Method for compositely modifying energetic material by adopting physical mixing method

The use of microcrystalline wax and sorbitan oleate to modify 2,4,6-trinitrophenol by physical mixing method solves its explosiveness and environmental hazards, improves storage and transportation safety, and achieves the High stability and environmentally friendly storage effect.

CN119019208APending Publication Date: 2024-11-26CHANGZHOU UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411137977.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, 2,4,6-trinitrophenol, as an energy-containing material, is explosive and has great harm to the human body and the environment. There is a risk of fire and explosion accidents during storage and transportation, and it is difficult to degrade.

Method used

Using the physical mixing method, microcrystalline wax as insensitizer and sorbitan oleate as emulsifier, TNP is wrapped in wax materials through stirring, drying and grinding, reducing its risk of decomposition Sex and sensitivity.

Benefits of technology

It effectively reduces the risk of decomposition of TNP under heated conditions, improves its stability and storage safety, enhances thermal stability, reduces thermal hazards during storage, and the materials used are environmentally friendly and degradable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019208A_ABST
    Figure CN119019208A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite modification of energetic materials, in particular to a method for compositely modifying an energetic material by adopting a physical mixing method. The modifier relates to a desensitizing agent and an emulsifying agent, and the effect of composite modification of the energetic material by the desensitizing agent and the emulsifying agent in a mass ratio of 1: 1 is researched. The modified sample can be prepared through heating stirring, preparation mixing, physical mixing, mechanical ball milling and vacuum drying. The method is applied to the field of compound modification, and the microcrystalline wax serving as the desensitizing agent can coat the surface of an energetic material, fill gaps among substances, reduce friction, disperse external acting force and absorb heat, so that the substances are desensitized. Sorbitan oleate serving as an emulsifier is an emulsifier commonly used in the field of emulsion explosives, and the composite modified material has the advantages of high stability, insensibility and easiness in storage, reduces the thermal risk in the storage process, and has guiding significance in storage and transportation of energetic substances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite modification of energetic materials, in particular to a method for composite modification of energetic materials by adopting a physical mixing method. Background Art

[0002] Energetic materials are a class of metastable compounds or mixtures, which have been widely used in explosives, propeller manufacturing, and aerospace in recent years. 2,4,6-Trinitrophenol (TNP), also known as picric acid, is a yellow or white needle-shaped crystalline powder that contains huge energy and is prone to explosion when subjected to friction or impact. In addition, this nitro-energetic substance causes great harm to the human body. Inhalation or contact can cause headaches, nausea, dizziness, difficulty in swallowing, diarrhea, vomiting, shock, convulsions or death, etc., causing irreversible damage to the central nervous system of organisms. It is difficult to degrade and adsorb in the environment, and will cause great harm to organisms in the water.

[0003] TNP can be used to make explosives, dyes, and matches. It explodes at a boiling point of 300°C. Improper storage can cause fires and explosions. In addition, contact with metals during storage can generate more sensitive picrates that can cause explosions. Summary of the invention

[0004] The technical problem to be solved by the present invention is: to overcome the deficiencies in the prior art and provide a method for composite modification of energetic materials using a physical mixing method. In the modification process, the present invention uses a composite modification method of a desensitizer and an emulsifier to reduce the risk of decomposition of picric acid under thermal conditions; wherein the desensitizer used is a wax-based desensitizer microcrystalline wax with good plasticity and is relatively economical and convenient, and the emulsifier uses an oil-in-water emulsifier sorbitan oleate that is currently commonly used in the field of emulsion explosives.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for composite modification of energetic materials by physical mixing method comprises the following steps:

[0007] Step S1, weigh the desensitizing agent and place it in a three-necked flask, and place the beaker in an oil bath at 80°C and stir evenly, then pour the molten desensitizing agent into the beaker and move it to an 80°C forced air drying oven for heat preservation and standby use;

[0008] Step S2, weighing a raw material TNP sample into a beaker, first pouring an emulsifier into the beaker containing the TNP sample, placing it under a magnetic stirrer and stirring it thoroughly, and after the TNP sample is fully emulsified, adding a molten desensitizer and a solvent carbon tetrachloride solution;

[0009] Step S3, placing the beaker on a dry magnetic stirrer and stirring at a temperature of 75° C. and a speed of 1200 r / min, and slowly cooling to room temperature after the solvent is completely evaporated to obtain a solid;

[0010] Step S4, grinding the solid in a planetary ball mill to obtain a sample powder;

[0011] Step S5: Place the obtained sample powder in a vacuum drying oven at 60° C. and dry for 12 h to obtain a finished product.

[0012] Furthermore, the desensitizing agent in step S1 is microcrystalline wax (MCW), which is a commonly used wax desensitizing agent with a melting point of 62-78° C., good plasticity, and economical; the oil bath stirring time is 10 minutes.

[0013] Furthermore, the emulsifier in step S2 is sorbitan oleate, an emulsifier commonly used in emulsion explosives, with a purity of 99.7%, and is a yellow viscous liquid; the mass ratio of the TNP sample, the emulsifier and the desensitizing agent is 2:1:1.

[0014] Furthermore, the ball milling time in step S4 is 30 minutes, and the grinding is specifically as follows: the solid and the steel ball are placed in a grinding bowl, and the direction is changed every 5 minutes to ensure uniform grinding.

[0015] TNP is a sensitive energetic material that is highly flammable and explosive under dry conditions. The use of emulsifiers can reduce the friction between TNP molecules, thus reducing sensitivity; the use of desensitizing agents can fill the cracks on the surface of TNP, thus reducing the friction between molecules and isolating water. The modification process makes the danger of TNP more controllable during storage and transportation.

[0016] The beneficial effects of the present invention are as follows: the present invention has a reasonable design, a simple preparation method, and has the following advantages:

[0017] (1) The insensitivity agent in the present invention is microcrystalline wax, which is different from nitro-based insensitivity agents. Nitro-based insensitivity agents have hidden dangers such as continuous environmental pollution and high risk. Microcrystalline wax is a green, environmentally friendly and degradable insensitivity agent that can be coated on the surface of energetic materials, fill the gaps between materials, reduce friction, disperse external forces and absorb heat, thereby making the material insensitive;

[0018] (2) The present invention adopts a relatively high emulsification property. The emulsifier of the present invention is different from other emulsifiers. The emulsifier sorbitan oleate is a water-in-oil emulsifier commonly used in the field of emulsion explosives and is green and environmentally friendly.

[0019] (3) The composite modifier of the present invention has high water-isolating properties and can effectively isolate moisture during storage to prevent 2,4,6-trinitrophenol from absorbing moisture;

[0020] (4) The composite modifier of the present invention has high stability, and the activation energy of the modified sample is significantly improved, thereby increasing the thermal stability of the sample;

[0021] (5) The composite modified material of the present invention has the advantages of high stability, insensitivity, and easy storage, which reduces the thermal risk of the storage process and has positive significance for the storage and transportation of energetic substances. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 is a composite modification flow chart of Example 1;

[0024] Figure 2 The microscopic morphology characterized by SEM before and after composite modification of Example 1, wherein a is before composite modification, and b is after composite modification;

[0025] Figure 3 FTIR and XPS characterization of the composite modified sample of Example 1;

[0026] Figure 4 1 is the temperature-heat flow curve of the sample before and after composite modification in Example 1, wherein a is before composite modification and b is after composite modification;

[0027] Figure 5 It is the activation energy curve predicted by the Kissinger method of the sample before and after the composite modification in Example 1;

[0028] Figure 6 These are the activation energy curves predicted by the KAS method of the samples before and after composite modification in Example 1. DETAILED DESCRIPTION

[0029] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] like Figure 1 A method for composite modification of energetic materials using a physical mixing method is shown, which specifically comprises the following steps:

[0034] Step S1, weigh microcrystalline wax (MCW) and place it in a three-necked flask, and place the beaker in an 80°C oil bath and stir evenly, then pour the molten microcrystalline wax into the beaker and move it to an 80°C forced air drying oven for heat preservation and standby use; the drying oven is heat-preserved and standby use.

[0035] Step S2, weighing 1 g of TNP sample into a beaker, pouring the emulsifier into the beaker containing the TNP sample in a mass ratio of microcrystalline wax to emulsifier of 1:1, placing the beaker under a magnetic stirrer and stirring thoroughly, and adding molten microcrystalline wax and 10 g of solvent carbon tetrachloride solution after the TNP sample is fully emulsified;

[0036] Step S3, placing the beaker on a dry magnetic stirrer and stirring at a temperature of 75° C. and a speed of 1200 r / min, and slowly cooling the temperature to room temperature of 25° C. after the solvent is completely evaporated to obtain a solid;

[0037] Step S4, grinding the solid in a planetary ball mill to obtain a sample powder;

[0038] Step S5: Place the obtained sample powder in a vacuum drying oven at 60° C. and dry for 12 h to obtain a finished product.

[0039] The emulsifier is sorbitan oleate, referred to as Span-80.

[0040] Step S2 is specifically as follows: 1 g of TNP (2,4,6-trinitrophenol) is weighed, and since the sample will change when dissolved in water, it is ensured to be dry during the weighing process; the mass ratio of Span 80 to microcrystalline wax is 1:1, that is, 0.5 g of microcrystalline wax and 0.5 g of Span 80 are weighed; the speed of the magnetic stirrer in step S2 is 1200 r / min; in step S2, TNP is insoluble in the solvent carbon tetrachloride solution, and the boiling point of the solvent is 76°C.

[0041] The products prepared in the above examples were analyzed by the following characterization methods. The test analysis results of the product prepared in Example 1 are as follows:

[0042] Scanning electron microscope (SEM) test: The powder sample is directly adhered to the conductive glue and tested directly after gold spraying. The test results are as follows: Figure 2 As shown. Figure 2 It can be seen that the surface of TNP is in a broken block shape with obvious cracks. After modification, the surface is in a clumpy shape with no voids, indicating that the composite modifier effectively fills the cracks on the sample surface.

[0043] Fourier transform infrared spectroscopy (FTIR) test: Take a certain amount of sample and use potassium bromide to press the tablet. The test results are as follows Figure 3 This indicates that the modified samples still have the typical chemical functional groups of the original samples.

[0044] X-ray Photoelectron Spectrometer (XPS) Test: Take an appropriate amount of sample and press it onto the sample plate. Place the sample into the sample chamber of the Thermo Scientific K-Alpha XPS instrument. When the pressure in the sample chamber is less than 2.0×10-7mbar, send the sample into the analysis chamber. The spot size is 400μm, the operating voltage is 12kV, and the filament current is 6mA. The test results are as follows: Figure 3 As shown, this shows that the samples before and after modification still have the chemical elements of the original samples, and the modification process has not changed the chemical element composition, indicating that microcrystalline wax, Span 80 and TNP have good compatibility.

[0045] Differential Scanning Calorimetry (DSC) test: According to the heating rate of 1, 3, 5, 8, 10 ° C / min, using a 25 μl closed gold-plated crucible and a nitrogen atmosphere of 50 ml / min. The test results are as follows Figure 4 This indicates that the composite modification effectively reduces the decomposition heat of the substance.

[0046] The data were processed according to the following method to quantitatively evaluate the changes in apparent activation energy before and after modification. The method of use is as follows:

[0047] Kissinger Method:

[0048] KAS method:

[0049] The results and performance comparison of the composite modified samples are shown in Table 1. Figure 4 , Figure 5 .

[0050] Table 1 Comparison of sample properties before and after composite modification

[0051]

[0052] Table 1 shows the activation energy prediction values ​​calculated by the Kissinger kinetic method before and after the composite modification. The apparent activation energy refers to the difference between the average energy of the activated molecules and the average energy of all molecules. The lower the activation energy, the lower the stability of the sample during thermal decomposition. It is calculated that the modification process increases the activation energy of TNP, increases its stability, and is conducive to storage and transportation.

[0053] Figure 5 This is the curve fitted by the Kissinger kinetic method. The fitting degree is above 0.9, indicating that the fitting degree is high and the calculated activation energy value is reliable. Figure 6 This is the curve fitted by the isoconversion KAS kinetic method, which shows that the activation energy predicted by KAS is reliable.

[0054] In summary, the beneficial effects of the present invention are: the present invention has a reasonable design, a simple preparation method, and has the following advantages:

[0055] (1) The insensitivity agent in the present invention is microcrystalline wax, which is different from nitro-based insensitivity agents. Nitro-based insensitivity agents have hidden dangers such as continuous environmental pollution and high risk. Microcrystalline wax is a green, environmentally friendly and degradable insensitivity agent that can be coated on the surface of energetic materials, fill the gaps between materials, reduce friction, disperse external forces and absorb heat, thereby making the material insensitive;

[0056] (2) The present invention adopts a relatively high emulsification property. The emulsifier of the present invention is different from other emulsifiers. The emulsifier sorbitan oleate is a water-in-oil emulsifier commonly used in the field of emulsion explosives and is green and environmentally friendly.

[0057] (3) The composite modifier of the present invention has high water-isolating properties and can effectively isolate moisture during storage to prevent 2,4,6-trinitrophenol from absorbing moisture;

[0058] (4) The composite modifier of the present invention has high stability, and the activation energy of the modified sample is significantly improved, thereby increasing the thermal stability of the sample;

[0059] (5) The composite modified material of the present invention has the advantages of high stability, insensitivity, and easy storage, which reduces the thermal risk of the storage process and has positive significance for the storage and transportation of energetic substances.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for composite modification of energetic materials using a physical mixing method, characterized in that: The specific steps include: Step S1, weigh the desensitizing agent and place it in a three-necked flask, and place the beaker in an oil bath at 80°C and stir evenly, then pour the molten desensitizing agent into the beaker and move it to an 80°C forced air drying oven for heat preservation and standby use; Step S2, weighing a raw material TNP sample into a beaker, first pouring an emulsifier into the beaker containing the TNP sample, placing it under a magnetic stirrer and stirring it thoroughly, and after the TNP sample is fully emulsified, adding a molten desensitizer and a solvent carbon tetrachloride solution; Step S3, placing the beaker on a dry magnetic stirrer and stirring at a temperature of 75° C. and a speed of 1200 r / min, and slowly cooling to room temperature after the solvent is completely evaporated to obtain a solid; Step S4, grinding the solid in a planetary ball mill to obtain a sample powder; Step S5: Place the obtained sample powder in a vacuum drying oven at 60° C. and dry for 12 h to obtain a finished product.

2. The method for composite modification of energetic materials by physical mixing according to claim 1, characterized in that: The desensitizing agent in step S1 is microcrystalline wax, and the melting point of the microcrystalline wax is 62-78°C.

3. The method for composite modification of energetic materials by physical mixing according to claim 1, characterized in that: The oil bath stirring time in step S1 is 10 min.

4. The method for composite modification of energetic materials by physical mixing according to claim 1, characterized in that: The emulsifier in step S2 is sorbitan oleate; the mass ratio of the TNP sample, the emulsifier and the desensitizing agent is 2:1:

1.

5. The method for composite modification of energetic materials by physical mixing according to claim 1, characterized in that: The rotation speed of the magnetic stirrer in step S2 is 1200 r / min.

6. The method for composite modification of energetic materials by physical mixing according to claim 1, characterized in that: The ball milling time in step S4 is 30 minutes, and the grinding is specifically as follows: the solid and the steel ball are placed in a grinding bowl, and the direction is changed every 5 minutes to ensure uniform grinding.

Citation Information

Patent Citations

  • Method for coating CL-20 explosive with plasticized Estane5703

    CN106083494A

  • Wax composite insensitive agent with adjustable friction coefficient and preparation method thereof

    CN108456124A

  • Explosive with high-sensitivity-reduction coating layer structure and preparation method of explosive

    CN114907173A

  • Trinitrotolyl composite casting explosive and preparation method and application thereof

    CN122444562A

  • Explosive and its production

    JP1999278975A