Mixing method and uniformity evaluation method of metallurgical steel waste residue-containing asphalt mixture
By using electromagnets in the magnetic stirring device to balance the gravity of steel waste slag and coarse aggregate, the problem of uneven mixing of the mixture caused by the density of steel waste slag is solved, the uniformity and performance of the asphalt mixture are improved, and the asphalt road surface is extended service life.
Patent Information
- Application Number
- CN202411091549.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The high density of steel slags leads to segregation of asphalt mixture containing steel slags during the mixing process, resulting in uneven mixing of the mixture, affecting the compaction degree and service life.
In the magnetic stirring device, the electromagnetic force is used to generate upward magnetic force on the steel waste slag, so that it is the same as the gravity applied to the coarse aggregate, and the magnetic field strength is adjusted to balance the current, thereby eliminating or reducing the density of the steel waste slag and not mixing the mixture. Even effect.
It effectively eliminates the impact of the density of steel sludge on uneven mixing of the mixture, improves the uniformity and overall performance of the asphalt mixture, and extends the service life of the asphalt pavement.
Smart Images

Figure CN119021061A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road engineering, and in particular to a mixing method and a uniformity evaluation method for an asphalt mixture containing steelmaking waste residue. Background Art
[0002] In recent years, my country's steel industry has developed rapidly. While the scale of steel production has continued to expand, tens of millions of tons of industrial by-products - steel slag have also been produced. The increasing amount of steel slag as an industrial by-product not only occupies a large amount of land, but also causes serious environmental pollution. It is also a waste of resources for the steel slag itself. It has been proven to be feasible to recycle and reuse steel slag as solid waste resources, such as using steel slag as aggregate for asphalt pavement. Using steel slag as aggregate for road engineering not only saves resources and reduces the cost of highway engineering, but also has positive significance in environmental protection.
[0003] However, the density of steel slag is significantly higher than that of conventional aggregates, which makes it easy for steel slag-containing asphalt mixtures to segregate during the mixing process, resulting in uneven mixing of the mixture, affecting the overall performance of the steel slag-containing asphalt mixtures, such as compaction and strength, and reducing the service life of asphalt pavement. In order to ensure the performance of steel slag-containing asphalt mixtures, it is necessary to develop a mixing method and uniformity evaluation method for steel slag-containing asphalt mixtures. Summary of the invention
[0004] In view of the problems existing in the above prior art, the present invention provides a mixing method and uniformity evaluation method of asphalt mixture containing steel slag. The mixing method of asphalt mixture containing steel slag of the present invention generates an upward magnetic force on the steel slag by an electromagnet arranged in the upper part of a magnetic stirring device, so that the steel slag and coarse aggregate of the same volume are subjected to the same gravity, which can eliminate or significantly reduce the influence of the high density of steel slag on the uneven mixing of the mixture. It is specifically achieved by the following technologies.
[0005] A mixing method of asphalt mixture containing steelmaking waste residue comprises the following steps:
[0006] The same volume of steelmaking waste slag and coarse aggregate is placed in a magnetic stirring device, and the magnetic field strength of the electromagnet is adjusted so that the steelmaking waste slag and the coarse aggregate are subjected to the same gravity to obtain a balanced current;
[0007] Raw materials including the steelmaking waste slag, coarse aggregate, fine aggregate, mineral powder and asphalt are added to the magnetic stirring device, and the electromagnet is energized and a balanced current is maintained for mixing to obtain an asphalt mixture containing steelmaking waste slag.
[0008] The uneven mixing of asphalt mixture containing steel waste slag is mainly due to the significant difference in density between steel waste slag and conventional coarse aggregate, which leads to a significant difference in gravity between the same volume of steel waste slag and conventional coarse aggregate. The steel waste slag is easy to sink during the mixing process, resulting in uneven mixing of the asphalt mixture. The present invention generates an upward magnetic force on the steel waste slag by adding an electromagnetic field in the magnetic stirring device to offset a part of the gravity. The magnetic field strength generated by the electromagnet can be adjusted by adjusting the current in the electromagnet, thereby adjusting the magnetic force on the steel waste slag. When the current of the electromagnet reaches a certain value, so that the same volume of steel waste slag and conventional coarse aggregate are subjected to the same gravity, it is a balanced current. Mixing the asphalt mixture containing steel waste slag in this state can eliminate or significantly reduce the influence of the high density of the steel waste slag on the uneven mixing of the mixture.
[0009] Furthermore, the steelmaking waste slag asphalt mixture comprises, by weight percentage, a mixture of 20-60% steelmaking waste slag and coarse aggregate, 25-65% fine aggregate, 0-10% mineral powder and 2-6% asphalt.
[0010] Furthermore, the particle sizes of the steelmaking waste slag and coarse aggregate are both 4.75-19 mm.
[0011] Furthermore, the particle size of the fine aggregate is less than 4.75 mm.
[0012] Furthermore, the mixing time is not less than 55s.
[0013] Furthermore, the steelmaking waste slag includes at least one of blast furnace ironmaking slag, converter slag, open-hearth slag and electric furnace slag produced in the steelmaking process. Converter slag, open-hearth slag and electric furnace slag can all be referred to as slag particles.
[0014] Furthermore, the coarse aggregate includes at least one of limestone aggregate, basalt aggregate and diabase aggregate.
[0015] Furthermore, the method for obtaining the balanced current comprises the following steps:
[0016] The steelmaking waste slag and coarse aggregate are placed in containers of the same weight, and then the containers are hung under the dynamometer, and the steelmaking waste slag and coarse aggregate are placed at the same height in the magnetic stirring device;
[0017] Turn on the power supply of the electromagnet and adjust the current intensity in the electromagnet. When the readings of the two dynamometers hanging the steelmaking waste slag and the coarse aggregate respectively are observed to be the same, record the current of the electromagnet, which is the balance current.
[0018] A magnetic stirring device for asphalt mixture containing steelmaking waste residue, wherein a feed port and an electromagnet are provided on the upper portion, stirring devices are provided on the inner walls on both sides, the stirring device comprises a stirring shaft, a fixed gear shaft and stirring teeth, the fixed gear shaft is fixedly connected to the stirring shaft, a plurality of stirring teeth are fixedly connected to the fixed gear shaft, the fixed gear shaft of the stirring device on one side is longer than the fixed gear shaft of the stirring device on the other side; a discharge baffle and a discharge port are provided at the lower portion of the magnetic stirring device.
[0019] Furthermore, electromagnets are symmetrically arranged on the upper part of the inner wall of the magnetic stirring device.
[0020] A method for evaluating the uniformity of an asphalt mixture containing steelmaking waste residue comprises the following steps:
[0021] For the mixed asphalt mixture containing steelmaking waste residue, samples were taken at the upper, middle and lower positions, and the masses were recorded as M 0上 、M 0中 、M 0下 ;
[0022] The samples at the upper, middle and lower positions are burned respectively. After burning, the aggregate mixture without asphalt is obtained. The mass is weighed and recorded as M 1上 、M 1中 、M 1下 ;
[0023] Measure the volume of the sample at the upper, middle and lower positions after combustion, and record them as V 上 、V 中 、V 下 ;
[0024] The deviation Δρ of the average density of the samples at the upper, middle and lower positions is calculated according to formula I; the deviation ΔR of the average volumetric dosage of asphalt is calculated according to formula II; wherein, (Formula I); (Formula II);
[0025] According to the deviation Δρ of the average density of the samples at the upper, middle and lower positions and the deviation ΔR of the average volume of asphalt, the mixing uniformity of the asphalt mixture containing steelmaking waste residue is judged according to the following method:
[0026] When Δρ≤0.2g / cm 3 And ΔR≤0.01g / cm 3 When mixing, the mixture is evenly mixed;
[0027] When Δρ>0.2g / cm 3 or ΔR>0.01g / cm 3 The mixture is not mixed evenly.
[0028] Compared with the prior art, the present invention is beneficial in that:
[0029] 1. The mixing method of the asphalt mixture containing steel slag of the present invention makes the steel slag and coarse aggregate with the same volume subjected to the same gravity by the electromagnet arranged in the upper part of the magnetic stirring device, thereby eliminating or significantly reducing the influence of the high density of the steel slag on the uneven mixing of the mixture;
[0030] 2. The magnetic stirring device of the present invention is easy to operate, and sampling ports are arranged at the upper, middle and lower positions of the side wall, which is convenient for sampling and testing the uniformity of the asphalt mixture containing steel waste slag; the stirring device is arranged on the side wall of the magnetic stirring device, and long strip-shaped stirring teeth are used for stirring, which is more conducive to uniform mixing of steel waste slag, coarse aggregate, fine aggregate, mineral powder and asphalt;
[0031] 3. The method for evaluating the uniformity of the asphalt mixture containing steelmaking waste residue of the present invention is simple to operate and produces reliable results. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A magnetic stirring device according to the present invention;
[0033] In the figure: 1. feed port; 2. inner top wall; 3. electromagnet; 4. stirring teeth; 5. stirring shaft; 6. sampling port; 7. fixed gear shaft; 8. sampling baffle; 9. discharge port; 10. discharge baffle. DETAILED DESCRIPTION
[0034] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0035] The present invention provides an exemplary mixing method of asphalt mixture containing steelmaking waste residue, comprising the following steps:
[0036] Add the same volume of steelmaking waste slag and coarse aggregate into the magnetic stirring device, adjust the magnetic field strength of the electromagnet so that the steelmaking waste slag and the coarse aggregate are subjected to the same gravity, and obtain a balanced current;
[0037] Adding raw materials including the steelmaking waste slag and coarse aggregate into the magnetic stirring device, energizing the electromagnet and maintaining a balanced current, and mixing to obtain an asphalt mixture containing steelmaking waste slag;
[0038] The raw materials also include other fine aggregates, mineral powder, asphalt, etc.
[0039] In some examples of the present invention, the steelmaking waste slag asphalt mixture may include, by weight percentage, a mixture of 20-60% steelmaking waste slag and coarse aggregate, 25-65% fine aggregate, 0-10% mineral powder and 2-6% asphalt.
[0040] In some examples of the present invention, the particle sizes of the steelmaking waste slag and the coarse aggregate can both be 4.75-19 mm.
[0041] In some examples of the present invention, the particle size of the fine aggregate may be less than 4.75 mm.
[0042] In some examples of the present invention, the mixing time may be no less than 55 seconds.
[0043] In some examples of the present invention, the coarse aggregate may include at least one of limestone aggregate, basalt aggregate, and diabase aggregate.
[0044] In the present invention, the steelmaking waste slag may include all solid particles with magnetic effect. In some examples of the present invention, the steelmaking waste slag may include at least one of blast furnace ironmaking slag, converter slag, open hearth slag and electric furnace slag produced in the steel smelting process.
[0045] The present invention also exemplarily provides a method for evaluating the uniformity of an asphalt mixture containing steelmaking waste residue, comprising the following steps:
[0046] For the mixed asphalt mixture containing steelmaking waste residue, samples were taken at the upper, middle and lower positions, and the masses were recorded as M 0上 、M 0中 、M 0下 ;
[0047] The samples at the upper, middle and lower positions are burned respectively. After burning, the aggregate mixture without asphalt is obtained. The mass is weighed and recorded as M 1上 、M 1中 、M 1下 ;
[0048] Measure the volume of the sample at the upper, middle and lower positions after combustion, and record them as V 上 、V 中 、V 下 ;
[0049] The deviation Δρ of the average density of the samples at the upper, middle and lower positions is calculated according to formula I; the deviation ΔR of the average volumetric dosage of asphalt is calculated according to formula II; wherein, (Formula I); (Formula II);
[0050] According to the deviation Δρ of the average density of the samples at the upper, middle and lower positions and the deviation ΔR of the average volume of asphalt, the mixing uniformity of the asphalt mixture containing steelmaking waste residue is judged according to the following method:
[0051] When Δρ≤0.2g / cm3 And ΔR≤0.01g / cm 3 When mixing, the mixture is evenly mixed;
[0052] When Δρ>0.2g / cm 3 or ΔR>0.01g / cm 3 The mixture is not mixed evenly.
[0053] In some examples of the present invention, the combustion may be carried out at 530±10° C. for 60-70 minutes.
[0054] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] like Figure 1 As shown, the magnetic stirring device of the present invention comprises a feed port 1, a discharge port 9, and an electromagnet 3 is symmetrically arranged on the inner top wall 2 of the magnetic stirring device; stirring devices are arranged on the inner walls on both sides of the magnetic stirring device, and the stirring device comprises a stirring shaft 5, a fixed gear shaft 7 is fixed on the stirring shaft 5, and two long and one short stirring teeth 4 are fixed on the fixed gear shaft 7, and the fixed gear shaft 7 of the stirring device on one side is longer than the fixed gear shaft 7 of the stirring device on the other side; a discharge baffle 10 is arranged at the discharge port 9. In order to facilitate the detection of the uniformity of the mixed material, the present invention is provided with sampling ports 6 at the upper, middle and lower positions of the inner wall of one side of the magnetic stirring device, and each sampling port 6 is provided with a sampling baffle 8.
[0056] In some examples of the present invention, the same volume of steelmaking waste slag and coarse aggregate can be obtained by drainage method, specifically:
[0057] In two water containers, steelmaking waste slag with a particle size of 4.75-19 mm and coarse aggregate with a particle size of 4.75-19 mm are placed respectively, so that the water level in the container rises or the volume of overflowed water is the same, that is, the same volume of steelmaking waste slag and coarse aggregate is obtained.
[0058] In some examples of the present invention, a method for obtaining a balanced current includes the following steps:.
[0059] Put the steelmaking waste slag into container A, put the coarse aggregate into container B, and hang container A and container B under the dynamometer respectively; containers A and B are plastic net bags of equal mass;.
[0060] Then, container A and container B are placed at the same height in the magnetic stirring device;.
[0061] Turn on the power supply of the electromagnet and adjust the current intensity in the electromagnet. When the readings of the two dynamometers hanging the steelmaking waste slag and the coarse aggregate respectively are observed to be the same, record the current of the electromagnet, which is the balance current.
[0062] In the following specific embodiments, fine aggregates include limestone aggregate, basalt aggregate, and diabase aggregate, and the particle size is less than 4.75 mm.
[0063] In the following specific embodiments, the mineral powder is obtained by processing and grinding limestone, and the content of particles below 0.075 mm is not less than 75%.
[0064] Example 1
[0065] This embodiment provides a mixing method for an asphalt mixture containing steelmaking waste residue, comprising the following steps:
[0066] S1. Put steel slag particles and limestone aggregates with a particle size of 9.5-13.2 mm into a beaker filled with 1000 mL of water, and raise the water level in the beaker by 500 mL to obtain steel slag particles and limestone aggregates of the same volume; put the steel slag particles and limestone aggregates into plastic net bags, and hang the plastic net bags under the spring dynamometer;
[0067] S2, placing the steel slag particles and limestone aggregates in step S1 at the same height in a magnetic stirring device, adjusting the current intensity in the electromagnet so that the readings of the spring dynamometers for suspending the steel slag particles and the limestone aggregates are the same, that is, the steel slag particles and the limestone aggregates are subjected to the same gravity, and recording the current in the electromagnet at this time to obtain the balanced current;
[0068] S3. Add the steel slag particles and limestone aggregate in step S2 into a magnetic stirring device, add fine aggregate, mineral powder and asphalt, energize the electromagnet and maintain the balanced current in step S2, and stir for 40 seconds to obtain an asphalt mixture containing steel slag, wherein the asphalt mixture containing steel slag includes, by mass percentage, a mixture of 50% steel slag and coarse aggregate, 45% fine aggregate, 3% mineral powder and 2% asphalt.
[0069] This embodiment also provides a method for evaluating the uniformity of the above-mentioned asphalt mixture containing steelmaking waste residue, comprising the following steps:
[0070] P1. For the asphalt mixture containing steel slag mixed in step S3 of this embodiment, samples are taken from the upper, middle and lower sampling ports of the magnetic stirring device, and the masses are weighed to obtain M, respectively. 0上 =2151.6g, M 0中 =2278.2g, M 0下 =2244.3g;
[0071] P2. Place the samples at the upper, middle and lower positions in step P1 in an asphalt combustion furnace and burn them at 530°C for 60 minutes. Weigh the mass and obtain M 1上 =2049.1g, M 1中 =2169.7g, M 1下 =2137.4g;
[0072] P3, the samples at the upper, middle and lower positions in step P2 are measured by the displacement method to obtain the volumes V 上 =759.8cm 3 、V 中 =758.1cm 3 、V 下 =721.1cm 3 ;
[0073] P4. Calculate the deviation Δρ of the average density of samples at the upper, middle and lower positions; calculate the deviation ΔR of the average volumetric dosage of asphalt;
[0074] P5, Δρ=0.267g / cm in step P4 3 , greater than 0.2g / cm 3 ; ΔR in step p4 = 0.0133 g / cm 3 , greater than 0.01g / cm 3 That is, the asphalt mixture containing steelmaking waste residue in this embodiment is not mixed evenly.
[0075] At the same time, according to the Technical Specifications for Highway Asphalt Pavement Construction (JTG F40-2004), the samples taken from the upper, middle and lower sampling holes of Example 1 were respectively subjected to the traditional screening method to test the mixing uniformity of the asphalt mixture. If one or more key sieve holes do not meet the requirements of the specification, it is judged to be unqualified, that is, the mixing is uneven. The screening results are shown in Table 1.
[0076] Table 1 Screening results of samples taken from different sampling holes (mixing for 40 seconds)
[0077]
[0078] The key sieve hole pass rates in Table 1 do not meet the requirements, and the mixed materials are not mixed evenly. The determination results of the method of the present invention are consistent with those of the traditional standard method.
[0079] Example 2
[0080] The mixing method of the asphalt mixture containing steelmaking waste slag in this embodiment is basically the same as that in Example 1, except that: the mixing time in step S3 is 45s; in terms of mass percentage, the asphalt mixture containing steelmaking waste slag includes a mixture of 60% steelmaking waste slag and coarse aggregate, 25% fine aggregate, 10% mineral powder and 5% asphalt.
[0081] This embodiment also provides a method for evaluating the uniformity of the above-mentioned asphalt mixture containing steelmaking waste residue, comprising the following steps:
[0082] P1. For the asphalt mixture containing steel slag mixed in step S3 of this embodiment, samples are taken from the upper, middle and lower sampling ports of the magnetic stirring device, and the masses are weighed to obtain M, respectively. 0上 =2162.3g, M 0中 =2289.3g, M 0下 =2256.6g;
[0083] P2. Place the samples at the upper, middle and lower positions in step P1 in an asphalt combustion furnace and burn them at 520°C for 65 minutes. Weigh the mass and obtain M 1上 =2056.4g, M 1中 =2180.3g, M 1下 =2149.1g;
[0084] P3, the samples at the upper, middle and lower positions in step P2 are measured by the displacement method to obtain the volumes V 上 =755.2 cm 3 、V 中 =762.6 cm 3 、V 下 =728.3cm 3 ;
[0085] P4. Calculate the deviation Δρ of the average density of samples at the upper, middle and lower positions; calculate the deviation ΔR of the average volumetric dosage of asphalt;
[0086] P5, Δρ=0.228g / cm in step P4 3 , greater than 0.2g / cm 3 That is, the asphalt mixture containing steelmaking waste residue in this embodiment is not mixed evenly.
[0087] At the same time, according to the Technical Specifications for Highway Asphalt Pavement Construction (JTG F40-2004), the samples taken from the upper, middle and lower sampling holes of Example 2 were respectively subjected to the traditional screening method to test the mixing uniformity of the asphalt mixture. If one or more key sieve holes do not meet the requirements of the specification, it is judged to be unqualified, that is, the mixing is uneven. The screening results are shown in Table 2.
[0088] Table 2 Screening results of samples taken from different sampling holes (mixing for 45 seconds)
[0089]
[0090] The passing rates of the 9.5 mm and 13.2 mm sieve holes in Table 2 do not meet the requirements, and the mixed materials are not mixed evenly. The determination results of the method of the present invention are consistent with those of the traditional standard method.
[0091] Example 3
[0092] The mixing method of the asphalt mixture containing steelmaking waste slag in this embodiment is basically the same as that in Example 1, except that: the mixing time in step S3 is 50s; in terms of mass percentage, the asphalt mixture containing steelmaking waste slag includes a mixture of 29% steelmaking waste slag and coarse aggregate, 65% fine aggregate and 6% asphalt.
[0093] This embodiment also provides a method for evaluating the uniformity of the above-mentioned asphalt mixture containing steelmaking waste residue, comprising the following steps:
[0094] P1. For the asphalt mixture containing steel slag mixed in step S3 of this embodiment, samples are taken from the upper, middle and lower sampling ports of the magnetic stirring device, and the masses are weighed to obtain M, respectively. 0上 =2113.5g, M 0中 =2232.4g, M 0下 =2293.2g;
[0095] P2. Place the samples at the upper, middle and lower positions in step P1 in an asphalt combustion furnace and burn them at 540°C for 70 minutes. Weigh the mass and obtain M 1上 =2012.3g, M 1中 =2131.2g, M 1下 =2173.6g;
[0096] P3, the samples at the upper, middle and lower positions in step P2 are measured by the displacement method to obtain the volumes V 上 =708.1cm 3 、V 中 =741.0cm 3 、V 下 =801.2cm 3 ;
[0097] P4. Calculate the deviation Δρ of the average density of samples at the upper, middle and lower positions; calculate the deviation ΔR of the average volumetric dosage of asphalt;
[0098] P5, ΔR in step P4 = 0.0126 g / cm3 , greater than 0.01g / cm 3 That is, the asphalt mixture containing steelmaking waste residue in this embodiment is not mixed evenly.
[0099] At the same time, according to the Technical Specifications for Highway Asphalt Pavement Construction (JTG F40-2004), the samples taken from the upper, middle and lower sampling holes of Example 3 were respectively subjected to the traditional screening method to test the mixing uniformity of the asphalt mixture. If one or more key sieve holes do not meet the requirements of the specification, it is judged to be unqualified, that is, the mixing is uneven. The screening results are shown in Table 3.
[0100] Table 3 Screening results of samples taken from different sampling holes (mixing for 50 seconds)
[0101]
[0102] The passing rates of 4.75 mm and 9.5 mm sieve holes in Table 3 do not meet the requirements, and the mixed materials are not mixed evenly. The determination results of the method of the present invention are consistent with those of the traditional standard method.
[0103] Example 4
[0104] The mixing method of the asphalt mixture containing steelmaking waste slag in this embodiment is basically the same as that in Example 1, except that: the mixing time in step S3 is 55s; in terms of mass percentage, the asphalt mixture containing steelmaking waste slag includes a mixture of 20% steelmaking waste slag and coarse aggregate, 65% fine aggregate, 10% mineral powder and 5% asphalt.
[0105] This embodiment also provides a method for evaluating the uniformity of the above-mentioned asphalt mixture containing steelmaking waste residue, comprising the following steps:
[0106] P1. For the asphalt mixture containing steel slag mixed in step S3 of this embodiment, samples are taken from the upper, middle and lower sampling ports of the magnetic stirring device, and the masses are weighed to obtain M, respectively. 0上 =2135.5g, M 0中 =2316.3g, M 0下 =2282.6g;
[0107] P2. Place the samples at the upper, middle and lower positions in step P1 in an asphalt combustion furnace and burn them at 530°C for 65 minutes. Weigh the mass and obtain M 1上 =2033.2g, M 1中 =2207.1g, M 1下 =2171.8g;
[0108] P3, the samples at the upper, middle and lower positions in step P2 are measured by the displacement method to obtain the volumes V 上 =703.5cm 3 、V中 =760.3cm 3 、V 下 =776.8cm 3 ;
[0109] P4. Calculate the deviation Δρ of the average density of samples at the upper, middle and lower positions; calculate the deviation ΔR of the average volumetric dosage of asphalt;
[0110] P5, Δρ=0.107 g / cm in step P4 3 , less than 0.2g / cm 3 ; ΔR in step p4 = 0.0028 g / cm 3 , less than 0.01g / cm 3 That is, the asphalt mixture containing steelmaking waste residue in this embodiment is not mixed evenly.
[0111] At the same time, according to the Technical Specifications for Highway Asphalt Pavement Construction (JTG F40-2004), the samples taken from the upper, middle and lower sampling holes of Example 4 were respectively subjected to the traditional screening method to test the mixing uniformity of the asphalt mixture. If one or more key sieve holes do not meet the requirements of the specification, it is judged to be unqualified, that is, the mixing is uneven. The screening results are shown in Table 4.
[0112] Table 4 Screening results of samples taken from different sampling holes (mixing for 55 seconds)
[0113]
[0114] The key sieve hole pass rates in Table 4 all meet the requirements, and the mixture is mixed evenly. The determination results of the method of the present invention are consistent with those of the traditional standard method.
[0115] The results of the above examples 1-4 show that the determination results of the uniformity evaluation method of the present invention are consistent with those of the conventional standard method, indicating that the uniformity evaluation method of the present invention has a reliable evaluation structure. The parameter settings in the uniformity evaluation method of the present invention are accurate and reasonable.
[0116] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.
Claims
1. A mixing method for asphalt mixture containing steelmaking waste residue, characterized in that: The following steps are involved: The same volume of steel waste slag and coarse aggregate are suspended in a magnetic stirring device respectively, and the magnetic field strength of the electromagnet is adjusted so that the steel waste slag and the coarse aggregate are subjected to the same gravity to obtain a balanced current; wherein the electromagnet is located at the upper part of the magnetic stirring device; Raw materials including the steelmaking waste slag, the coarse aggregate, the fine aggregate, the mineral powder and the asphalt are added into the magnetic stirring device, the electromagnet is energized and the balanced current is maintained, and the mixture is stirred to obtain an asphalt mixture containing the steelmaking waste slag.
2. The mixing method according to claim 1, characterized in that: The steelmaking waste slag includes at least one of blast furnace ironmaking slag, converter slag, open-hearth slag and electric furnace slag generated in the steel smelting process.
3. The mixing method according to claim 1, characterized in that: The mixing time is not less than 55s.
4. The mixing method according to claim 1, characterized in that: Calculated by weight percentage, the steelmaking waste slag asphalt mixture includes a mixture of 20-60% steelmaking waste slag and coarse aggregate, 25-65% fine aggregate, 0-10% mineral powder and 2-6% asphalt.
5. The mixing method according to claim 1, characterized in that: The particle sizes of the steelmaking waste slag and coarse aggregate are both 4.75-19 mm.
6. The mixing method according to claim 1, characterized in that: The method for obtaining the balancing current comprises the following steps: The steelmaking waste slag and coarse aggregate are placed in containers of the same weight, and then the containers are hung under the dynamometer, and the steelmaking waste slag and coarse aggregate are placed at the same height in the magnetic stirring device; The power supply of the electromagnet is turned on, and the current intensity in the electromagnet is adjusted. When the readings of the two dynamometers hanging the steelmaking waste slag and the coarse aggregate are observed to be the same, the current of the electromagnet is recorded as the balance current.
7. The mixing method according to claim 1, characterized in that: A feed port and an electromagnet are provided at the top of the magnetic stirring device, stirring devices are provided on the inner walls on both sides, the stirring device comprises a stirring shaft, a fixed gear shaft and stirring teeth, the fixed gear shaft is fixedly connected to the stirring shaft, a plurality of stirring teeth are fixedly connected to the fixed gear shaft, the fixed gear shaft of the stirring device on one side is longer than the fixed gear shaft of the stirring device on the other side; a discharge baffle and a discharge port are provided at the bottom of the magnetic stirring device.
8. The mixing method according to claim 7, characterized in that: Electromagnets are symmetrically arranged on the upper part of the inner wall of the magnetic stirring device.
9. A method for evaluating the uniformity of asphalt mixture containing steelmaking waste residue, characterized in that: The following steps are involved: For the mixed asphalt mixture containing steelmaking waste residue, samples were taken at the upper, middle and lower positions, and the masses were recorded as M 0上 、M 0中 、M 0下 ; The samples at the upper, middle and lower positions are burned respectively, and the mixture without asphalt is obtained after burning. The mass is weighed and recorded as M 1上 、M 1中 、M 1下 ; Determine their volumes and record them as V 上 、V 中 、V 下 ; The deviation Δρ of the average density of the samples at the upper, middle and lower positions is calculated according to formula I; the deviation ΔR of the average volumetric dosage of asphalt is calculated according to formula II; wherein, (Formula I); (Formula II); According to the deviation Δρ of the average density of the samples at the upper, middle and lower positions and the deviation ΔR of the average volume of asphalt, the mixing uniformity of the asphalt mixture containing steelmaking waste residue is judged according to the following method: When Δρ≤0.2g / cm 3 And ΔR≤0.01g / cm 3 When mixing, the mixture is evenly mixed; When Δρ>0.2g / cm 3 or ΔR>0.01g / cm 3 The mixture is not mixed evenly.
Citation Information
Patent Citations
Electroslag smelting casting device with additional electromagnetic stirring and method
CN101480715A
Method for preparing composite steel slag carbonized bricks
CN107879704A
Emulsified asphalt cold paving material
CN108033711A
Evaluation method for mixing uniformity of cement stabilized macadam mixture
CN113552121A
Magnetic field auxiliary powder distribution device and method for magnetic powder filling cavity
CN117282963A