Low-thermal-conductivity epoxy resin composition and preparation method of glass cloth laminated board

By hot-pressing forming of low thermal conductivity epoxy resin composition and glass cloth, the problem of insufficient thermal conductivity of the existing epoxy glass cloth laminate was solved, and a low thermal conductivity epoxy glass cloth layer that meets the requirements of new energy battery packs was prepared. Pressure plate, with excellent heat and flame retardant properties.

CN119019811APending Publication Date: 2024-11-26SICHUAN D&F ELECTRICAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411012822.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The thermal conductivity of the existing epoxy glass cloth laminate cannot meet the requirements of the thermal conductivity of the epoxy resin separator for new energy battery packs less than 0.20W/(m K).

Method used

The preparation method of low thermal conductivity epoxy resin composition includes synthesizing epoxy resin, curing agent, catalyst, high-strength hollow foam resin powder and aluminum hydroxide, and hot-pressing it with a glass cloth to prepare Epoxy glass cloth laminate with thermal conductivity below 0.20W/(m K).

Benefits of technology

The prepared epoxy glass cloth laminate has excellent humidity and heat resistance, flame retardant performance and halogen-free flame retardant performance, meets the thermal conductivity requirements of new energy battery packs, and retains the bending strength under high temperature and humidity conditions. The rate reaches more than 85%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019811A_ABST
    Figure CN119019811A_ABST
Patent Text Reader

Abstract

The invention discloses a low-thermal-conductivity epoxy resin composition and a preparation method of a glass cloth laminated board, and relates to the technical field of laminated boards, and the preparation method comprises the following steps: adding 100 parts by weight of epoxy resin and 20-40 parts by weight of a curing agent into a reaction kettle, starting the reaction kettle for stirring and heating, and after the temperature of the materials in the reaction kettle is raised to 110-130 DEG C, cooling to room temperature to obtain the low-thermal-conductivity epoxy resin composition. The preparation method comprises the following steps: reacting for 1-3 hours, sequentially adding a solvent, 0.5-3.0 parts by weight of a catalyst, 40-90 parts by weight of high-strength hollow foaming resin powder and 100-150 parts by weight of aluminum hydroxide when the temperature of materials in a reaction kettle is reduced to 40-60 DEG C, and stirring at a high speed through the reaction kettle, the problem that the epoxy resin glass cloth laminated board prepared by the existing preparation method of the epoxy resin glass cloth laminated board cannot meet the heat conductivity coefficient requirement of the epoxy resin partition board for the new energy battery pack during use is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laminated boards, and in particular to a low thermal conductivity epoxy resin composition and a method for preparing a glass cloth laminated board. Background Art

[0002] New energy battery packs usually use insulating separators to isolate the positive and negative electrodes to prevent short circuits and mutual interference between battery components. Insulating separators can play the role of electrical isolation, flame retardancy and high temperature resistance, ensuring the safe and stable operation of the battery pack. Common materials used to make insulating separators include epoxy resin, plastic, polyimide, etc. Epoxy resin separators have excellent electrical insulation properties, mechanical strength and heat resistance, and are suitable for high temperature environments in new energy battery packs.

[0003] At present, epoxy resin separators in new energy battery packs generally refer to epoxy glass cloth laminates. Epoxy glass cloth laminates are made by impregnating glass cloth with modified epoxy resin solution, baking at high temperature to obtain prepreg, and then laminating and hot pressing. The thermal conductivity of this type of epoxy glass cloth laminate is above 0.35W / (m K), which currently cannot meet the requirement that the thermal conductivity of epoxy resin separators for new energy battery packs is less than 0.20W / (m K).

[0004] In the invention with application number: CN201310354024.2 and publication number: CN103465556B, a manufacturing process of epoxy glass cloth laminate is disclosed, which includes the following steps: immersing glass cloth in a paint tank containing epoxy resin and gluing it through a gluing furnace, wherein the glass cloth is a coarse cloth type glass cloth; placing the glued glass cloth into a tempering furnace for curing treatment; cutting the cured glass cloth at equal distances according to actual length requirements; stacking the cut glass cloths, and according to different thickness requirements, using steel plates to longitudinally separate the stacked glass cloths to complete the panel matching; using a press to press the glass cloths separated by the steel plates to obtain an epoxy glass cloth laminate. The epoxy resin glass cloth laminate prepared by the epoxy resin glass cloth laminate still cannot meet the thermal conductivity requirements of epoxy resin separators for new energy battery packs. Summary of the invention

[0005] Based on this, in order to solve the above problems, the present invention proposes a low thermal conductivity epoxy resin composition and a glass cloth laminate preparation method, which solves the problem that the epoxy resin glass cloth laminate prepared by the current epoxy resin glass cloth laminate preparation method cannot meet the thermal conductivity requirements of the epoxy resin separator for new energy battery packs when used.

[0006] The technical solution of the present invention is:

[0007] A method for preparing a low thermal conductivity epoxy resin composition comprises the following steps:

[0008] Step S1: 100 parts by weight of epoxy resin and 20 to 40 parts by weight of curing agent are added into a reaction kettle, and the reaction kettle is opened for stirring and heating. After the temperature of the materials in the reaction kettle rises to 110 to 130° C., the reaction is carried out for 1 to 3 hours;

[0009] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0010] Step S2: when the temperature of the material in the reaction kettle drops to 40-60° C., a solvent, 0.5-3.0 parts by weight of a catalyst, 40-90 parts by weight of a high-strength hollow foamed resin powder, and 100-150 parts by weight of aluminum hydroxide are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0011] The solid content of the low thermal conductivity epoxy resin composition is 60%.

[0012] Preferably, in step S1, the epoxy resin is any one of phenolic phosphorus-containing epoxy resin, dicyclopentadiene phosphorus-containing epoxy resin or o-cresol phosphorus-containing epoxy resin, or a mixture of the two in any ratio.

[0013] Preferably, in step S1, the curing agent is any one of 4,4'-diaminodiphenylmethane DDM, 4,4'-diaminodiphenyl sulfone DDS or meta-xylylenediamine.

[0014] Preferably, in step S2, the catalyst is any one of 2-methylimidazole and 2-ethyl-4-methylimidazole, or a mixture of the two in any ratio.

[0015] Preferably, in step S2, the high-strength hollow foamed resin powder is any one of benzoxazine resin hollow powder and phenolic resin hollow powder, or a mixture of the two in any ratio.

[0016] Preferably, in step S2, the particle size of the high-strength hollow foamed resin powder is any one or two of 30 μm, 40 μm or 50 μm.

[0017] Preferably, in step S2, the particle size specification of aluminum hydroxide is any one or two of 3 μm, 5 μm or 8 μm.

[0018] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0019] A1: Install the glass cloth on the vertical impregnation and drying production line, and heat the temperature in the vertical oven in the vertical impregnation and drying production line to 160±10℃;

[0020] Among them, the weight specification of glass cloth is 210g / m 2 , 180g / m 2 or 140g / m 2 Either or both of the following:

[0021] A2: injecting the low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above into a dipping device in a vertical dipping and drying production line, and manufacturing a glass cloth prepreg at a speed of 5 to 8 m / min, and then cutting the manufactured glass cloth prepreg into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0022] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0023] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0024] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0025] Preferably, in step A4, the weight composition of the prepared low thermal conductivity epoxy glass cloth laminate is 50% to 55% glass cloth and 45% to 50% low thermal conductivity epoxy resin composition.

[0026] Preferably, in step A4, the thermal conductivity of the low thermal conductivity epoxy glass cloth laminate prepared is lower than 0.20 W / (m K).

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The low thermal conductivity epoxy glass cloth laminate prepared by the present invention has excellent moisture and heat resistance stability. After 1000 hours of testing under the conditions of temperature 85°C and humidity 85%, its bending strength retention rate reaches more than 85%.

[0029] 2. The low thermal conductivity epoxy glass cloth laminate prepared by the present invention has excellent flame retardant properties. At the same time, the low thermal conductivity epoxy glass cloth laminate prepared by the present invention realizes the halogen-free flame retardant properties of the laminate, and its vertical flammability level reaches FV0.

[0030] 3. The low thermal conductivity epoxy glass cloth laminate prepared by the present invention has a low thermal conductivity. The thermal conductivity of the low thermal conductivity epoxy glass cloth laminate prepared by the present invention is lower than 0.20W / (m K), which meets the requirement that the thermal conductivity of the epoxy resin separator for new energy battery packs is less than 0.20W / (m K). BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic structural diagram of the vertical impregnation and drying production line described in an embodiment of the present invention;

[0032] Figure 2 The structure of the dipping device described in the embodiment of the present invention is schematically shown in FIG. Figure 1 ;

[0033] Figure 3 It is a schematic diagram of the local structure of the dipping device described in the embodiment of the present invention Figure 1 ;

[0034] Figure 4 The structure of the dipping device described in the embodiment of the present invention is schematically shown in FIG. Figure 2 ;

[0035] Figure 5 It is a schematic diagram of the local structure of the dipping device described in the embodiment of the present invention Figure 2 ;

[0036] Description of reference numerals:

[0037] 10-glass cloth unwinding machine, 20-front cloth storage device, 30-impregnation device, 300-installation bracket, 301-first roller body, 302-second roller body, 303-third roller body, 304-fourth roller body, 305-auxiliary rotating rod, 306-liquid storage tank, 307-driving assembly, 308-worm gear, 309-worm, 310-rotating motor, 311-motor bracket, 312-rotating seat, 313-protective cover, 314-inclined surface, 315-flow trough, 316-liquid supply pipe, 317-liquid discharge pipe, 318-valve, 319-baffle, 40-vertical oven, 50-deviation adjustment machine, 60-traction machine, 70-edge cutting machine, 80-rear cloth storage device, 90-glass cloth winding machine. DETAILED DESCRIPTION

[0038] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0039] Example:

[0040] This embodiment discloses a method for preparing a low thermal conductivity epoxy resin composition, comprising the following steps:

[0041] Step S1: 100 parts by weight of epoxy resin and 20 to 40 parts by weight of curing agent are added into a reaction kettle, and the reaction kettle is opened for stirring and heating. After the temperature of the materials in the reaction kettle rises to 110 to 130° C., the reaction is carried out for 1 to 3 hours;

[0042] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0043] Step S2: when the temperature of the material in the reaction kettle drops to 40-60° C., a solvent, 0.5-3.0 parts by weight of a catalyst, 40-90 parts by weight of a high-strength hollow foamed resin powder, and 100-150 parts by weight of aluminum hydroxide are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0044] The solid content of the low thermal conductivity epoxy resin composition is 60%.

[0045] Preferably, in step S1, the epoxy resin is any one of phenolic phosphorus-containing epoxy resin, dicyclopentadiene phosphorus-containing epoxy resin or o-cresol phosphorus-containing epoxy resin, or a mixture of the two in any ratio.

[0046] Preferably, in step S1, the curing agent is any one of 4,4'-diaminodiphenylmethane DDM, 4,4'-diaminodiphenyl sulfone DDS or meta-xylylenediamine.

[0047] Preferably, in step S2, the catalyst is any one of 2-methylimidazole and 2-ethyl-4-methylimidazole, or a mixture of the two in any ratio.

[0048] Preferably, in step S2, the high-strength hollow foamed resin powder is any one of benzoxazine resin hollow powder and phenolic resin hollow powder, or a mixture of the two in any ratio.

[0049] Preferably, in step S2, the particle size of the high-strength hollow foamed resin powder is any one or two of 30 μm, 40 μm or 50 μm.

[0050] Preferably, in step S2, the particle size specification of aluminum hydroxide is any one or two of 3 μm, 5 μm or 8 μm.

[0051] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0052] A1: Install the glass cloth on the vertical impregnation drying production line, and heat the temperature in the vertical oven 40 in the vertical impregnation drying production line to 160±10°C;

[0053] Among them, the weight specification of glass cloth is 210g / m 2 , 180g / m 2 or 140g / m 2 Either or both of the following:

[0054] A2: injecting the low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above into the dipping device 30 in the vertical dipping and drying production line, and manufacturing the glass cloth prepreg at a speed of 5 to 8 m / min, and then cutting the manufactured glass cloth prepreg into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0055] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0056] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0057] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0058] Preferably, in step A4, the weight composition of the prepared low thermal conductivity epoxy glass cloth laminate is 50% to 55% glass cloth and 45% to 50% low thermal conductivity epoxy resin composition.

[0059] Preferably, in step A4, the thermal conductivity of the low thermal conductivity epoxy glass cloth laminate prepared is lower than 0.20 W / (m K).

[0060] 1. The low thermal conductivity epoxy glass cloth laminate prepared by the present invention has excellent moisture and heat resistance stability. After 1000 hours of testing under the conditions of temperature 85°C and humidity 85%, its bending strength retention rate reaches more than 85%.

[0061] 2. The low thermal conductivity epoxy glass cloth laminate prepared by the present invention has excellent flame retardant properties. At the same time, the low thermal conductivity epoxy glass cloth laminate prepared by the present invention realizes the halogen-free flame retardant properties of the laminate, and its vertical flammability level reaches FV0.

[0062] 3. The low thermal conductivity epoxy glass cloth laminate prepared by the present invention has a low thermal conductivity. The thermal conductivity of the low thermal conductivity epoxy glass cloth laminate prepared by the present invention is lower than 0.20W / (m K), which meets the requirement that the thermal conductivity of the epoxy resin separator for new energy battery packs is less than 0.20W / (m K).

[0063] The present invention realizes the halogen-free flame retardant performance of the laminated board through the synthesis of the low thermal conductivity epoxy resin composition and the PA l(OH)3 synergistic flame retardant technology, and the vertical flammability level thereof reaches FV0.

[0064] The present invention realizes the low thermal conductivity of epoxy glass cloth laminates through the dispersion composite technology of high-strength hollow foamed resin powder and phosphorus-containing epoxy resin. The thermal conductivity of the obtained low thermal conductivity epoxy glass cloth laminate is lower than 0.20W / (mK), which meets the requirement that the thermal conductivity of insulating partitions for new energy battery packs is less than 0.20W / (mK).

[0065] Embodiment 1:

[0066] Process for preparing low thermal conductivity epoxy resin composition:

[0067] A method for preparing a low thermal conductivity epoxy resin composition comprises the following steps:

[0068] Step S1: 100 parts by weight of phenolic phosphorus-containing epoxy resin and 30 parts by weight of DDS are added into a reactor, and the reactor is opened for stirring and heating. After the temperature of the materials in the reactor rises to 110-130° C., the reaction is carried out for 2 hours;

[0069] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0070] Step S2: when the temperature of the material in the reactor drops to 40-60° C., toluene, 1.2 parts by weight of 2-methylimidazole, 60 parts by weight of high-strength benzoxazine hollow foaming resin powder with a particle size of 40 μm, and 125 parts by weight of aluminum hydroxide with a particle size of 5 μm are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0071] Preparation process of glass cloth prepreg and low thermal conductivity epoxy glass cloth laminate:

[0072] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0073] A1: Install the glass cloth on the vertical impregnation drying production line, and heat the temperature in the vertical oven 40 in the vertical impregnation drying production line to 160±10°C;

[0074] Among them, the weight specification of glass cloth is 180g / m 2 ;

[0075] A2: The low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above is injected into the dipping device 30 in the vertical dipping and drying production line, and the glass cloth prepreg is manufactured at a vehicle speed, i.e., a line speed of 5 to 8 m / min, and then the manufactured glass cloth prepreg is cut into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0076] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0077] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0078] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0079] Embodiment 2:

[0080] Process for preparing low thermal conductivity epoxy resin composition:

[0081] A method for preparing a low thermal conductivity epoxy resin composition comprises the following steps:

[0082] Step S1: 100 parts by weight of phenolic phosphorus-containing epoxy resin and 40 parts by weight of DDS are added into a reactor, and the reactor is opened for stirring and heating. After the temperature of the materials in the reactor rises to 110-130° C., the reaction is carried out for 2 hours;

[0083] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0084] Step S2: when the temperature of the material in the reactor drops to 40-60° C., toluene, 1.2 parts by weight of 2-methylimidazole, 60 parts by weight of high-strength benzoxazine hollow foaming resin powder with a particle size of 40 μm, and 125 parts by weight of aluminum hydroxide with a particle size of 5 μm are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0085] Preparation process of glass cloth prepreg and low thermal conductivity epoxy glass cloth laminate:

[0086] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0087] A1: Install the glass cloth on the vertical impregnation drying production line, and heat the temperature in the vertical oven 40 in the vertical impregnation drying production line to 160±10°C;

[0088] Among them, the weight specification of glass cloth is 140g / m 2 ;

[0089] A2: The low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above is injected into the dipping device 30 in the vertical dipping and drying production line, and the glass cloth prepreg is manufactured at a vehicle speed, i.e., a line speed of 5 to 8 m / min, and then the manufactured glass cloth prepreg is cut into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0090] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0091] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0092] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0093] Embodiment 3:

[0094] Process for preparing low thermal conductivity epoxy resin composition:

[0095] A method for preparing a low thermal conductivity epoxy resin composition comprises the following steps:

[0096] Step S1: 100 parts by weight of phenolic phosphorus-containing epoxy resin and 20 parts by weight of DDS are added into a reactor, and the reactor is opened for stirring and heating. After the temperature of the materials in the reactor rises to 110-130° C., the reaction is carried out for 2 hours;

[0097] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0098] Step S2: when the temperature of the material in the reactor drops to 40-60° C., toluene, 1.2 parts by weight of 2-methylimidazole, 60 parts by weight of high-strength benzoxazine hollow foaming resin powder with a particle size of 40 μm, and 125 parts by weight of aluminum hydroxide with a particle size of 5 μm are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0099] Preparation process of glass cloth prepreg and low thermal conductivity epoxy glass cloth laminate:

[0100] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0101] A1: Install the glass cloth on the vertical impregnation drying production line, and heat the temperature in the vertical oven 40 in the vertical impregnation drying production line to 160±10°C;

[0102] Among them, the weight specification of glass cloth is 210g / m 2 ;

[0103] A2: The low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above is injected into the dipping device 30 in the vertical dipping and drying production line, and the glass cloth prepreg is manufactured at a vehicle speed, i.e., a line speed of 5 to 8 m / min, and then the manufactured glass cloth prepreg is cut into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0104] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0105] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0106] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0107] Embodiment 4:

[0108] Process for preparing low thermal conductivity epoxy resin composition:

[0109] A method for preparing a low thermal conductivity epoxy resin composition comprises the following steps:

[0110] Step S1: 100 parts by weight of phenolic phosphorus-containing epoxy resin and 35 parts by weight of DDS are added into a reactor, and the reactor is opened for stirring and heating. After the temperature of the materials in the reactor rises to 110-130° C., the reaction is carried out for 2 hours;

[0111] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0112] Step S2: when the temperature of the material in the reactor drops to 40-60° C., toluene, 1.2 parts by weight of 2-methylimidazole, 60 parts by weight of high-strength benzoxazine hollow foaming resin powder with a particle size of 40 μm, and 125 parts by weight of aluminum hydroxide with a particle size of 5 μm are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0113] Preparation process of glass cloth prepreg and low thermal conductivity epoxy glass cloth laminate:

[0114] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0115] A1: Install the glass cloth on the vertical impregnation drying production line, and heat the temperature in the vertical oven 40 in the vertical impregnation drying production line to 160±10°C;

[0116] Among them, the weight specification of glass cloth is 210g / m 2 ;

[0117] A2: The low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above is injected into the dipping device 30 in the vertical dipping and drying production line, and the glass cloth prepreg is manufactured at a vehicle speed, i.e., a line speed of 5 to 8 m / min, and then the manufactured glass cloth prepreg is cut into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0118] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0119] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0120] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0121] Embodiment 5:

[0122] Process for preparing low thermal conductivity epoxy resin composition:

[0123] A method for preparing a low thermal conductivity epoxy resin composition comprises the following steps:

[0124] Step S1: 100 parts by weight of phenolic phosphorus-containing epoxy resin and 30 parts by weight of DDS are added into a reactor, and the reactor is opened for stirring and heating. After the temperature of the materials in the reactor rises to 110-130° C., the reaction is carried out for 2 hours;

[0125] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0126] Step S2: when the temperature of the material in the reactor drops to 40-60° C., toluene, 3.0 parts by weight of 2-methylimidazole, 60 parts by weight of high-strength benzoxazine hollow foaming resin powder with a particle size of 40 μm, and 125 parts by weight of aluminum hydroxide with a particle size of 5 μm are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0127] Preparation process of glass cloth prepreg and low thermal conductivity epoxy glass cloth laminate:

[0128] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0129] A1: Install the glass cloth on the vertical impregnation drying production line, and heat the temperature in the vertical oven 40 in the vertical impregnation drying production line to 160±10°C;

[0130] Among them, the weight specification of glass cloth is 140g / m 2 ;

[0131] A2: The low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above is injected into the dipping device 30 in the vertical dipping and drying production line, and the glass cloth prepreg is manufactured at a vehicle speed, i.e., a line speed of 5 to 8 m / min, and then the manufactured glass cloth prepreg is cut into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0132] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0133] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0134] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0135] Embodiment 6:

[0136] Process for preparing low thermal conductivity epoxy resin composition:

[0137] A method for preparing a low thermal conductivity epoxy resin composition comprises the following steps:

[0138] Step S1: 100 parts by weight of phenolic phosphorus-containing epoxy resin and 30 parts by weight of DDS are added into a reactor, and the reactor is opened for stirring and heating. After the temperature of the materials in the reactor rises to 110-130° C., the reaction is carried out for 2 hours;

[0139] Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%;

[0140] Step S2: when the temperature of the material in the reactor drops to 40-60° C., toluene, 0.5 parts by weight of 2-methylimidazole, 60 parts by weight of high-strength benzoxazine hollow foaming resin powder with a particle size of 40 μm, and 125 parts by weight of aluminum hydroxide with a particle size of 5 μm are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained;

[0141] Preparation process of glass cloth prepreg and low thermal conductivity epoxy glass cloth laminate:

[0142] A method for preparing a low thermal conductivity epoxy resin glass cloth laminate comprises the following steps:

[0143] A1: Install the glass cloth on the vertical impregnation drying production line, and heat the temperature in the vertical oven 40 in the vertical impregnation drying production line to 160±10°C;

[0144] Among them, the weight specification of glass cloth is 210g / m 2 ;

[0145] A2: The low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition described above is injected into the dipping device 30 in the vertical dipping and drying production line, and the glass cloth prepreg is manufactured at a vehicle speed, i.e., a line speed of 5 to 8 m / min, and then the manufactured glass cloth prepreg is cut into a size of 1250*2470 mm to obtain the required glass cloth prepreg;

[0146] Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm;

[0147] A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min;

[0148] A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

[0149] Embodiment 7:

[0150] The preparation of Example 1 was repeated, except that in the process of preparing the low thermal conductivity epoxy resin composition, the phenolic phosphorus-containing epoxy resin was replaced with a dicyclopentadiene phenolic phosphorus-containing epoxy resin, and in the process of preparing the glass cloth prepreg and the low thermal conductivity epoxy glass cloth laminate, the specification of the glass cloth used was 210 g / m 2 The other steps are the same as those in Example 1.

[0151] Example 8

[0152] The preparation of Example 1 was repeated, except that in the process of preparing the low thermal conductivity epoxy resin composition, the phenolic phosphorus-containing epoxy resin was replaced with an o-cresol phenolic phosphorus-containing epoxy resin, and in the process of preparing the glass cloth prepreg and the low thermal conductivity epoxy glass cloth laminate, the specification of the glass cloth used was 140 g / m 2 The other steps are the same as those in Example 1.

[0153] Example 9

[0154] The preparation of Example 1 was repeated, except that 2-methylimidazole was replaced with 2-ethyl-4-methylimidazole during the preparation of the low thermal conductivity epoxy resin composition. The other steps were the same as those of Example 1.

[0155] Example 10

[0156] The preparation of Example 1 was repeated, except that in the process of preparing the low thermal conductivity epoxy resin composition, the phenolic phosphorus-containing epoxy resin was replaced with an o-cresol phenolic phosphorus-containing epoxy resin, and in the process of preparing the glass cloth prepreg and the low thermal conductivity epoxy glass cloth laminate, the specification of the glass cloth used was 140 g / m 2 The other steps are the same as those in Example 1.

[0157] Embodiment 11

[0158] The preparation of Example 10 was repeated, except that in the process of preparing the low thermal conductivity epoxy resin composition, DDS was replaced with DDM, the weight of benzoxazine and hollow powder was increased to 90 parts by weight, and in the process of preparing the glass cloth prepreg and the low thermal conductivity epoxy glass cloth laminate, the specification of the glass cloth used was 180 g / m 2 The other steps are the same as those in Example 10.

[0159] Example 12

[0160] The preparation of Example 10 was repeated, except that in the process of preparing the low thermal conductivity epoxy resin composition, DDS was replaced with m-xylylenediamine, the weight of benzoxazine and hollow powder was increased to 80 parts by weight, and in the process of preparing the glass cloth prepreg and the low thermal conductivity epoxy glass cloth laminate, the specification of the glass cloth used was 180 g / m 2 The other steps are the same as those in Example 10.

[0161] Embodiment 13

[0162] The preparation of Example 11 was repeated, except that in the process of preparing the low thermal conductivity epoxy resin composition, the benzoxazine hollow powder was reduced to 40 parts by weight, and in the process of preparing the glass cloth prepreg and the low thermal conductivity epoxy glass cloth laminate, the specification of the glass cloth used was 210 g / m 2 The other steps are the same as those in Example 11.

[0163] Embodiment 14

[0164] The preparation of Example 11 was repeated, except that during the preparation of the low thermal conductivity epoxy resin composition, the particle size of the benzoxazine hollow powder was changed to 30 μm, and the particle size of the aluminum hydroxide was changed to 8 μm. The other steps of the preparation were the same as those of Example 11.

[0165] Embodiment 15

[0166] The preparation of Example 11 was repeated, except that during the preparation of the low thermal conductivity epoxy resin composition, the particle size of the benzoxazine hollow powder was changed to 50 μm, and the particle size of the aluminum hydroxide was changed to 3 μm. The other steps of the preparation were the same as those of Example 11.

[0167] Example 16

[0168] The preparation of Example 15 was repeated, except that during the preparation of the low thermal conductivity epoxy resin composition, the benzoxazine hollow powder with a particle size of 50 μm was replaced with a phenolic resin hollow powder with a particle size of 50 μm, the amount of aluminum hydroxide added was increased to 150 parts by weight, and the other preparation steps were the same as in Example 15.

[0169] Embodiment 17

[0170] The preparation of Example 16 was repeated, except that during the preparation of the low thermal conductivity epoxy resin composition, the particle size of the phenolic resin hollow powder was changed to 40 μm, the amount of aluminum hydroxide added was reduced to 100 parts by weight, and the other preparation steps were the same as Example 16.

[0171] Table 1

[0172]

[0173] A total of 17 low thermal conductivity epoxy glass cloth laminates were prepared from Example 1 to Example 17, and their thermal conductivity, bending strength after 1000 hours of testing at a temperature of 85°C and a humidity of 85%, and flammability are shown in Table 1. The test at a temperature of 85°C and a humidity of 85% for 1000 hours is referred to as the "double 85" test in Table 1.

[0174] The above embodiments are only some embodiments. It can be seen from Table 1 that the thermal conductivity of 17 different low thermal conductivity epoxy glass cloth laminates all meet the requirement that the thermal conductivity of the epoxy resin separator for the new energy battery pack is less than 0.20W / (m K). Therefore, the low thermal conductivity epoxy glass cloth laminate prepared by the method of the present invention meets the requirement that the thermal conductivity of the epoxy resin separator for the new energy battery pack is less than 0.20W / (m K).

[0175] Impregnation and drying technology is a technology that controls the entire process of continuous resin impregnation, drying, shearing or rolling up semi-finished products of rolled decorative paper, kraft paper and other impregnated paper or cloth. It is one of the important links in the production process of laminated products such as laminated boards and decorative boards, and plays a key role in the quality and performance of products such as melamine veneer in the wood-based panel industry.

[0176] In the wood-based panel industry, various impregnation and drying equipment that are compatible with the impregnation and drying technology are divided into two categories according to their layout: horizontal and vertical production lines. Impregnation equipment with different structures is used according to different process methods and production requirements.

[0177] Generally speaking, horizontal impregnation and drying production lines process paper-based materials, which are characterized by good quality, high efficiency and large output, and are widely used in large-scale production enterprises. Horizontal impregnation and drying production lines are mainly suitable for the impregnation and drying production of laminate flooring, low-pressure melamine and high-pressure melamine impregnated paper, and are also suitable for the production of impregnated paper for cement formwork.

[0178] The vertical impregnation and drying production line is mostly used to process cloth-based materials or the surface paper of thermosetting resin decorative laminates, and is also used for the production of decorative paper impregnation with a small output. Its main features are low investment, small footprint, and low technical requirements for paper. The vertical impregnation and drying production line is mainly used for the impregnation and drying of glass fiber cloth, and is one of the important automated production lines in the production of copper clad laminates.

[0179] The present invention adopts a vertical impregnation and drying production line to produce glass cloth prepreg.

[0180] like Figure 1 As shown, the vertical impregnation and drying production line at least includes a glass cloth unwinding machine 10, a front cloth storage device 20, a dipping device 30, a vertical oven 40, a deviation adjusting machine 50, a traction machine 60, a trimming machine 70, a rear cloth storage device 80 and a glass cloth winding machine 90 which are connected in sequence.

[0181] Among them, the glass cloth unwinding machine 10, the front cloth storage device 20, the vertical oven 40, the deflection adjusting machine 50, the traction machine 60, the edge trimming machine 70, the rear cloth storage device 80 and the glass cloth winding machine 90 can respectively adopt the glass cloth unwinding machine 10, the front cloth storage device 20, the vertical oven 40, the deflection adjusting machine 50, the traction machine 60, the edge trimming machine 70, the rear cloth storage device 80 and the glass cloth winding machine 90 in the prior art that can realize the functions of the present invention.

[0182] like Figure 2 As shown, in order to facilitate the immersion of the glass cloth in the low thermal conductivity epoxy resin composition, it is further preferred in this embodiment that the dipping device 30 includes a mounting bracket 300, a first roller body 301, a second roller body 302, a third roller body 303, a fourth roller body 304, an auxiliary rotating rod 305, a liquid storage tank 306 and a driving assembly 307, the liquid storage tank 306 is arranged on the mounting bracket 300 and is fixedly connected to the mounting bracket 300, the first roller body 301 and the fourth roller body 304 are arranged at the upper end of the mounting bracket 300 and are connected to the mounting bracket The mounting bracket 300 is rotatably connected, the first roller body 301 and the fourth roller body 304 are respectively located on both sides of the mounting bracket 300, the auxiliary rotating rod 305 is arranged on the mounting bracket 300 and is rotatably connected to the mounting bracket 300, the auxiliary rotating rod 305 is located above the fourth roller body 304, the driving assembly 307 is arranged on one side of the mounting bracket 300, and is cooperated with the fourth roller body 304 to drive the fourth roller body 304, the second roller body 302 and the third roller body 303 are arranged in the liquid storage tank 306, and are rotatably connected to the liquid storage tank 306.

[0183] When in use, the glass cloth enters from above the first roller body 301, then passes through the second roller body 302 and the third roller body 303 in the liquid storage tank 306, and then passes through between the fourth roller body 304 and the auxiliary rotating rod 305. The fourth roller body 304 is driven to rotate by the driving component 307, so that the glass cloth can be continuously fed, and the prepared low thermal conductivity epoxy resin composition is injected into the liquid storage tank 306, so that the glass cloth can be fully immersed in the low thermal conductivity epoxy resin composition when passing through the liquid storage tank 306, thereby completing the pre-impregnation process of the glass cloth.

[0184] like Figure 3 As shown, preferably, the driving assembly 307 includes a worm wheel 308, a worm 309 and a rotating motor 310, one end of the fourth roller body 304 passes through the mounting bracket 300 and is fixedly connected to the worm wheel 308, the worm 309 is arranged in coordination with the worm wheel 308, the rotating motor 310 is arranged at one end of the worm 309 and is fixedly connected to the worm 309, and is used to drive the worm 309 to rotate, and a motor bracket 311 for mounting the rotating motor 310 is provided on the mounting bracket 300, the motor bracket 311 is fixedly connected to one side of the mounting bracket 300 by bolts, and the rotating motor 310 is mounted on the mounting bracket 300.

[0185] When in use, the motor 310 is used to drive the worm 309 to rotate, thereby driving the worm wheel 308 matched with the worm 309 to rotate, and then driving the fourth roller 304 to rotate, so that the glass cloth can pass between the fourth roller 304 and the auxiliary rotating rod 305.

[0186] Preferably, a rotating seat 312 cooperating with the worm 309 is provided on the mounting bracket 300, and the rotating seat 312 is fixedly connected to the mounting bracket 300 by bolts. One end of the worm 309 is rotatably connected to the rotating seat 312, and the other end is fixedly connected to the output shaft of the rotating motor 310.

[0187] The provision of the rotating seat 312 can effectively improve the installation stability of the worm 309, so that the worm 309 can be transmitted more stably.

[0188] like Figure 4 As shown, preferably, a protective cover 313 for protecting the worm wheel 308 is provided on the mounting bracket 300, the protective cover 313 is sleeved on the outside of the worm wheel 308 and the worm 309, and one side of the protective cover 313 is fixedly connected to the mounting bracket 300 by bolts.

[0189] The provision of the protective cover 313 can effectively prevent dust or other objects from falling on the fitting position of the worm wheel 308 and the worm 309 , thereby effectively protecting the worm wheel 308 and the worm 309 .

[0190] like Figure 5As shown, preferably, a pair of inclined surfaces 314 inclined toward the middle of the liquid storage tank 306 are provided at the bottom of the liquid storage tank 306, and a flow groove 315 is provided at the intersection of the pair of inclined surfaces 314. The flow groove 315 runs through both ends of the liquid storage tank 306, and a liquid infusion pipe 316 connected to the flow groove 315 is provided at one end of the flow groove 315, and a liquid discharge pipe 317 connected to the flow groove 315 is provided at the other end of the flow groove 315. Valves 318 are provided on the liquid infusion pipe 316 and the liquid discharge pipe 317. The valve 318 can be a pneumatic valve or a solenoid valve.

[0191] The bottom of the liquid storage tank 306 is inclined, and a flow groove 315 is provided at the intersection, so that after the process is completed, the low thermal conductivity epoxy resin composition can be collected in the flow groove 315, and then discharged and recovered through the drain pipe 317 connected to the flow groove 315; when liquid replenishment is needed, the low thermal conductivity epoxy resin composition can be injected from the liquid replenishment pipe 316, so that the liquid level in the liquid storage tank 306 rises, thereby completing the injection process of the low thermal conductivity epoxy resin composition. This injection method can effectively avoid liquid splashing during pouring.

[0192] Preferably, a baffle plate 319 is provided on the liquid storage tank 306, and the baffle plate 319 is fixedly connected to the top of the liquid storage tank 306 by bolts.

[0193] The baffle 319 can effectively prevent a portion of dust from entering the liquid storage tank 306, thereby improving the prepreg quality of the glass cloth.

[0194] Working principle of the present invention:

[0195] The present invention comprises the following steps: adding 100 parts by weight of epoxy resin and 20 to 40 parts by weight of curing agent into a reaction kettle, and opening the reaction kettle for stirring and heating. After the temperature of the materials in the reaction kettle rises to 110 to 130° C., reacting for 1 to 3 hours. When the temperature of the materials in the reaction kettle drops to 40 to 60° C., sequentially adding a solvent, 0.5 to 3.0 parts by weight of a catalyst, 40 to 90 parts by weight of a high-strength hollow foaming resin powder and 100 to 150 parts by weight of aluminum hydroxide, and stirring at a high speed through the reaction kettle. After the materials in the reaction kettle are uniformly stirred, a low thermal conductivity epoxy resin composition is obtained. Then, the glass cloth is installed on a vertical impregnation and drying production line, and the temperature in a vertical oven 40 in the vertical impregnation and drying production line is heated to 160±10° C.; then The prepared low thermal conductivity epoxy resin composition is injected into the dipping device 30 in the vertical impregnation and drying production line, and the glass cloth prepreg is manufactured at a speed of 5 to 8 m / min, and then the manufactured glass cloth prepreg is cut into a size of 1250*2470 mm to obtain the required glass cloth prepreg; then the required glass cloth prepreg is prepared, and then the glass cloth prepreg with a size of 1250*2470 mm is hot-pressed under the process conditions of temperature of 170 to 190°C, pressure of 7 to 8 MPa, and insulation time ≥150 min; after hot-pressing, cooling water is introduced to cool down until the temperature drops below 50°C, and then the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming; the present invention realizes the halogen-free flame retardant performance of the laminate through the synthesis of the low thermal conductivity epoxy resin composition and the PA l(OH)3 synergistic flame retardant technology, and its vertical flammability level reaches FV0. The present invention realizes the low thermal conductivity of epoxy glass cloth laminates through the dispersion composite technology of high-strength hollow foamed resin powder and phosphorus-containing epoxy resin. The thermal conductivity of the prepared low thermal conductivity epoxy glass cloth laminate is lower than 0.20W / (m K), which meets the requirement that the thermal conductivity of insulating partitions for new energy battery packs is less than 0.20W / (m K).

[0196] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a low thermal conductivity epoxy resin composition, characterized in that: The following steps are involved: Step S1: 100 parts by weight of epoxy resin and 20 to 40 parts by weight of curing agent are added into a reaction kettle, and the reaction kettle is opened for stirring and heating. After the temperature of the materials in the reaction kettle rises to 110 to 130° C., the reaction is carried out for 1 to 3 hours; Among them, the phosphorus content of epoxy resin is 2.8% to 3.5%; Step S2: when the temperature of the material in the reaction kettle drops to 40-60° C., a solvent, 0.5-3.0 parts by weight of a catalyst, 40-90 parts by weight of a high-strength hollow foamed resin powder, and 100-150 parts by weight of aluminum hydroxide are added in sequence, and the reaction kettle is stirred at a high speed. After the materials in the reaction kettle are stirred evenly, a low thermal conductivity epoxy resin composition can be obtained; The solid content of the low thermal conductivity epoxy resin composition is 60%.

2. The method for preparing a low thermal conductivity epoxy resin composition according to claim 1, characterized in that: In step S1, the epoxy resin is any one of phenolic phosphorus-containing epoxy resin, dicyclopentadiene phosphorus-containing epoxy resin or o-cresol phosphorus-containing epoxy resin, or a mixture of the two in any ratio.

3. The method for preparing a low thermal conductivity epoxy resin composition according to claim 1, characterized in that: In step S1 , the curing agent is any one of 4,4′-diaminodiphenylmethane DDM, 4,4′-diaminodiphenyl sulfone DDS or meta-xylylenediamine.

4. The method for preparing a low thermal conductivity epoxy resin composition according to claim 1, characterized in that: In step S2, the catalyst is any one of 2-methylimidazole and 2-ethyl-4-methylimidazole, or a mixture of the two in any ratio.

5. The method for preparing a low thermal conductivity epoxy resin composition according to claim 1, characterized in that: In step S2, the high-strength hollow foamed resin powder is any one of benzoxazine resin hollow powder and phenolic resin hollow powder, or a mixture of the two in any ratio.

6. The method for preparing a low thermal conductivity epoxy resin composition according to claim 1, characterized in that: In step S2, the particle size specification of the high-strength hollow foamed resin powder is any one or two of 30 μm, 40 μm or 50 μm.

7. The method for preparing a low thermal conductivity epoxy resin composition according to claim 1, characterized in that: In step S2, the particle size specification of aluminum hydroxide is any one or two of 3 μm, 5 μm or 8 μm.

8. A method for preparing a low thermal conductivity epoxy resin glass cloth laminate, characterized in that: The following steps are involved: A1: installing the glass cloth on a vertical dipping and drying production line, and heating the temperature in a vertical oven (40) in the vertical dipping and drying production line to 160±10° C.; Among them, the weight specification of glass cloth is 210g / m 2 , 180g / m 2 or 140g / m 2 Either or both of the following: A2: injecting the low thermal conductivity epoxy resin composition prepared by the method for preparing a low thermal conductivity epoxy resin composition according to any one of claims 1 to 7 into a dipping device (30) in a vertical dipping and drying production line, and manufacturing glass cloth prepreg at a speed of 5 to 8 m / min, and then cutting the manufactured glass cloth prepreg into a size of 1250*2470 mm to obtain the required glass cloth prepreg; Among them, the required central control indicators of the glass cloth prepreg are: the content of the low thermal conductivity epoxy resin composition is 45% to 50%, and the fluidity is 20 to 25 mm; A3: Prepare the required glass cloth prepreg, and then hot-press the glass cloth prepreg with a size of 1250*2470mm under the process conditions of temperature of 170-190℃, pressure of 7-8MPa, and insulation time of ≥150min; A4: After hot pressing, cool water is introduced to cool down until the temperature drops below 50°C. Then, the low thermal conductivity epoxy glass cloth laminate is obtained by unloading and trimming.

9. The method for preparing a low thermal conductivity epoxy resin glass cloth laminate according to claim 8, characterized in that: In step A4, the weight composition of the prepared low thermal conductivity epoxy glass cloth laminate is 50% to 55% of glass cloth and 45% to 50% of the low thermal conductivity epoxy resin composition.

10. The method for preparing a low thermal conductivity epoxy resin glass cloth laminate according to claim 9, characterized in that: In step A4, the thermal conductivity of the low thermal conductivity epoxy glass cloth laminate prepared is lower than 0.20 W / (m K).