Novel polyacrylamide as well as preparation method and application thereof
Through the self-polymerization of acrylic monomers and amino alcohol reaction, a safe new polyacrylamide was prepared, which solved the problem of using highly toxic substances in the prior art, and achieved safe application in the food field and improved dough performance.
Patent Information
- Application Number
- CN202410974052.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-26
AI Technical Summary
The use of highly toxic and harmful substances acrylonitrile and intermediate acrylamide in the existing synthesis methods of polyacrylamide has resulted in limited application in food and a food-safe and non-toxic production process is required.
Acrylic monomer is used to generate sodium polyacrylate of different acidity through self-polymerization, and esterification modification and amino alcohol reaction are carried out under nitrogen protection to prepare a new polyacrylamide, avoiding the use of highly toxic substances.
It realizes the safe application of polyacrylamide in the food field, improves the water-retaining and oil-retaining properties of the dough and can control the amide degree to meet different application needs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of edible colloid preparation, and specifically relates to a preparation method of a novel polyacrylamide. Background Art
[0002] Polyacrylamide is a linear organic high molecular polymer widely used in petroleum, water treatment, metallurgy and other industries. It can be used in food as a texture improver to improve the oil and water retention stability of the product. At present, the commonly used synthesis method of polyacrylamide is to first prepare acrylamide from acrylonitrile, and then generate polyacrylamide through polymerization. Although polyacrylamide itself is harmless, the synthetic raw material acrylonitrile and the intermediate acrylamide are highly toxic and harmful substances, and their inevitable residues are serious safety hazards. Therefore, polyacrylamide cannot be used as an ingredient in food. Therefore, a food-safe and non-toxic production process is urgently needed, which will greatly enhance the application prospects of sodium polyacrylate. Summary of the invention
[0003] The present invention aims at the shortcomings and deficiencies in the prior art, and provides a sodium polyacrylate synthesized from acrylic acid monomers, which is prepared by propylene glycol esterification modification and amino alcohol reaction. The new modified sodium polyacrylate used in this process uses safe acrylic acid as a raw material, and the production process adopts steam contact and nitrogen protection, so the production process is safer. It is applied to flour products, can improve the water and oil retention properties of dough, and improve the stability of oil in dough. The new polyacrylamide and its preparation method and application.
[0004] To achieve the above objectives, the present invention is implemented by the following technical scheme: The novel polyacrylamide and its preparation method and application provided by the present invention include the following steps:
[0005] Acrylic acid and sodium hydroxide in different proportions are subjected to self-polymerization reaction under the condition of sodium sulfite as an initiator to generate sodium polyacrylates with different acidities, which are then subjected to esterification reaction under nitrogen protection; they are then subjected to amidation reaction with amino alcohol under low temperature conditions, and after drying, polyacrylamides with different amide degrees are obtained.
[0006] Preferably, in the preparation method of sodium polyacrylate with different acidities, the molar ratio of acrylic acid to sodium hydroxide is 1:1-2; the concentration of acrylic acid aqueous solution is 15%-20%, and the mass ratio of sodium sulfite to acrylic acid is 0.01:1;
[0007] The reaction temperature in the self-polymerization reaction is 75°C to 85°C, and the time is 1h to 2h.
[0008] Preferably, the specific steps of the esterification reaction of sodium polyacrylate include the following:
[0009] (1) quantitatively weighing the prepared sodium polyacrylate;
[0010] (2) Dehydration: After centrifugation, the water content of the dehydrated sodium polyacrylate is 40% to 50%, which is directly used for the esterification reaction;
[0011] (3) Esterification: The sodium polyacrylate treated in step (2) and propylene oxide are put into a kneader. Under nitrogen protection, the kneader is turned on for esterification reaction for 1 h to 2 h, and post-treatment is performed to obtain propylene glycol esterified modified sodium polyacrylate.
[0012] Preferably, the post-processing step comprises:
[0013] (4) Cooling: After the esterification reaction is completed, the product is cooled, and when the temperature drops to 20° C. or below, the waste liquid is discharged;
[0014] (5) Hot air treatment: After the waste liquid in the kneader is removed, the kneader is closed and dry hot air is introduced into the kneader to remove the propylene oxide remaining in the propylene glycol esterified modified sodium polyacrylate;
[0015] (6) Drying: subjecting the propylene glycol esterified modified sodium polyacrylate product obtained after the hot air treatment in step (5) to rapid drying;
[0016] (7) Crushing: The dried product in step (6) is crushed and sieved using a crusher to obtain propylene glycol esterified modified sodium polyacrylate of a desired particle size.
[0017] Preferably, in step (3), the weight ratio of sodium polyacrylate to propylene oxide is 1:0.6-0.8; in step (5), the hot air condition is dry air at 50°C to 70°C;
[0018] In step (3), the kneading machine is a self-made device, which can vaporize propylene oxide and then cyclically contact with sodium polyacrylate to carry out esterification reaction. Under the protection of nitrogen, high-temperature reaction can be carried out to reduce reaction time and improve esterification degree.
[0019] Preferably, the method comprises subjecting the propylene glycol esterified modified sodium polyacrylate obtained in step (7) to an amidation reaction, and the specific steps are as follows:
[0020] The propylene glycol esterified modified sodium polyacrylate is added to a mixed solution of ammonia water / alcohol, and stirred continuously. The reaction temperature is 10°C-30°C, the amidation reaction time is 1h-2h, and the reaction pH is controlled to be greater than or equal to 11; after the reaction is completed, centrifugation is performed, and the residual ammonia water is washed away with a 0.5-1 mol / L acid / alcohol solution to neutralize the excess ammonia water. After the pH is adjusted to 7-8 to neutral, centrifugation, drying, and crushing are performed to obtain polyacrylamide.
[0021] Preferably, in the mixed solution of ammonia water / alcohol, the concentration of ammonia water is 1-5 mol / L, the mass ratio of ammonia water to alcohol solution is 1:1-4, and the proportion of alcohol solution shall not be less than 50%, otherwise dissolution will occur, and the mass ratio of propylene glycol esterified modified sodium polyacrylate to alcohol solution addition is 1:1-2.
[0022] Preferably, the alcohol solution is one or more of ethanol solution and isopropanol solution; the acid solution is one or more of citric acid solution and dilute hydrochloric acid solution;
[0023] The mass ratio of the acid solution to the alcohol solution in the acid / alcohol solution is 1:1-4.
[0024] The novel polyacrylamide of the present invention is prepared by the preparation method of the novel polyacrylamide, and the amidation degree of the polyacrylamide is 60%-80%.
[0025] The application of the novel polyacrylamide of the present invention is that the polyacrylamide prepared by the preparation method of the novel polyacrylamide is applied to the preparation of food colloids.
[0026] The present invention provides a novel polyacrylamide and a preparation method and application thereof, which have the following beneficial effects:
[0027] The preparation method of the novel polyacrylamide of the invention comprises the following steps: the polyacrylamide is firstly prepared by polymerizing acrylic acid and sodium hydroxide to produce sodium polyacrylate with different neutralization degrees, esterifying with propylene oxide under nitrogen protection, and then amidating with ammonia alcohol under low temperature conditions to prepare the polyacrylamide; the preparation process involves the synthesis of sodium polyacrylate with different neutralization degrees, esterification in a kneader filled with nitrogen, drying and crushing, ammonia alcohol reaction, neutralization, centrifugation, drying and crushing.
[0028] The production process of polyacrylamide of the invention is scientific and reasonable, and the production process and production raw materials are safe. The use of acrylic acid as a monomer raw material avoids the use of acrylonitrile, a highly toxic and harmful organic substance, in the synthesis of the prior art, and realizes the possibility of applying polyacrylamide in the food field.
[0029] Different amide degrees can be controlled to make it have different properties, and it has a wide range of applications, especially in the food field: when used in flour products, it can improve the water and oil retention properties of the dough and enhance the stability of the oil in the dough. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0031] Example 1
[0032] The preparation method of the novel polyacrylamide of the present invention comprises the following steps:
[0033] (1) Polymerization reaction: 500 g of acrylic acid and 140 g of sodium hydroxide were dissolved in 2500 g of water, and 5 g of sodium sulfite was added. After the self-polymerization reaction was started at 70° C. for 1.5 h, the reaction was centrifuged to make the moisture content of the sodium polyacrylate reach 40% after dehydration.
[0034] (2) Esterification: The sodium polyacrylate treated in step (1) and 420 g of propylene oxide are placed in a kneader, and nitrogen is introduced into the kneader for 10 min. Then, the kneader is turned on under nitrogen protection to carry out esterification reaction for 1 h. The kneader is a self-made device, and the propylene oxide can be vaporized and then cyclically contacted with the sodium polyacrylate for esterification reaction. Under the protection of nitrogen, a high temperature reaction can be carried out, which reduces the reaction time and improves the degree of esterification.
[0035] (3) Cooling: After the esterification reaction is completed, the product is cooled, and when the temperature drops to 20° C. or below, the waste liquid is discharged;
[0036] (4) Hot air treatment: After the waste liquid in the kneader is removed, the kneader is closed and dry hot air is introduced into the kneader. The hot air condition is dry air at 50°C to 70°C to discharge the propylene oxide remaining in the propylene glycol esterified modified sodium polyacrylate;
[0037] (5) Drying: After the hot air treatment in step (4), the propylene glycol esterified modified sodium polyacrylate product is subjected to rapid drying treatment;
[0038] (6) Crushing: The dried product in step (5) is crushed and sieved using a crusher to obtain propylene glycol esterified modified sodium polyacrylate of a desired particle size.
[0039] (7) Amidation: Take the above-mentioned propylene glycol esterified modified sodium polyacrylate, add 600g of an ammonia alcohol solution with an ammonia alcohol ratio of 2:3, wherein the concentration of ammonia water is 1mol / L, carry out an amidation reaction at 20°C for 2h, and control the reaction pH to be greater than or equal to 11; after the reaction is completed, centrifuge, use 100g of an acid alcohol solution with a concentration of 0.5mol / L to wash off the excess ammonia water, and after the pH is adjusted to a neutral 7.2, centrifuge, dry, and crush to obtain an amidated sodium polyacrylate product. The alcohol solution is an ethanol solution; the acid solution is a citric acid solution.
[0040] The polyacrylamide production method can produce a polyacrylamide product with an amide degree of 64.9%.
[0041] Example 2
[0042] The preparation method of the novel polyacrylamide of the present invention comprises the following steps:
[0043] (1) Polymerization reaction: 600 g of acrylic acid and 140 g of sodium hydroxide were dissolved in 2500 g of water, and 5 g of sodium sulfite was added. After the self-polymerization reaction was started at 70° C. for 1 hour, the reaction was centrifuged to make the moisture content of the sodium polyacrylate reach 40% after dehydration.
[0044] (2) Esterification: The sodium polyacrylate treated in (1) and 420 g of propylene oxide were placed in a kneader, nitrogen was introduced into the kneader for 10 min, and then the kneader was started under nitrogen protection to carry out esterification reaction for 1 h;
[0045] (3) Cooling: After the esterification reaction is completed, the product is cooled, and when the temperature drops below 20° C., the waste liquid is discharged;
[0046] (4) Hot air treatment: After the waste liquid in the kneader is removed, the kneader is closed and dry hot air is introduced into the kneader. The hot air condition is dry air at 50°C to 70°C to discharge the propylene oxide remaining in the propylene glycol esterified modified sodium polyacrylate;
[0047] (5) Drying: After the hot air treatment in step (4), the propylene glycol esterified modified sodium polyacrylate product is subjected to rapid drying treatment;
[0048] (6) Crushing: The dried product in step (5) is crushed by a crusher and sieved to obtain propylene glycol esterified modified sodium polyacrylate of a desired particle size.
[0049] (7) Amidation: Take the above-mentioned propylene glycol esterified modified sodium polyacrylate, add 500g of an ammonia alcohol solution with an ammonia alcohol ratio of 2:3, wherein the concentration of ammonia water is 1 mol / L, carry out an amidation reaction at 20°C for 2h, and control the reaction pH to be greater than or equal to 11; after the reaction is completed, centrifuge, use 100g of an acid alcohol solution with a concentration of 0.5 mol / L to wash off the excess ammonia water, and after the pH is adjusted to 7.2, centrifuge, dry, and crush to obtain an amidated sodium polyacrylate product. The alcohol solution is an ethanol solution; the acid solution is a citric acid solution.
[0050] The polyacrylamide production method can produce a polyacrylamide product with an amide degree of 70.6%.
[0051] Example 3
[0052] The preparation method of the novel polyacrylamide of the present invention comprises the following steps:
[0053] (1) Polymerization reaction: 500 g of acrylic acid and 100 g of sodium hydroxide were dissolved in 2500 g of water, and 5 g of sodium sulfite was added to start polymerization. After the self-polymerization reaction started at 70° C. for 1 hour, the mixture was centrifuged to make the moisture content of the sodium polyacrylate reach 40% after dehydration.
[0054] (2) Esterification: The sodium polyacrylate treated in (1) and 420 g of propylene oxide were placed in a kneader, nitrogen was introduced into the kneader for 10 min, and then the kneader was started under nitrogen protection to carry out esterification reaction for 1.5 h;
[0055] (3) Cooling: After the esterification reaction is completed, the product is cooled, and when the temperature drops below 20° C., the waste liquid is discharged;
[0056] (4) Hot air treatment: After the waste liquid in the kneader is removed, the kneader is closed and dry hot air is introduced into the kneader. The hot air condition is dry air at 50°C to 70°C to discharge the propylene oxide remaining in the propylene glycol esterified modified sodium polyacrylate;
[0057] (5) Drying: subjecting the propylene glycol esterified modified sodium polyacrylate product to rapid drying after the hot air treatment in step (4);
[0058] (6) Crushing: The dried product in step (5) is crushed by a crusher and sieved to obtain propylene glycol esterified modified sodium polyacrylate of a desired particle size.
[0059] (7) Amidation: Take the above-mentioned propylene glycol esterified modified sodium polyacrylate, add 400g of an ammonia alcohol solution with an ammonia alcohol ratio of 2:3, wherein the concentration of ammonia water is 1 mol / L, carry out an amidation reaction at 20°C for 1.5h, and control the reaction pH to be greater than or equal to 11; after the reaction is completed, centrifuge, use 100g of an acid alcohol solution with a concentration of 0.5 mol / L to wash off the excess ammonia water, and after the pH is adjusted to a neutral 7.4, centrifuge, dry, and crush to obtain an amidated sodium polyacrylate product. The alcohol solution is an ethanol solution; the acid solution is a citric acid solution.
[0060] The polyacrylamide product prepared by the polyacrylamide production method has an amide degree of 63.8%.
[0061] Example 4
[0062] The preparation method of the novel polyacrylamide of the present invention comprises the following steps:
[0063] (1) Polymerization reaction: 1000 g of acrylic acid and 250 g of sodium hydroxide were dissolved in 4000 g of water, and 8 g of sodium sulfite was added. After starting the self-polymerization reaction at 70° C. for 1.5 h, the mixture was centrifuged to make the moisture content of the sodium polyacrylate reach 40% after dehydration.
[0064] (2) Esterification: The sodium polyacrylate treated in (1) and 600 g of propylene oxide were placed in a kneader, nitrogen was introduced into the kneader for 10 min, and then the kneader was started under nitrogen protection to carry out esterification reaction for 1 h;
[0065] (3) Cooling: After the esterification reaction is completed, the product is cooled, and when the temperature drops to 20° C. or below, the waste liquid is discharged;
[0066] (4) Hot air treatment: After the waste liquid in the kneader is removed, the kneader is closed and dry hot air is introduced into the kneader. The hot air condition is dry air at 50°C to 70°C to discharge the propylene oxide remaining in the propylene glycol esterified modified sodium polyacrylate;
[0067] (5) Drying: subjecting the propylene glycol esterified modified sodium polyacrylate product to rapid drying after the hot air treatment in step (4);
[0068] (6) Crushing: The dried product in step (5) is crushed by a crusher and sieved to obtain propylene glycol esterified modified sodium polyacrylate of a desired particle size.
[0069] (7) Amidation: Take the above-mentioned propylene glycol esterified modified sodium polyacrylate, add 700g of an ammonia alcohol solution with an ammonia alcohol ratio of 2:3, wherein the concentration of ammonia water is 1 mol / L, carry out an amidation reaction at 20°C for 2h, and control the reaction pH to be greater than or equal to 11; after the reaction is completed, centrifuge, use 200g of an acid alcohol solution with a concentration of 0.5 mol / L to wash off the excess ammonia water, and after the pH is adjusted to 7.8, centrifuge, dry, and crush to obtain an amidated sodium polyacrylate product. The alcohol solution is an ethanol solution; the acid solution is a citric acid solution.
[0070] The polyacrylamide production method can produce a polyacrylamide product with an amide degree of 68.7%.
[0071] Example 5
[0072] The preparation method of the novel polyacrylamide of the present invention comprises the following steps:
[0073] (1) Polymerization reaction: 500 g of acrylic acid and 140 g of sodium hydroxide were dissolved in 2500 g of water, and 5 g of sodium sulfite was added. After the self-polymerization reaction was started at 70° C. for 2 h, the reaction was centrifuged to make the moisture content of the sodium polyacrylate reach 40% after dehydration.
[0074] (2) Esterification: The sodium polyacrylate treated in (1) and 400 g of propylene oxide were placed in a kneader, nitrogen was introduced into the kneader for 10 min, and then the kneader was started under nitrogen protection to carry out esterification reaction for 1 h;
[0075] (3) Cooling: After the esterification reaction is completed, the product is cooled, and when the temperature drops to 20° C. or below, the waste liquid is discharged;
[0076] (4) Hot air treatment: After the waste liquid in the kneader is removed, the kneader is closed and dry hot air is introduced into the kneader. The hot air condition is dry air at 50°C to 70°C to discharge the propylene oxide remaining in the propylene glycol esterified modified sodium polyacrylate;
[0077] (5) Drying: subjecting the propylene glycol esterified modified sodium polyacrylate product to rapid drying after the hot air treatment in step (4);
[0078] (6) Crushing: The dried product in step (5) is crushed by a crusher and sieved to obtain propylene glycol esterified modified sodium polyacrylate of a desired particle size.
[0079] (7) Amidation: Take the above-mentioned propylene glycol esterified modified sodium polyacrylate, add 630g of an ammonia-alcohol solution with an ammonia-alcohol ratio of 2:3, wherein the concentration of ammonia water is 1mol / L, carry out an amidation reaction at 20°C for 1.5h, and control the reaction pH to be greater than or equal to 11; after the reaction is completed, centrifuge, use 100g of an acid-alcohol solution with a concentration of 0.5mol / L to wash off the excess ammonia water, and after the pH is adjusted to a neutral pH of 7.1, centrifuge, dry, and crush to obtain an amidated sodium polyacrylate product. The alcohol solution is an ethanol solution; the acid solution is a citric acid solution.
[0080] The polyacrylamide production method above produces a polyacrylamide product with an amide degree of 66.1%.
[0081] In summary, compared with the traditional polyacrylamide synthesis process, the polyacrylamide production process of the present invention is prepared by sodium polyacrylate synthesized from acrylic acid monomers through propylene glycol esterification modification and amino alcohol reaction; wherein, the production process and production raw materials are food-safe, safe acrylic acid is used as the initial raw material, and the production process adopts steam contact and nitrogen protection, thereby avoiding the use of highly toxic and harmful organic matter acrylonitrile. The entire production process provides safety guarantee for its application in the food field, and realizes the possibility of application in food.
[0082] The preparation method of polyacrylamide of the present invention has safer production process and production raw materials, can control different amide degrees to make it have different properties, and is feasible for application in food. When applied to flour products, it can improve the water and oil retention properties of dough and enhance the stability of oil in dough.
[0083] The above are only embodiments of the present invention. For example, the alcohol solution is one or more of ethanol solution and isopropanol solution; the acid solution is one or more of citric acid solution and dilute hydrochloric acid solution, all of which can realize the polyacrylamide and its preparation method and application of the present invention.
[0084] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a novel polyacrylamide, characterized in that: The steps include: Acrylic acid and sodium hydroxide in different proportions are subjected to self-polymerization reaction under the condition of sodium sulfite as an initiator to generate sodium polyacrylates with different acidities, and then esterification reaction is carried out under nitrogen protection conditions; Then, it is subjected to amidation reaction with amino alcohol at low temperature, and after drying, polyacrylamide with different amide degrees is obtained.
2. The method for preparing a novel polyacrylamide according to claim 1, characterized in that: In the preparation method of sodium polyacrylate with different acidities, the molar ratio of the amount of acrylic acid added to sodium hydroxide is 1:1-2; the concentration of the acrylic acid aqueous solution is 15%-20%, and the mass ratio of the amount of sodium sulfite added to acrylic acid is 0.01:1; The reaction temperature in the self-polymerization reaction is 75° C. to 85° C., and the reaction time is 1 h to 2 h.
3. The method for preparing a novel polyacrylamide according to claim 2, characterized in that: The specific steps of the esterification reaction of sodium polyacrylate include the following: (1) Sodium polyacrylate prepared from polymerization reaction; (2) Dehydration: After centrifugation, the water content of the dehydrated sodium polyacrylate is 40% to 50%, which is directly used for the esterification reaction; (3) Esterification: The sodium polyacrylate treated in step (2) and propylene oxide are put into a kneader. Under nitrogen protection, the kneader is turned on for esterification reaction for 1 h to 2 h, and post-treatment is performed to obtain propylene glycol esterified modified sodium polyacrylate.
4. The method for preparing a novel polyacrylamide according to claim 3, characterized in that: The post-processing steps include: (4) Cooling: After the esterification reaction is completed, the product is cooled, and when the temperature drops to 20° C. or below, the waste liquid is discharged; (5) Hot air treatment: After the waste liquid in the kneader is removed, the kneader is closed and dry hot air is introduced into the kneader to remove the propylene oxide remaining in the propylene glycol esterified modified sodium polyacrylate; (6) Drying: subjecting the propylene glycol esterified modified sodium polyacrylate product obtained after the hot air treatment in step (5) to rapid drying; (7) Crushing: The dried product in step (6) is crushed and sieved using a crusher to obtain propylene glycol esterified modified sodium polyacrylate of a desired particle size.
5. A method for preparing a novel polyacrylamide according to claim 4, characterized in that: In the step (3), the weight ratio of the sodium polyacrylate to propylene oxide is 1:0.6-0.8; in the step (5), the hot air condition is dry air at 50°C to 70°C; In the step (3), the kneading machine is a self-made device, which can vaporize propylene oxide and then cyclically contact with sodium polyacrylate to carry out esterification reaction. Under the protection of nitrogen, high-temperature reaction can be carried out to reduce reaction time and improve esterification degree.
6. The method for preparing a novel polyacrylamide according to claim 4, characterized in that: The method comprises subjecting the propylene glycol esterified modified sodium polyacrylate obtained in step (7) to an amidation reaction, and the specific steps are as follows: The propylene glycol esterified modified sodium polyacrylate is added to a mixed solution of ammonia water / alcohol, and stirred continuously. The reaction temperature is 10°C-30°C, the amidation reaction time is 1h-2h, and the reaction pH is controlled to be greater than or equal to 11; after the reaction is completed, centrifugation is performed, and the residual ammonia water is washed away with a 0.5-1 mol / L acid / alcohol solution to neutralize the excess ammonia water. After the pH is adjusted to 7-8, centrifugation, drying, and crushing are performed to obtain polyacrylamide.
7. The method for preparing a novel polyacrylamide according to claim 6, characterized in that: In the ammonia / alcohol mixed solution, the concentration of ammonia is 1-5 mol / L, the mass ratio of ammonia to alcohol solution is 1:1-4, and the mass ratio of the propylene glycol esterified modified sodium polyacrylate to the alcohol solution is 1:1-2.
8. The method for preparing a novel polyacrylamide according to claim 6, characterized in that: The alcohol solution is one or more of ethanol solution and isopropanol solution; the acid solution is one or more of citric acid solution and dilute hydrochloric acid solution; The mass ratio of the acid solution to the alcohol solution in the acid / alcohol solution is 1:1-4.
9. A novel polyacrylamide, characterized in that: The polyacrylamide is prepared by the preparation method of the novel polyacrylamide according to any one of claims 1 to 8, wherein the degree of amidation of the polyacrylamide is 60% to 80%.
10. Application of a novel polyacrylamide, characterized in that: The polyacrylamide prepared by the method for preparing a novel polyacrylamide according to any one of claims 1 to 8 is used in the preparation of food colloids.