Amino metal catalyst composition and method for catalyzing polycondensation of lactic acid monomer and / or synthesis of lactide

By using an amine-based metal catalyst composition, the problems of limited number of catalyst application and product impurities in the polylactic acid synthesis process are solved, and efficient and economical lactide synthesis is achieved, and product purity and process economy are improved.

CN119019668AActive Publication Date: 2024-11-26WANHUA CHEM GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310596250.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

In the existing polylactic acid synthesis process, the number of catalysts is applied is limited, resulting in high cost, high product miscellaneous acid value and color, and the optical purity of traditional industrial catalysts is not high, affecting process economy and product indexes.

Method used

An amine metal catalyst composition is used, including stannous octanoate, 2-[[bis(2-methoxyethyl)amine]methyl]-4,6-bis(1,1-dimethylbenzene ethyl pyruvate (triphenylphosphine)pyruvate, through specific molar ratios and preparation methods, forms an efficient catalyst composition for catalyzing polycondensation of lactic acid monomers and lactide synthesis, improving catalyst stability and selection sex.

Benefits of technology

It significantly enhances the number of times the catalyst is applied and optical purity, reduces the uneven acid value and chromaticity, improves the ring opening conversion rate and product purity of lactide, and enhances the economic and controllability of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004247314140000051
    Figure BDA0004247314140000051
Patent Text Reader

Abstract

The invention discloses an amino metal catalyst composition and a method for catalyzing polycondensation of lactic acid monomers and / or synthesis of lactide, the amino metal catalyst composition comprises the following components: stannous octoate, 2-[[bis (2-methoxyethyl) amino] methyl]-4, 6-bis (1, 2, 4-triazole-1-yl)-1, 2, 4-triazole-1-yl)-1, 2, 4-triazole-1-yl)-1, 2, 4-triazole-1-yl)-1, 2, 4-triazole-1-yl-1, 2, 4-triazole-1-yl the ratio of the 1, 1-dimethyl ethyl) phenol to the dihydroxytoluene to the (triphenylphosphine) ethyl pyruvate is 1: (1.1-3): (1.1-4): (1.1-6). The catalyst composition is used for catalyzing polycondensation of lactic acid monomers and synthesis of lactide, the problem that more D-lactide and MESO-lactide are generated while L-lactide is generated in the existing lactide synthesis process is solved, the heteroacid value in a system can be remarkably reduced, the chromatic value of a lactide product is reduced, the application frequency of a catalyst is increased, and the production cost is reduced. The process economy is obviously enhanced, and the industrial application prospect is relatively strong.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polylactic acid degradable materials, and in particular relates to an amine-based metal catalyst composition and a method for catalyzing the polycondensation of lactic acid monomers and / or the synthesis of lactide. Background Art

[0002] Polylactic acid, also known as polylactide, is a polymer with excellent performance, biocompatibility and biodegradability. It is mainly used in degradable packaging materials, drug microsphere carriers, anti-adhesive films, biological catheters, orthopedic fixations, orthopedic surgical devices, artificial bones, etc.

[0003] Polylactic acid can be synthesized in two ways. One is the direct polycondensation of lactic acid monomers. This method is generally difficult to prepare polymers with high relative molecular mass. The other is a two-step method, that is, first dehydrating and polycondensing lactic acid to obtain lactic acid oligomers, and then undergoing a self-cyclization reaction of the oligomers to synthesize the intermediate product lactide, and then ring-opening polymerization of lactide to generate polylactic acid. This method can obtain a high molecular weight product with a molecular weight of millions through ionic polymerization or coordination polymerization, and thus has become the preferred method for preparing polylactic acid. In the currently developed lactide synthesis process, the process of applying the residual product is one of the key steps to reduce costs. How to reduce costs and increase efficiency in this step and improve the application quality is one of the core directions of optimizing the process. At the same time, developing environmentally friendly synthesis processes and realizing green and environmentally friendly processes to produce polyesters are of great significance to green chemistry. Most of the synthetic processes reported so far focus on the optimization of catalysts. For example, Mehrkhodavandi's group introduced secondary amines or imines to coordinate metal zinc to improve the catalytic activity of the reaction (Inorg. Chem., 2016, 55, 9445-9453). However, most of them do not pay attention to the economic feasibility of product acid value, chromaticity and kettle residue application and their influence on product indicators. In addition, the optical purity of traditional industrial catalysts is not high, and thus the cost is high.

[0004] In view of the above problems, the present invention proposes to add a reaction aid to the existing industrial catalyst to obtain a catalyst composition, which can not only enhance the stability of the catalyst (increase the number of applications) so that it still performs well under high-temperature reaction conditions, but also provide significant enhancement of the selectivity of lactide, and can still ensure high optical purity and low impurity acid content after multiple applications. It is a new method for simply and efficiently preparing lactide materials, which is of great significance for achieving high-activity and high-controllability synthesis of lactones and promoting the development of sustainable polymers. Summary of the invention

[0005] The object of the present invention is to provide an amine-based metal catalyst composition, which can be used to catalyze the polycondensation of lactic acid monomers and / or the synthesis of lactide. In the process of lactide synthesis, the number of times the catalyst is applied can be increased, the heteroacid value of the reaction product can be reduced, the monomer polycondensation and oligomer cyclization reactions can be significantly promoted, and in particular, the occurrence of side reactions in the cyclization process can be inhibited, and the lactide ring-opening conversion rate can be increased.

[0006] Another object of the present invention is to provide a method for using the amino metal catalyst composition for polycondensation of lactic acid monomer and / or synthesis of lactide, which has the advantages of high reaction activity, high product purity and high raw material conversion rate.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solution:

[0008] The invention discloses an amine-based metal catalyst composition, which comprises the following components: stannous octoate, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate.

[0009] In a specific embodiment, the molar ratio of each component is stannous octoate: 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol: dihydroxytoluene: (triphenylphosphine)ethyl pyruvate = 1: (1.1-3): (1.1-4): (1.1-6).

[0010] In a specific embodiment, the amine-based metal catalyst composition is prepared by the following steps: adding stannous octoate, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate into a reactor, and introducing a solvent under the protection of an inert gas, stirring the mixture to react and reflux, and removing excess solvent to obtain the amine-based metal catalyst composition; preferably, the solvent is selected from acetone, lactic acid, toluene, tetrahydrofuran or ethylene glycol dimethyl ether, preferably lactic acid or acetone.

[0011] In a specific embodiment, the molar ratio of stannous octoate, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate is 1:(1.1-1.5):(1.1-2):(1.1-4).

[0012] In a specific embodiment, the reaction temperature of the mixture stirring reaction is 40-60° C., and the reaction time is 1-6 hours.

[0013] In a specific embodiment, the reaction temperature of the mixture stirring reaction is 50-55° C., and the reaction time is 1-2 hours.

[0014] On the other hand, a method for catalyzing the polycondensation of lactic acid monomers and / or the synthesis of lactide, wherein the catalyst comprises the aforementioned amine-based metal catalyst composition; preferably, the catalyst is the aforementioned amine-based metal catalyst composition.

[0015] In a specific embodiment, in the polycondensation stage of lactic acid monomer, the reaction temperature is 140-170°C, preferably 150-160°C, the reaction pressure is 30-50 hPa, and the reaction time is 0.5-3 h.

[0016] In a specific embodiment, in the lactide synthesis stage, the reaction temperature is 140-200°C, preferably 150-160°C, the reaction pressure is 10-25 hPa, and the reaction time is 0.5-1 h.

[0017] In a specific embodiment, the amount of the amine-based metal catalyst composition added in the catalytic lactic acid monomer condensation and / or lactide synthesis stage is 0.1% to 1%, preferably 0.4% to 1%, based on the mass of stannous octoate in the amine-based metal catalyst composition accounting for 87wt% of the lactic acid aqueous solution added to the reaction.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The amine-based metal catalyst composition of the present invention is used for polycondensation of lactic acid monomers and / or synthesis of lactide, and can significantly inhibit the generation of D-, MESO-lactide during the reaction process, and convert it into L-lactide, thereby solving the problem that a large amount of D-, MESO-lactide is generated along with the generation of L-lactide during the existing lactide synthesis process; in addition, it can also significantly reduce the impurity acid value in the system, reduce the chromaticity value, increase the number of catalyst applications, significantly enhance the process economy, and have prospects for industrial scale-up. DETAILED DESCRIPTION

[0020] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0021] The amine-based metal catalyst composition of the present invention is used for polycondensation of lactic acid monomers and / or lactide synthesis reaction, replacing the metal catalyst in the prior art. In the amine-based metal catalyst composition, the material components and molar ratios are stannous octoate: 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol: dihydroxytoluene: (triphenylphosphine)ethyl pyruvate=1:(1.1-3):(1.1-4):(1.1-6), for example, 1:1.1:1.1:1.1, 1:1.2:1.5:1.5, 1:1.3:1.8:2, 1:1.5:1.1:2, 1:1.5:2:4, 1:2:3:5, 1:3:4:6, etc.

[0022] Among them, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, also known as {phenol, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl}, has a CAS number of 870680-83-4, and its supplier is, for example, Chemieliva Pharmaceutical, etc. The structural formula is as follows:

[0023]

[0024] The invention prepares an amine-based metal catalyst composition by pretreating a stannous octoate metal catalyst with 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate. Compared with the metal catalyst used in the prior art, the invention uses N and O electron-donating groups to improve the catalytic stability of the catalyst and regulate the charge distribution at the reaction point, so that Sn 2+ It is easier to induce the carbonyl group to bite into a ring; at the same time, it is speculated that the steric hindrance formed by the composition can well control the methyl form of lactide during the ring formation process, which is beneficial to inhibit the formation reaction of R-lactide and M-lactide.

[0025] Furthermore, the preparation method of the amine-based metal catalyst composition comprises the following steps: adding stannous octoate, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate into a reactor in a molar ratio of 1:(1.1-3):(1.1-4):(1.1-6), and introducing lactic acid as a solvent under the protection of an inert gas, stirring the mixture to react and reflux, and then drying and evaporating the excess solvent to obtain the amine-based metal catalyst composition.

[0026] Wherein, the addition of solvent lactic acid is based on fully dissolving each component, and there is no particular restriction, and excessive does not affect, and subsequent post-processing can be spin-dried to remove excess solvent. The mixed solution formed by the aforementioned mixture and the solvent is stirred to react and refluxed, and the reaction temperature is 40~60 ℃, such as 41 ℃, 42 ℃, 43 ℃, 44 ℃, 45 ℃, 46 ℃, 47 ℃, 48 ℃, 49 ℃, 50 ℃, 51 ℃, 52 ℃, 53 ℃, 54 ℃, 55 ℃, 56 ℃, 57 ℃, 58 ℃, 59 ℃, 60 ℃, etc., preferably 50~55 ℃, and the reaction time is 1~6h, such as 1h, 1.5h, 2h, 3h, 4h, 5h, 6h, etc., preferably 1~2h.

[0027] The present invention also provides the use of the amino-metal catalyst composition for catalyzing the polycondensation of lactic acid monomers and the synthesis of lactide, that is, in the process of catalyzing the polycondensation of lactic acid monomers and the synthesis of lactide, the amino-metal catalyst composition of the present invention is used to replace the metal catalyst in the prior art. For other matters not specifically described, reference can be made to the prior art, such as CN202210876468.1. The relevant contents in the prior art of polycondensation of lactic acid monomers and synthesis of lactide can be introduced into the present invention, which can be understood by those skilled in the art.

[0028] Specifically, in the lactic acid condensation stage, the amount of the amine-based metal catalyst composition added is 0.1% to 1%, based on the mass of stannous octoate in the amine-based metal catalyst composition accounting for 87wt% of the lactic acid aqueous solution added to the reaction, for example, the amount added is 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, etc., preferably 0.4wt% to 1wt%; wherein, 87wt% of the lactic acid aqueous solution is usually added as a raw material in the lactide preparation reaction, and the amount of the amine-based metal catalyst composition added of the present invention is based on the mass of stannous octoate contained therein accounting for 87wt% of the lactic acid aqueous solution added to the reaction. The reaction temperature is 140-170°C, for example, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, etc., preferably 150°C-160°C, the reaction pressure is 30-50hPa, for example, 30hPa, 35hPa, 40hPa, 45hPa, 50hPa, etc., and the reaction time is 0.5-3h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, etc.

[0029] In actual production, the second step of lactide synthesis is usually carried out by continuing to heat up the lactic acid polycondensation reaction product in the first step. In this process, there is no need to repeatedly add the amino metal catalyst composition of the present invention in the second step.

[0030] In an independent process for synthesizing lactide, the amount of the amino metal catalyst composition added is 0.1% to 1%, based on the mass of stannous octoate in the catalyst composition to the lactic acid aqueous solution (87wt%) added in the first step reaction; the reaction temperature is 140 to 200°C, for example, 140°C, 150°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, etc., preferably 150°C to 160°C, the reaction pressure is 10 to 25hPa, for example, 10hPa, 15hPa, 20hPa, 25hPa, etc., and the reaction time is 0.5 to 1h, for example, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, etc.

[0031] By using the amine-based metal catalyst composition of the present invention as a catalyst, the optical purity of crude lactide obtained in the lactide reaction process under optimal conditions can reach 97.8-99.9%, which is higher than 90% in the prior art.

[0032] The present invention is further explained below by more specific examples, but does not constitute any limitation.

[0033] The analytical test methods involved in the following implementation are as follows:

[0034] 1) GPC test molecular weight and distribution

[0035] GPC measurements were performed on a LC-20AD solvent delivery pump, a Wyatt OPTILAB rEX refractive index detector and a combination of Styragel P8512-10E3A10, P8512-10E4A10 and P8512-10E5A10, with effective molar mass ranges of 100 to 40,000, 400 to 500,000 and 10,000 to 2,000,000, respectively. THF was used as the eluent (flow rate 1 mL min1, T = 40°C).

[0036] 2) GC test of impurity acid content

[0037] Agilent6820 gas chromatograph, chromatographic column: OV-1 capillary column (50m*0.25mm); column temperature: (programmed temperature rise) initial temperature 129℃, hold for 4min, heating rate 0.5℃ / min, end temperature 132℃, hold for 35min; vaporization temperature: 280℃; detector temperature: 250℃; split ratio: 80:1; carrier gas: high-purity hydrogen, pressure 0.1MPa; tail gas: 29ml / min; injection mode: split injection; injection volume: 0.2uL.

[0038] 3.) Chroma detection: Liquid colorimeter - CRED D040 colorimeter (high-precision platinum-cobalt Gardner colorimeter). The platinum-cobalt colorimeter is expressed in Hazen units with a numerical range of 1 to 500.

[0039] Preparation Example 1 Amine Metal Catalyst Composition 1

[0040] Stannous octoate: 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol: dihydroxytoluene: (triphenylphosphine)ethyl pyruvate = 0.003:0.0033:0.006:0.0033 (molar ratio) are added sequentially into 150 mL of acetone solution, heated to 50°C, refluxed and stirred for 1 hour, and then the excess solvent is dried to obtain 3.9 g of light yellow liquid, which is added to lactic acid solution to prepare 15.7 g of a 25wt% solution for standby use as composition solution 1.

[0041] Preparation Example 2 Amine Metal Catalyst Composition 2

[0042] Stannous octoate: 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol: dihydroxytoluene: (triphenylphosphine)ethyl pyruvate = 0.003:0.0045:0.0033:0.012 (molar ratio) are added sequentially into 150 mL of lactic acid solution, heated to 55°C, refluxed and stirred for 5 hours, and then the excess solvent is dried to obtain 6.9 g of light yellow liquid, which is added to lactic acid solution to prepare 27.8 g of a 25wt% solution for later use as composition solution 2.

[0043] Preparation Example 3 Amine Metal Catalyst Composition 3

[0044] Stannous octoate: 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol: dihydroxytoluene: (triphenylphosphine)ethyl pyruvate = 0.007:0.0105:0.0077:0.028 (molar ratio) are added sequentially into 150 mL of lactic acid solution, heated to 55°C, refluxed with stirring for 5 hours, and then the excess solvent is dried to obtain 16.22 g of light yellow liquid, which is added to lactic acid solution to prepare 64.91 g of a 25wt% solution for later use as composition solution 3.

[0045] Example 1

[0046] The condensation reaction and the lactide synthesis reaction are as follows: 300g of L-lactic acid aqueous solution (87wt%) are added to a 1L prepolymerization reactor, the system temperature is raised to 150°C, the pressure is 50hpa, and the water content is detected to be less than 1%; subsequently, 15.7g (the content of stannous octoate in the composition accounts for about 0.4wt% of the reaction raw material lactic acid aqueous solution) of the prepared amino metal catalyst composition 1 solution is added, the reaction system is heated to 170°C, the system pressure is 30hpa, and the reaction is carried out for 60min. The molecular weight distribution of the lactic acid oligomer obtained by the prepolymerization reaction is about 1500, and the distribution coefficient is 1.31; finally, the prepolymerization reaction liquid is taken out and placed in a depolymerization reactor, the temperature is raised to 150°C, the system pressure is 25hpa, and the reaction is carried out for 1h to obtain crude lactide with an optical purity of 99.5%, an acid value of 80.4ppm, and a chromaticity of 32hazen.

[0047] Example 2

[0048] The condensation reaction and lactide synthesis reaction are as follows: 300g L-lactic acid aqueous solution (87wt%) are added to a 1L prepolymerization reactor, the system temperature is raised to 150°C, the pressure is 50hPa, and dehydration is carried out for 30min, and the water content is detected to be less than 1%; subsequently, 27.8g (the content of stannous octoate in the composition accounts for about 0.4wt% of the reaction raw material lactic acid aqueous solution) of the prepared amino metal catalyst composition 2 solution is added, the temperature is kept constant, the system pressure is 50hPa, and the reaction is carried out for 3h. The molecular weight distribution of the lactic acid oligomer obtained by the prepolymerization reaction is about 1500, and the distribution coefficient is 1.4; finally, the prepolymerization reaction liquid is taken out and placed in a depolymerization reactor, the temperature is raised to 200°C, the system pressure is 10hPa, and the reaction is carried out for 30min to obtain crude lactide with an optical purity of 99.5%, an acid value of 137ppm, and a chromaticity of 24hazen.

[0049] Example 3

[0050] The condensation reaction and the lactide synthesis reaction are as follows: 300g of L-lactic acid aqueous solution (87wt%) are added into a 1L prepolymerization reactor, the system temperature is raised to 150°C, the pressure is 50hpa, dehydration is carried out for 30min, and the water content is detected to be less than 1%; subsequently, 64.91g of the prepared amino metal catalyst composition 3 solution (the stannous octoate content in the composition accounts for about 0.4wt% of the reaction raw material lactic acid aqueous solution) is added, the reaction system is heated to 160°C, the system pressure is 30hpa, the reaction is carried out for 0.5h, the molecular weight distribution of the lactic acid oligomer obtained by the prepolymerization reaction is about 1000, and the distribution coefficient is 1.04; finally, the prepolymerization reaction liquid is taken out and placed in a depolymerization reactor, the temperature is raised to 160°C, the system pressure is 10hpa, and the reaction is carried out for 30min to obtain crude lactide with an optical purity of 99.2%, an acid value of 54ppm, and a chromaticity of 17hazen.

[0051] Embodiment 4 (application test)

[0052] In the lactide synthesis reaction process of Example 1, when 190 g of lactide was distilled out of the reactants, the reaction was stopped, and 256 g of lactic acid solution was added to the kettle residue for each reaction. After 10 cycles, the optical purity of the distilled lactide was tested, and the optical purity of the crude lactide obtained was 97.4%, the acid value was 172 ppm, and the chromaticity was 54 hazen.

[0053] Comparative Example 1 (Compared with Example 2)

[0054] The condensation reaction and the lactide synthesis reaction are as follows: 300g of L-lactic acid aqueous solution (87wt%) are added to a 1L prepolymerization reactor, the system temperature is raised to 150°C, the pressure is 50hpa, dehydration is carried out for 30min, and the water content is detected to be less than 1%; subsequently, 4.86g of lactic acid solution (the lactic acid solution is prepared from 1.2g of stannous octoate as a 25wt% lactic acid solution; wherein the content of stannous octoate accounts for about 0.4wt% of the reaction raw material lactic acid aqueous solution) is added, the temperature is kept constant, the system pressure is 50hpa, the reaction is carried out for 3h, the molecular weight distribution of the lactic acid oligomer obtained by the prepolymerization reaction is about 1500, and the distribution coefficient is 2.1; finally, the prepolymerization reaction liquid is taken out and placed in a depolymerization reactor, the temperature is raised to 200°C, the system pressure is 10hpa, and the reaction is carried out for 30min to obtain crude lactide with an optical purity of 90.5%, an acid value of 372ppm, and a chromaticity of 52hazen.

[0055] Comparative Example 2 (Application Test)

[0056] In the lactide synthesis reaction process of the comparative example 1, the reaction was stopped when 190 g of lactide was distilled out of the reactants, and 256 g of lactic acid solution was added to the kettle residue for application. After 10 cycles, the optical purity of the distilled lactide was tested, and the optical purity of the crude lactide obtained was 87.3%, the acid value was 753 ppm, and the chromaticity was 172 hazen.

[0057] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. An amine-based metal catalyst composition, It is characterized in that The amine-based metal catalyst composition comprises the following components: stannous octoate, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate.

2. The amine-based metal catalyst composition according to claim 1, It is characterized in that The molar ratio of each component is stannous octoate: 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol: dihydroxytoluene: (triphenylphosphine) ethyl pyruvate = 1: (1.1-3): (1.1-4): (1.1-6).

3. The amine-based metal catalyst composition according to claim 1 or 2, It is characterized in that The amine-based metal catalyst composition is prepared by the following steps: adding stannous octoate, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate into a reactor, introducing a solvent under the protection of an inert gas, stirring the mixture for reaction and refluxing, and removing excess solvent to obtain the amine-based metal catalyst composition; preferably, the solvent is selected from acetone, lactic acid, toluene, tetrahydrofuran or ethylene glycol dimethyl ether, preferably lactic acid or acetone.

4. The amine-based metal catalyst composition according to claim 2, It is characterized in that The molar ratio of stannous octoate, 2-[[bis(2-methoxyethyl)amino]methyl]-4,6-bis(1,1-dimethylethyl)phenol, dihydroxytoluene and ethyl (triphenylphosphine)pyruvate is 1:(1.1-1.5):(1.1-2):(1.1-4).

5. The amine-based metal catalyst composition according to claim 3, It is characterized in that The reaction temperature of the mixture is 40-60° C. and the reaction time is 1-6 hours.

6. The amine-based metal catalyst composition according to claim 5, It is characterized in that The reaction temperature of the mixture is 50-55° C. and the reaction time is 1-2 hours.

7. A method for catalyzing the polycondensation of lactic acid monomers and / or the synthesis of lactide, It is characterized in that The catalyst comprises the amine metal catalyst composition according to any one of claims 1 to 6.

8. The method according to claim 7, It is characterized in that In the polycondensation stage of lactic acid monomer, the reaction temperature is 140-170°C, preferably 150-160°C, the reaction pressure is 30-50 hPa, and the reaction time is 0.5-3 h.

9. The method according to claim 7, It is characterized in that In the lactide synthesis stage, the reaction temperature is 140-200°C, preferably 150-160°C, the reaction pressure is 10-25hpa, and the reaction time is 0.5-1h.

10. The method according to any one of claims 7 to 10, It is characterized in that The amount of the amine-based metal catalyst composition added in the catalytic polycondensation of lactic acid monomers and / or the lactide synthesis stage is 0.1% to 1%, preferably 0.4% to 1%, based on the mass of stannous octoate in the amine-based metal catalyst composition accounting for 87wt% of the lactic acid aqueous solution added to the reaction.

Citation Information

Patent Citations

  • Catalyst / initiator system

    CN101817923A

  • Diamine-based metal catalyst as well as preparation method and application thereof

    CN114349941A

  • Mixed catalyst systems and methods of using the same

    WO2018075245A1