primary washing filter cake; s3, conversion: taking 2.5-3.5 kg of the yellow first-washing filter cake, adding 8.0-12.0 kg of water, 200-800 g of a phosphoric acid solution and 120-180 g of titanium sulfate, pulping and stirring uniformly, and performing suction filtration and washing to obtain a light pink second-washing filter cake; s4, calcining: drying the light pink secondary washing filter cake to obtain iron phosphate dihydrate, and calcining and crushing the iron phosphate dihydrate to obtain a finished product of iron phosphate; the iron phosphate prepared by the hydrothermal method is high in crystallinity, high in iron-phosphorus ratio and high in titanium doping rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of batteries, and in particular to a method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method. Background Art

[0002] Compared with ternary batteries, the rate performance of lithium iron phosphate batteries has always been a shortcoming. Element doping can improve the lithium ion diffusion channel and increase the discharge current. Doping is the introduction of impurity elements into the crystal structure of lithium iron phosphate, which will directly affect the crystallinity of lithium iron phosphate and cause the final electrical performance of the battery to be damaged. Therefore, how to ensure the crystallinity of the material while introducing doping elements is a difficult problem that materials workers have been working hard to overcome in recent years.

[0003] As a precursor of lithium iron phosphate, various indicators of iron phosphate will directly affect the final battery performance. The preparation of doped lithium iron phosphate can start with doping iron phosphate. The conventional iron phosphate preparation process can be divided into two stages, namely the synthesis stage of raw material mixing and the conversion stage of temperature-increasing phase change. Wet doping can mix doping salts into the raw materials, such as ferrous sulfate solution, monoammonium phosphate solution, or as a separate additive in the synthesis stage or conversion stage. This method is simple to operate, has low equipment requirements and low cost.

[0004] The conventional doping process is to mix the doping salt with other raw materials or add it as an additive to perform doping. This method is simple to operate but has many problems: ① The iron phosphate grains are small and needle-shaped or flake-shaped: This is mainly due to three reasons. First, the conventional stirring and heating process is limited by the boiling point of water, and the temperature of the conversion insulation is generally lower than 100°C. The low temperature makes it difficult for the conversion phase change process to cross the energy barrier, resulting in incomplete growth; secondly, after the introduction of doping elements, the orderliness of the iron phosphate crystals is destroyed. Affected by the different valences and electronegativity of the doped elements, the ion stacking is disrupted, causing the crystal growth to stop; finally, in an environment of intense stirring, the grains rub and collide with each other, making it difficult for the grains to grow.

[0005] ② The iron-phosphorus ratio is too low, and the proportion of pure iron phosphate phase is small: This is mainly caused by two reasons. First, the substitution of doping elements for iron positions will itself cause the iron content to decrease, thus affecting the iron-phosphorus ratio; secondly, the conversion process of ammonium ferric phosphate to iron phosphate is usually carried out in a low pH, phosphate-rich environment, which will cause the outer periphery of the iron phosphate crystal to be coated with a layer of phosphate framework. This phosphate layer will increase the phosphorus content. When the grain size decreases, the proportion of the phosphate layer increases, and the effect is particularly significant.

[0006] ③ The doping rate of doping elements is low, and the cost of doping salt and wastewater treatment is high: the conversion temperature of the conventional reactor system is low, the ion thermal motion is low, and during the grain formation process, the doping elements are not easy to participate in the framework construction. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method, comprising the following steps: S1. Raw material preparation: prepare 0.5-2.0 mol / L ammonium phosphate solution, 0.5-2.0 mol / L phosphoric acid solution, 0.5-2.0 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 30-60 min to obtain slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 2.5-3.5 kg of yellow first-wash filter cake, add 8.0-12.0 kg of water, 200-800 g of phosphoric acid solution prepared in step S1, and 120-180 g of titanium sulfate, beat and stir evenly, place in a hydrothermal kettle, place the hydrothermal kettle in a 160-180° C. oven and keep it still for 20-28 h, take out the hydrothermal kettle, cool it to room temperature, take out the internal slurry, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

[0008] Moreover, in step S1, the pH of the ammonium phosphate solution is 6.5-7.5.

[0009] Moreover, in the step S1, the mass ratio is 0.8-1.2 of ferrous titanium dioxide solution and ammonium phosphate solution.

[0010] Moreover, in the step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide is 1: 1.00-1.08: 0.60-0.65.

[0011] Moreover, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide into the reaction container is: the titanium dioxide ferrous solution is used as the base, and the ammonium phosphate solution and the hydrogen peroxide are added in parallel.

[0012] Moreover, the feeding rate of the ammonium phosphate solution is 100-300 ml / min, the feeding rate of the hydrogen peroxide is 5-15 ml / min, and the reaction temperature is maintained at 30-60°C.

[0013] Moreover, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution, and the hydrogen peroxide solution into the reaction container is: using pure water as the base, adding the ammonium phosphate solution and the titanium dioxide ferrous solution in parallel into the reaction container, and then adding the hydrogen peroxide solution.

[0014] Moreover, the feeding rate of the ammonium phosphate solution and the titanium dioxide ferrous solution is 100-300 ml / min, the feeding rate of the hydrogen peroxide is 5-15 ml / min, and the reaction temperature is 30-60°C.

[0015] Moreover, during the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

[0016] 10. A method for improving the morphology and crystallinity of titanium-doped ferric phosphate grains by hydrothermal method as claimed in claim 1, characterized in that during the conversion in step S3, the hydrothermal autoclave used is a stainless steel high-pressure hydrothermal autoclave with a temperature of 160-180°C and a pressure of 6-10 atm.

[0017] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention obtains iron phosphate crystals by converting ammonium iron phosphate through a hydrothermal method. The primary particles of iron phosphate are thicker sheets, and the sheets are irregularly stacked, or regular large blocks, with a length of about 500 nm, and clear boundaries between particles. During the preparation process, a high temperature and high pressure growth environment and doping elements are simultaneously introduced to reduce the influence of doping on the crystallinity of iron phosphate, and finally the iron-phosphorus ratio of the finished iron phosphate is as high as 98.63%, and the Ti element incorporation rate is nearly 100%. The iron phosphate prepared by the hydrothermal method of the present invention has high crystallinity, high iron-phosphorus ratio, and high titanium incorporation rate.

[0018] 2. As the precursor of lithium iron phosphate, the physical and chemical indicators of iron phosphate will directly affect the performance of the back-end finished product. Doping at the iron phosphate end is expected to improve the compaction and electrical properties of the finished product. Doping can improve the electrochemical properties of lithium iron phosphate. The current doping process usually introduces doping salts into the iron phosphate synthesis raw materials or in the synthesis conversion process. Because the valence, ion radius, and electronegativity of the doping elements are different from those of the replaced elements, the order of the crystal structure will inevitably be destroyed after doping, which will cause the iron phosphate grains to become smaller and the iron phosphate phase to be reduced at the microscopic level, thereby causing the electrical properties of the finished lithium iron phosphate to be damaged; the present invention improves the iron-phosphorus ratio of the material while doping, as follows: ① The iron-to-phosphorus ratio of doped iron phosphate increases and the crystallinity is improved: By applying a sealed high-pressure environment, the hydrothermal kettle can increase the conversion temperature from the original 80-100°C to 160-180°C. The high temperature environment can increase the reversibility of chemical bond formation and breaking, and promote amorphous ammonium iron phosphate to spontaneously generate a low-energy, stable iron phosphate phase. Theoretically, the iron-to-phosphorus ratio of pure iron phosphate is 1. As the proportion of the iron phosphate phase increases, the iron-to-phosphorus ratio and crystallinity of the final product will increase.

[0019] ② Improved utilization of doping elements: High temperature can promote the thermal motion of ions and increase their kinetic energy. According to collision reaction theory, violent molecular thermal motion can increase the probability of ion collision, allowing originally low-energy ions to participate in the reaction process, thereby improving the utilization of doping elements.

[0020] ③ Grain enlargement and complete development: In the low-temperature stirring environment of the traditional reactor, the grains need to withstand collision and friction between grains during the growth process, and the low temperature also reduces the reversibility of chemical bonds during the growth of the crystal, resulting in limited grain growth. In contrast, the high-temperature static environment of the hydrothermal reactor is more conducive to the full development and growth of the grains, thereby obtaining thicker and larger primary grains. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The SEM image of iron phosphate obtained in Example 3; Figure 2 The X-ray diffraction pattern of ferric phosphate dihydrate obtained for Example 3; Figure 3 The SEM image of iron phosphate obtained in Example 3; Figure 4 The X-ray diffraction pattern of ferric phosphate dihydrate obtained for Example 6; Figure 5 The SEM image of iron phosphate obtained for Comparative Example 1; Figure 6 The X-ray diffraction pattern of iron phosphate dihydrate obtained for Comparative Example 1; Figure 7 The SEM image of iron phosphate obtained for Comparative Example 2; Figure 8 The X-ray diffraction pattern of iron phosphate dihydrate was obtained for Comparative Example 2. DETAILED DESCRIPTION

[0022] Example 1 A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method comprises the following steps: S1. Raw material preparation: prepare 0.5 mol / L ammonium phosphate solution, 0.5 mol / L phosphoric acid solution, 0.5 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 30 min to obtain slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 2.5 kg of yellow first-wash filter cake, add 8.0 kg of water, 200 g of phosphoric acid solution prepared in step S1, and 120 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 160° C. oven and keep it warm for 20 h, take out the hydrothermal kettle, cool it to room temperature, take out the internal slurry, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

[0023] Preferably, in step S1, the pH of the ammonium phosphate solution is 6.5.

[0024] Preferably, in step S1, the mass ratio of titanium dioxide ferrous solution to ammonium phosphate solution is 0.8.

[0025] Preferably, in step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide solution is 1:1.00:0.60.

[0026] Preferably, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide into the reaction container is: the titanium dioxide ferrous solution is used as the base, and the ammonium phosphate solution and the hydrogen peroxide are added in parallel.

[0027] Preferably, the feeding rate of the ammonium phosphate solution is 100 ml / min, the feeding rate of the hydrogen peroxide is 5 ml / min, and the reaction temperature is maintained at 30°C.

[0028] Preferably, during the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

[0029] Preferably, during the conversion in step S3, the hydrothermal kettle used is a stainless steel high-pressure hydrothermal kettle with a temperature of 160° C. and a pressure of 6 atm.

[0030] Example 2 A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method comprises the following steps: S1. Raw material preparation: prepare 2.0 mol / L ammonium phosphate solution, 2.0 mol / L phosphoric acid solution, 2.0 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 60 min to obtain slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 3.5 kg of yellow first-wash filter cake, add 12.0 kg of water, 800 g of phosphoric acid solution prepared in step S1, and 180 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 180°C oven and keep it still for 28 h, take out the hydrothermal kettle, cool it to room temperature, take out the internal slurry, filter and wash until the conductivity of the wash water drops to below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

[0031] Preferably, in step S1, the pH of the ammonium phosphate solution is 7.5.

[0032] Preferably, in step S1, the mass ratio of titanium dioxide ferrous solution to ammonium phosphate solution is 1.2.

[0033] Preferably, in step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide is 1:1.08:0.65.

[0034] Preferably, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide into the reaction container is: the titanium dioxide ferrous solution is used as the base, and the ammonium phosphate solution and the hydrogen peroxide are added in parallel.

[0035] Preferably, the feeding rate of the ammonium phosphate solution is 300 ml / min, the feeding rate of the hydrogen peroxide is 15 ml / min, and the reaction temperature is maintained at 60°C.

[0036] Preferably, during the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

[0037] Preferably, during the conversion in step S3, the hydrothermal kettle used is a stainless steel high-pressure hydrothermal kettle with a temperature of 180° C. and a pressure of 10 atm.

[0038] Example 3 A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method comprises the following steps: S1. Raw material preparation: prepare 1.0 mol / L ammonium phosphate solution, 1.0 mol / L phosphoric acid solution, 1.0 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 45 minutes to obtain a slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 3.0 kg of yellow first-wash filter cake, add 10.0 kg of water, 600 g of phosphoric acid solution prepared in step S1, and 150 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 170°C oven and keep it warm for 24 h, take out the hydrothermal kettle, take out the internal slurry after cooling to room temperature, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

[0039] Preferably, in step S1, the pH of the ammonium phosphate solution is 7.

[0040] Preferably, in step S1, the mass ratio of titanium dioxide ferrous solution to ammonium phosphate solution is 1.0.

[0041] Preferably, in step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide is 1:1.04:0.63.

[0042] Preferably, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide into the reaction container is: the titanium dioxide ferrous solution is used as the base, and the ammonium phosphate solution and the hydrogen peroxide are added in parallel.

[0043] Preferably, the feeding rate of the ammonium phosphate solution is 200 ml / min, the feeding rate of the hydrogen peroxide is 10 ml / min, and the reaction temperature is maintained at 45°C.

[0044] Preferably, during the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

[0045] Preferably, during the conversion in step S3, the hydrothermal autoclave used is a stainless steel high-pressure hydrothermal autoclave with a temperature of 170° C. and a pressure of 8 atm.

[0046] Example 4 A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method comprises the following steps: S1. Raw material preparation: prepare 0.5 mol / L ammonium phosphate solution, 0.5 mol / L phosphoric acid solution, 0.5 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 30 min to obtain slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 2.5 kg of yellow first-wash filter cake, add 8.0 kg of water, 200 g of phosphoric acid solution prepared in step S1, and 120 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 160° C. oven and keep it warm for 20 h, take out the hydrothermal kettle, cool it to room temperature, take out the internal slurry, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

[0047] Preferably, in step S1, the pH of the ammonium phosphate solution is 6.5.

[0048] Preferably, in step S1, the mass ratio of titanium dioxide ferrous solution to ammonium phosphate solution is 0.8.

[0049] Preferably, in step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide solution is 1:1.00:0.60.

[0050] Preferably, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide solution into the reaction container is: using pure water as the base, adding the ammonium phosphate solution and the titanium dioxide ferrous solution into the reaction container in parallel, and then adding the hydrogen peroxide.

[0051] Preferably, the feeding rate of the ammonium phosphate solution and the titanium dioxide ferrous solution is 100 ml / min, the feeding rate of the hydrogen peroxide is 5 ml / min, and the reaction temperature is 30°C.

[0052] Preferably, during the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

[0053] Preferably, during the conversion in step S3, the hydrothermal autoclave used is a stainless steel high-pressure hydrothermal autoclave with a temperature of 160° C. and a pressure of 6 atm.

[0054] Example 5 A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method comprises the following steps: S1. Raw material preparation: prepare 2.0 mol / L ammonium phosphate solution, 2.0 mol / L phosphoric acid solution, 2.0 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 60 min to obtain slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 3.5 kg of yellow first-wash filter cake, add 12.0 kg of water, 800 g of phosphoric acid solution prepared in step S1, and 180 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 180°C oven and keep it still for 28 h, take out the hydrothermal kettle, cool it to room temperature, take out the internal slurry, filter and wash until the conductivity of the wash water drops to below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

[0055] Preferably, in step S1, the pH of the ammonium phosphate solution is 7.5.

[0056] Preferably, in step S1, the mass ratio of titanium dioxide ferrous solution to ammonium phosphate solution is 1.2.

[0057] Preferably, in step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide is 1:1.08:0.65.

[0058] Preferably, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide solution into the reaction container is: using pure water as the base, adding the ammonium phosphate solution and the titanium dioxide ferrous solution into the reaction container in parallel, and then adding the hydrogen peroxide.

[0059] Preferably, the feeding rate of the ammonium phosphate solution and the titanium dioxide ferrous solution is 300 ml / min, the feeding rate of the hydrogen peroxide is 15 ml / min, and the reaction temperature is 60°C.

[0060] Preferably, during the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

[0061] Preferably, during the conversion in step S3, the hydrothermal kettle used is a stainless steel high-pressure hydrothermal kettle with a temperature of 180° C. and a pressure of 10 atm.

[0062] Example 6 A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method comprises the following steps: S1. Raw material preparation: prepare 1.0 mol / L ammonium phosphate solution, 1.0 mol / L phosphoric acid solution, 1.0 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 45 minutes to obtain a slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 3.0 kg of yellow first-wash filter cake, add 10.0 kg of water, 600 g of phosphoric acid solution prepared in step S1, and 150 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 170°C oven and keep it warm for 24 h, take out the hydrothermal kettle, take out the internal slurry after cooling to room temperature, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

[0063] Preferably, in step S1, the pH of the ammonium phosphate solution is 7.

[0064] Preferably, in step S1, the mass ratio of titanium dioxide ferrous solution to ammonium phosphate solution is 1.0.

[0065] Preferably, in step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide is 1:1.04:0.63.

[0066] Preferably, in step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide solution into the reaction container is: using pure water as the base, adding the ammonium phosphate solution and the titanium dioxide ferrous solution into the reaction container in parallel, and then adding the hydrogen peroxide.

[0067] Preferably, the feeding rate of the ammonium phosphate solution and the titanium dioxide ferrous solution is 200 ml / min, the feeding rate of the hydrogen peroxide is 10 ml / min, and the reaction temperature is 45°C.

[0068] Preferably, during the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

[0069] Preferably, during the conversion in step S3, the hydrothermal autoclave used is a stainless steel high-pressure hydrothermal autoclave with a temperature of 170° C. and a pressure of 8 atm.

[0070] Comparative Example 1 The difference between this comparative example and Example 3 is that the conversion temperature is controlled at 90°C, the pressure is normal pressure (101.3 kPa), and the temperature is kept for 2 hours, as follows: S3, conversion: take 3 kg of yellow first-wash filter cake, add 10.0 kg of water, 500 g of phosphoric acid solution prepared in step S1, and 160 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 90°C oven and keep it warm for 2 hours, take out the hydrothermal kettle, take out the internal slurry after cooling to room temperature, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake;

[0071] Comparative Example 2 The difference between this comparative example and Example 3 is that: In S2: the specific methods of adding the ammonium phosphate solution, the titanium dioxide ferrous solution, and the hydrogen peroxide solution into the reaction container are different; In S3: the conversion temperature is controlled at 90°C, the pressure is normal pressure (101.3 kPa), and the temperature is kept for 2 hours, as follows: S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 45 minutes to obtain a slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; Preferably, in step S2, the specific method of adding the ammonium phosphate solution, the ferrous titanium dioxide solution and the hydrogen peroxide into the reaction container is: the iron source solution is mixed with phosphoric acid to form a base, and the ammonium phosphate solution and the hydrogen peroxide are added in stages and sequentially, the feeding rate of the ammonium phosphate solution is 200 ml / min, the feeding rate of the hydrogen peroxide is maintained at 10 ml / min, and the reaction temperature is maintained at 45°C.

[0072] S3, conversion: take 3 kg of yellow first-wash filter cake, add 10.0 kg of water, 500 g of phosphoric acid solution prepared in step S1, and 160 g of titanium sulfate, beat and stir evenly, put it in a hydrothermal kettle, put the hydrothermal kettle in a 90°C oven and keep it warm for 2 hours, take out the hydrothermal kettle, take out the internal slurry after cooling to room temperature, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake;

[0073] Experimental Section

[0074] Experiment 1 The iron phosphate obtained in Example 3 was subjected to electron microscope scanning and iron phosphate dihydrate was subjected to X-ray analysis. Figure 1 , 2 As shown, Figure 1 The SEM image of iron phosphate obtained in Example 3, Figure 2 The X-ray diffraction pattern of ferric phosphate dihydrate obtained for Example 3; from Figure 1 It can be seen that the primary iron phosphate particles converted under the high pressure and high temperature conditions of the present invention are regular large blocks with a length of about 500 nm and clear boundaries between particles.

[0075] Figure 2 In the X-ray diffraction pattern (XRD) of iron phosphate, obvious peaks of dihydrate iron phosphate can be seen. Even without high-temperature calcination, the diffraction peaks of the crystals are very strong, showing good crystallinity.

[0076] Experiment 2 The iron phosphate obtained in Example 6 was subjected to electron microscope scanning, and the iron phosphate dihydrate was subjected to X-ray analysis. Figure 3 , 4 As shown, Figure 3 The SEM image of iron phosphate obtained in Example 6 is as follows: Figure 4 The X-ray diffraction pattern of ferric phosphate dihydrate obtained for Example 6; from Figure 3 It can be seen that the primary particles of iron phosphate converted under high pressure and high temperature conditions of the present invention are in the form of thicker flakes, and the flakes are irregularly stacked.

[0077] Figure 4 In the X-ray diffraction pattern of ferric phosphate dihydrate, obvious ferric phosphate dihydrate peaks can be seen. Even without high-temperature calcination, the diffraction peaks of the crystals are very strong, showing good crystallinity.

[0078] Experiment 3 The iron phosphate obtained in Comparative Example 1 was subjected to electron microscope scanning, and the iron phosphate dihydrate was subjected to X-ray analysis. Figure 5 , 6 As shown, Figure 5 The SEM image of iron phosphate obtained in Comparative Example 1 is as follows: Figure 6 The X-ray diffraction pattern of iron phosphate dihydrate obtained for Comparative Example 1; from Figure 5 It can be seen that the primary particles of iron phosphate converted under normal pressure and low temperature conditions are long needle-shaped with a length of about 200 nm, and form small round flakes after accumulation. Compared with the morphology prepared by the hydrothermal method (the present invention), the size of the primary particles in the conventional process is much smaller than that of Examples 2 and 3, and the particles are not fully developed.

[0079] Figure 6 The X-ray diffraction spectrum of the product obtained by transformation under normal pressure and low temperature conditions is shown. It can be seen that its peak shape basically corresponds to the monoclinic dihydrate iron phosphate standard card. However, the intensity of each diffraction peak is low and the half-peak width is wide, indicating that the degree of grain development is poor. Compared with the sharp diffraction peaks of Examples 3 and 6, the crystallinity of the grains is worse.

[0080] Experiment 4 The iron phosphate obtained in Comparative Example 2 was subjected to electron microscope scanning, and the iron phosphate dihydrate was subjected to X-ray analysis. Figure 7 , 8 As shown, Figure 7 The SEM image of iron phosphate obtained in Comparative Example 2 is as follows: Figure 8The X-ray diffraction pattern of ferric phosphate dihydrate was obtained for Comparative Example 2; from Figure 7 It can be seen that the primary particles of iron phosphate converted under normal pressure and low temperature conditions are long needle-shaped with a length of about 200 nm, and form small round flakes after accumulation. Compared with the morphology prepared by the hydrothermal method (the present invention), the size of the primary particles in the conventional process is much smaller than that of Examples 2 and 3, and the particles are not fully developed.

[0081] Figure 8 The X-ray diffraction spectrum of the product obtained by transformation under normal pressure and low temperature conditions is shown. It can be seen that its peak shape basically corresponds to the monoclinic iron phosphate dihydrate standard card. However, the intensity of each diffraction peak is low and the half-peak width is wide, indicating that the degree of grain development is poor. Compared with the sharp diffraction peaks of Examples 3 and 6, the crystallinity of the grains is worse.

[0082] Experiment 5 The Fe content, P content, H2O content, iron-phosphorus ratio (Fe / P), specific surface area (BET), density (TD), Ti content, and D50 (the particle size corresponding to the cumulative particle size distribution percentage of the sample reaching 50%) of the finished iron phosphate prepared in Example 3, Example 6, Comparative Example 1, and Comparative Example 2 were respectively measured, as shown in Table 1.

[0083] Table 1 Physical and chemical indicators of ferric phosphate

[0084] It can be seen from Table 1 that after the calcined iron phosphate in Example 3 is doped with Ti, the iron-phosphorus ratio of the iron phosphate is 98.63%, which is about 0.96-0.98 for the undoped Ti sample in the prior art, and the iron-phosphorus ratio of the iron phosphate is maintained at a relatively high level; under the technical scheme of Example 6, the theoretical value of the doping amount of the finished iron phosphate should be 2500 ppm; the actual doping rate of the sample is 2662 ppm, which is equivalent to the theoretical doping rate, and the Ti element doping rate is nearly 100%.

[0085] The physical and chemical indicators of iron phosphate after calcination in Example 6 show that after Ti doping, the iron-phosphorus ratio of iron phosphate is 98.56%, which is maintained at a relatively high level compared with the iron-phosphorus ratio of non-Ti-doped samples in the prior art of about 0.96-0.98. Under the technical scheme of Example 6, the theoretical value of the doping amount of finished iron phosphate should be 2500 ppm. The actual doping rate of the sample is 2576 ppm, which is equivalent to the theoretical doping rate, and the Ti element doping rate is nearly 100%.

[0086] The physical and chemical indicators of the iron phosphate after calcination in Comparative Example 1 show that after Ti doping, the iron-phosphorus ratio of the iron phosphate is 94.25%, which is significantly reduced compared with the iron-phosphorus ratio of the non-Ti-doped sample in the prior art of about 0.96-0.98. Under the technical scheme of Comparative Example 1, the theoretical value of the doping amount of the finished iron phosphate should be 2500 ppm. The actual doping rate of the sample is 2025 ppm, and about 19% of the Ti element is lost.

[0087] The physical and chemical indicators of iron phosphate after calcination in Comparative Example 2 show that after Ti doping, the iron-phosphorus ratio of iron phosphate is 94.71%, which is significantly reduced compared with the iron-phosphorus ratio of the non-Ti-doped sample in the prior art of about 0.96-0.98. Under the technical scheme of Comparative Example 1, the theoretical value of the doping amount of the finished iron phosphate should be 2500 ppm. The actual doping rate of the sample is 1998 ppm, and about 20% of the Ti element is lost.

Claims

1. A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by a hydrothermal method, characterized in that: The steps include: S1. Raw material preparation: prepare 0.5-2.0 mol / L ammonium phosphate solution, 0.5-2.0 mol / L phosphoric acid solution, 0.5-2.0 mol / L titanium dioxide ferrous solution, and 30% hydrogen peroxide for standby use; S2, synthesis: adding ammonium phosphate solution, titanium dioxide ferrous solution and hydrogen peroxide into a reaction container, reacting for 30-60 min to obtain slurry; filtering and washing the slurry until the conductivity of the washing water is less than 4000 μS / cm to obtain a yellow washed filter cake; S3, conversion: take 2.5-3.5 kg of yellow first-wash filter cake, add 8.0-12.0 kg of water, 200-800 g of phosphoric acid solution prepared in step S1, and 120-180 g of titanium sulfate, beat and stir evenly, place in a hydrothermal kettle, place the hydrothermal kettle in a 160-180° C. oven and keep it still for 20-28 h, take out the hydrothermal kettle, cool it to room temperature, take out the internal slurry, filter and wash until the conductivity of the wash water drops below 1000 μS / cm, and obtain a light pink second-wash filter cake; S4, calcination: drying the light pink second-wash filter cake to obtain ferric phosphate dihydrate, calcining and crushing the ferric phosphate dihydrate to obtain finished ferric phosphate.

2. A method for increasing the iron-phosphorus ratio of an iron phosphate material as claimed in claim 1, characterized in that: In step S1, the pH of the ammonium phosphate solution is 6.5-7.

5.

3. The method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 1, characterized in that: In the step S1, the mass ratio is 0.8-1.2 of ferrous titanium dioxide solution and ammonium phosphate solution.

4. The method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 1, characterized in that: In step S2, the mass ratio of titanium dioxide ferrous solution: ammonium phosphate solution: hydrogen peroxide is 1: 1.00-1.08: 0.60-0.

65.

5. The method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 1, characterized in that: In step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide into the reaction container is: the titanium dioxide ferrous solution is used as the base, and the ammonium phosphate solution and the hydrogen peroxide are added in parallel.

6. A method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 5, characterized in that: The feeding rate of the ammonium phosphate solution is 100-300 ml / min, the feeding rate of the hydrogen peroxide is 5-15 ml / min, and the reaction temperature is maintained at 30-60°C.

7. The method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 1, characterized in that: In step S2, the specific method of adding the ammonium phosphate solution, the titanium dioxide ferrous solution and the hydrogen peroxide solution into the reaction container is: using pure water as the base, adding the ammonium phosphate solution and the titanium dioxide ferrous solution into the reaction container in parallel, and then adding the hydrogen peroxide.

8. The method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 7, characterized in that: The feeding rate of the ammonium phosphate solution and the titanium dioxide ferrous solution is 100-300 ml / min, the feeding rate of the hydrogen peroxide is 5-15 ml / min, and the reaction temperature is 30-60°C.

9. The method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 1, characterized in that: During the synthesis in step S2, the reaction vessel used is a glass stirring kettle.

10. The method for improving the morphology and crystallinity of titanium-doped iron phosphate grains by hydrothermal method according to claim 1, characterized in that: During the conversion in step S3, the hydrothermal kettle used is a stainless steel high-pressure hydrothermal kettle with a pressure of 6-10 atm.

Citation Information

Cited By

  • Method for preparing low-aluminum titanium-doped iron phosphate material by utilizing ferrophosphorus slag

    CN120246954A