Plasmon TiN / TiO2-x heterostructure rich in oxygen vacancies, synthesis method of plasmon TiN / TiO2-x heterostructure and application of plasmon TiN / TiO2-x heterostructure in nitrogen fixation and ammonia synthesis
By introducing the synergistic effect of oxygen vacancies and plasmon TiN on the surface of TiO2, a TiN/TiO2-x heterostructure rich in oxygen vacancies was prepared, which solved the problems of high energy consumption of existing ammonia synthesis and poor responsiveness of photocatalysts to visible light. , achieving efficient photonitrogen fixation and ammonia synthesis effect.
Patent Information
- Application Number
- CN202411184733.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The synthesis of existing ammonia depends on the high temperature and high pressure Harber-Bosch method, which consumes a lot of energy and generates a large amount of greenhouse gas CO2, making it difficult to achieve green and sustainable ammonia preparation, and the TiO2 photocatalyst has poor responsiveness to visible light, making it difficult to effectively utilize solar energy.
By introducing plasmon TiN/TiO2-x heterostructure of oxygen vacancies, combined with in-situ oxidation method and NaBH4 reduction method, the oxygen vacancies concentration on the surface of the catalyst is adjusted, and the light absorption capacity of the catalyst and the adsorption and activation capacity of nitrogen molecules are improved. , photo-fixed nitrogen under visible light to synthesize ammonia.
The rate of ammonia synthesis by photonitrogen fixation was significantly improved. The rate of catalytic ammonia generation in TiN/TiO2-x heterostructure reached 40.35 µmol g-1h-1 under visible light, which was better than TiN and TiO2 alone, and maintained the crystal structure and stability of the catalyst. sex.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of material chemistry, and specifically relates to a plasmonic TiN / TiO rich in oxygen vacancies 2-x Heterostructures, methods for their synthesis and their use in nitrogen fixation and ammonia synthesis. Background Art
[0002] Nitrogen (N 2 ) is one of the main components of the Earth's atmosphere, accounting for about 78.1% of the air. 2 The molecular bond energy is high (945 kJ / mol), making N 2 It is very stable and difficult to be used directly by humans. Nitrogen molecules need to be fixed into ammonia or nitrogen oxides before they can be used by organisms. As one of the most important basic chemicals in the world, ammonia has a wide range of uses in modern industrial and agricultural production. In addition, ammonia is a hydrogen-rich compound and can also be used as a hydrogen storage carrier. By decomposing ammonia to produce hydrogen, it can solve the problems of low-cost and long-distance transportation of hydrogen energy, and further expand the scale of the hydrogen energy industry. Therefore, the large-scale synthesis of ammonia is crucial to human development. However, the current synthesis of ammonia relies on the traditional industrial Harber-Bosch method, which requires high temperature and high pressure, consumes a lot of energy and produces a large amount of greenhouse gas CO. 2 Therefore, it is urgent to develop green ammonia production methods. 2 Using water molecules as raw materials to provide protons, ammonia is generated under the drive of sustainable solar energy, which has the advantages of being economical, green, sustainable and environmentally friendly.
[0003] Semiconductor TiO 2 Photocatalysts have the advantages of good stability, simple synthesis, low cost, and no secondary pollution. They are widely used in photocatalytic water splitting to produce hydrogen, photocatalytic CO 2 reduction, photo-nitrogen fixation, and ammonia synthesis. However, TiO 2 The band gap is wide and only responds to ultraviolet light, making it difficult to absorb and utilize visible light, which accounts for a large proportion of sunlight. Plasmonic nanomaterials, including metal and non-metal nanostructures, can be used as photosensitizers to modify and improve TiO 2 The carrier concentration of plasmonic TiN is close to that of Au nanoparticles, and it also has the advantages of low price and wide light capture range. 2 Composite, is expected to improve the photocatalytic performance of the catalyst. 2 The adsorption and activation of molecules are the key steps in the conversion of nitrogen molecules. The introduction of active sites (including vacancies, metal unsaturated sites, metal promoters, etc.) on the catalyst surface is crucial for the efficient synthesis of ammonia. 2The construction of abundant oxygen vacancies on the surface is crucial to improving the efficiency of photo-nitrogen fixation to synthesize ammonia. Summary of the invention
[0004] The present invention aims to provide a plasmonic TiN / TiO rich in oxygen vacancies. 2-x Heterostructure, synthesis method thereof and application thereof in nitrogen fixation and ammonia synthesis. The method of introducing oxygen vacancies in the present invention is simple and easy to operate, and the concentration of oxygen vacancies on the catalyst surface can be regulated by changing the reaction time. Due to the introduction of TiN, the light absorption capacity of the prepared catalyst is improved, and the construction of oxygen vacancies is conducive to the adsorption and activation of nitrogen molecules by the catalyst. Based on the synergistic effect of plasmon effect and oxygen vacancies, the prepared TiN / TiO 2-x The rate of photo-nitrogen fixation and ammonia synthesis in heterojunction is significantly higher than that of TiN and TiO 2 and TiO 2-x .
[0005] The present invention combines the in-situ oxidation method and NaBH 4 Reduction method to prepare TiN / TiO with localized surface plasmon resonance effect and rich oxygen vacancies 2-x Heterostructure, the synthesized TiN / TiO 2-x It has excellent catalytic activity for synthesizing ammonia under visible light.
[0006] TiN / TiO for photo-nitrogen fixation and ammonia synthesis according to the present invention 2-x The preparation method and specific steps of the heterojunction are as follows: (1) Commercial TiN nanoparticles were placed in an alumina crucible and calcined in a muffle furnace at a specific temperature to obtain TiN / TiO 2 Heterogeneous structures; (2) The obtained TiN / TiO 2 Use H 2 / N 2 atmosphere or in NaBH 4 Reduction treatment in aqueous solution to form TiN / TiO 2 TiN / TiO was prepared by introducing oxygen vacancies on the surface 2-x Heterogeneous structure.
[0007] Furthermore, in step (1), the volume of the alumina crucible is 50 mL, and the appropriate amount of TiN nanoparticles added is 0.2 g. If the amount added is too low, the product is small, and if the amount added is too high, uneven oxidation is caused. In step (1), the calcination temperature is 350-450°C, and the calcination time is 2-12 h. Preferably, in step (1), the calcination temperature is 400°C, and the time is 2, 4, 6 and 12 h, respectively.
[0008] Furthermore, in step (2), H 2 / N2 The heat treatment temperature in the atmosphere is 350-450°C and the time is 2-12 h. Specifically, in step (2), H 2 / N 2 The heat treatment temperatures are 350℃, 400℃ and 450℃, and the reaction times are 2 and 12 h, respectively.
[0009] Furthermore, in step (2), NaBH 4 The temperature of the reduction treatment is 30-60°C, and the reaction time is 1-24 h. Specifically, in step (2), NaBH 4 The reduction temperatures were 30°C and 60°C, and the reaction times were 1, 2, 4, 6 and 24 h, respectively.
[0010] Furthermore, in step (2), H 2 / N 2 Atmosphere 2 and N 2 The volume ratio is (5~10): (90~95), H 2 / N 2 The gas flow rate of the mixed gas is 10~100 mL / min, NaBH 4 The concentration of the aqueous solution is 0.1~0.5 mol / L.
[0011] Furthermore, H 2 / N 2 Mixed gas heat treatment, 30℃ NaBH 4 and 60℃ NaBH 4 Reducing TiN / TiO 2-x Named TiN / TiO 2-x -H y 、TiN / TiO 2-x -N30 and TiN / TiO 2-x -N60.
[0012] Plasmonic TiN / TiO prepared by the above preparation method 2-x Heterogeneous structure.
[0013] The above TiN / TiO 2-x Application of heterostructures as photocatalysts for catalytic nitrogen fixation and ammonia synthesis under light irradiation.
[0014] Furthermore, in order to avoid the interference of the hole sacrificial agent on the detection method, TiN / TiO 2-x The heterogeneous structure was added to pure water, and after being uniformly dispersed by ultrasonication, it was irradiated with a light source with a wavelength of 420 nm to 780 nm under nitrogen atmosphere and stirring.
[0015] The light source is a 300 W xenon lamp equipped with a 420 nm cut-off filter. Preferably, the light power density is 200-300 mW / cm 2 , nitrogen flow rate is 20~100 mL / min.
[0016] Furthermore, 1.5 mL of sample was taken every 1 h, and Nessler's reagent was used to determine the concentration of Hg in the sample according to the 2[HgI 4 ] 2- + NH 3 + 3OH - →Hg 2 ONH 2 I + 7I - + 2H 2 O, detect the ammonia concentration in the solution, end the reaction after 3 h, and calculate the rate of ammonia synthesis under visible light.
[0017] The present invention combines NaBH with in situ oxidation 4 The plasmonic TiN / TiO rich in oxygen vacancies was prepared by reduction method. 2-x Heterojunction. Due to the localized surface plasmon resonance effect of TiN, the spectral absorption range of the catalyst is significantly broadened. The abundant oxygen vacancies on the surface provide reaction sites for the adsorption and activation of nitrogen molecules, and the catalyst exhibits excellent photo-nitrogen fixation and ammonia synthesis activity. λ ≥ 420 nm), due to the lack of adsorption sites for nitrogen molecules on the TiN surface, TiO 2 The visible light responsiveness of TiO2 is low, and the photo-nitrogen fixation activity of both is very low. The introduction of oxygen vacancies can not only provide reaction sites for synthesizing ammonia, but also increase the light response range of the catalyst, making TiO2 2-x The ammonia synthesis rate increased to 8.27 µmol g -1 h -1 Due to the lack of sufficient reaction sites, TiN / TiO 2 The ammonia synthesis rate is only 3.12 µmol g -1 h -1 Under the synergistic effect of plasmonic TiN and oxygen vacancies, H 2 / N 2 and NaBH 4 TiN / TiO obtained by reduction method 2-x The photo-nitrogen fixation and ammonia synthesis activities of the heterogeneous structures were significantly improved. 4 TiN / TiO obtained by reduction for 4 h 2-x The ammonia synthesis rate was the highest, at 40.35 µmol g -1 h -1 , is a single component TiO 2-xThe rate of ammonia synthesis by different reduction methods is different, indicating that the appropriate oxygen vacancy concentration is crucial to the improvement of ammonia synthesis activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 TiN and TiN / TiO obtained by calcining at different times 2 、TiO 2 (a) UV-visible absorption spectrum and (b) X-ray diffraction pattern of .
[0019] Figure 2 TiN, TiO 2 、TiN / TiO 2 and TiN / TiO 2-x UV-visible absorption spectrum (a) and X-ray diffraction pattern (b) of -N30, in which TiO 2 The product of TiN calcined for 12 h, TiN / TiO 2 The product of TiN calcined for 4 h, TiN / TiO 2-x -N30 stands for TiN / TiO 2 At 30℃ NaBH 4 Samples after solution reduction for 4 h.
[0020] Figure 3 TiN (a), TiO 2 (b) TiN / TiO 2 (c) and TiN / TiO 2-x -SEM image of N30 (d).
[0021] Figure 4 TiN (a), TiO 2 (b) TiN / TiO 2 (c) and TiN / TiO 2-x -Transmission electron microscopy image of N30 (d).
[0022] Figure 5 H 2 / N 2 Mixed gas reduction (a), 30℃ NaBH 4 Reduction (b) and 60 °C NaBH 4 TiN / TiO prepared by reduction (c) method 2-x Electron paramagnetic resonance spectrum of the heterojunction and comparison with other samples (d).
[0023] Figure 6 TiN, TiO 2 、TiO 2-x 、TiN / TiO 2、TiN / TiO 2-x -H450, TiN / TiO 2-x -N30 and TiN / TiO 2-x -N60 photo-nitrogen fixation rate diagram for ammonia synthesis, TiN / TiO 2-x -H450 is H 2 / N 2 The sample reduced by mixed gas at 450℃ for 2 h, TiN / TiO 2-x -N30 is NaBH 4 The solution was reduced at 30℃ for 4 h, TiN / TiO 2-x -N60 is NaBH 4 The solution was reduced at 60 °C for 4 h. DETAILED DESCRIPTION
[0024] In order to make the technical purpose, technical solution and beneficial effects of the present invention clearer, the technical solution of the present invention is further described below in conjunction with specific examples, but the protection scope of the present invention is not limited thereto. The water used in the experiment was 18.2 MΩ ultrapure water, and the purchased drugs were all analytically pure.
[0025] Example 1 (1) TiN / TiO 2 and TiO 2 Preparation of nanostructures 0.2 g of TiN nanoparticles were spread in a 50 mL alumina crucible and then transferred to a muffle furnace and calcined at 400 °C for 2 h, 4 h, 6 h, and 12 h, respectively. As the calcination time increased, the TiN nanoparticles first transformed into TiN / TiO 2 Heterojunction, further transformed into TiO 2 Nanoparticles, TiO 2 It is the product of TiN calcined for 12 h.
[0026] (2) H 2 / N 2 Preparation of TiN / TiO by mixed gas reduction 2-x Heterojunction according to Figure 1 UV-visible absorption spectrum and X-ray diffraction pattern of TiN / TiO obtained by calcining TiN for 4 h 2 TiN and TiO 2 The ratio of TiN to TiO is moderate, so the product of TiN calcined for 4 h was selected as the preparation of TiN / TiO 2-x Take 0.2g TiN / TiO 2 The powder was spread evenly on an alumina crucible boat and then heated in H 2 / N 2 In the mixed gas (H2 and N 2 The volume ratio of TiN / TiO was 5:95, and the gas flow rate was 50 mL / min) and calcined at 350℃ for 2h and 12h, 400℃ for 2h and 12h, and 450℃ for 2h and 12h, respectively, to introduce oxygen vacancies on the catalyst surface. The oxygen vacancy concentration was regulated by changing the calcination temperature and time. 2 The product obtained by calcination at 450 °C for 2 h was named TiN / TiO 2-x -H450.
[0027] (3) NaBH 4 Preparation of TiN / TiO by reduction 2-x Heterojunction Take 0.1 g TiN / TiO 2 Powder dispersed in NaBH 4 The solution (0.1 mol / L, 40 mL) was ultrasonically mixed for 10 min and then reduced at 30℃ or 60℃ for 1, 2, 4, 6, and 24 h. The products obtained by reduction at 30℃ and 60℃ for 4 h were named TiN / TiO 2-x -N30 and TiN / TiO 2-x -N60.
[0028] Take 0.1g TiO 2 Powder dispersed in NaBH 4 The solution (0.1 mol / L, 40 mL) was mixed by ultrasound for 10 min and then reduced at 30 °C for 4 h. The obtained product was named TiO 2-x .
[0029] (4) Rate test of nitrogen fixation and ammonia synthesis by plasmonic TiN and its heterostructures under visible light 20 mg of the prepared catalysts (TiN, TiO 2 、TiO 2-x 、TiN / TiO 2 or TiN / TiO 2-x ) and 50 mL ultrapure water, and subjected to 100 W ultrasound for 3 min, and the reaction was carried out at room temperature. The light source used in the present invention to study the photocatalytic activity was a 300 W xenon lamp equipped with a 420 nm cutoff filter, i.e., a spectral range of λ ≥420 nm. Stirring and irradiation from the top, light power density 250 mW / cm 2Before the light source is turned on, the reaction solution is pre-blown with nitrogen for 30 minutes (gas flow rate: 100 mL / min) to fill the reaction solution and the reactor with nitrogen. Then the nitrogen flow rate is adjusted to 50 mL / min and the light source is turned on. 1.5 mL of the reaction solution is taken with a 5 mL syringe at 0, 1 h, 2 h and 3 h of illumination and transferred to a centrifuge tube. After the reaction is completed and the sampling is completed, centrifuge at 8000 rpm for 10 min, and the supernatant is taken out and filtered again with a 0.22 µm needle filter to ensure that there is no catalyst residue in the test solution. Take 1 mL of the supernatant of each sample after secondary filtration and add it to a 1.5 mL cuvette. Then potassium sodium tartrate solution (0.25 mL, 0.2 mol / L) and Nessler's reagent (0.25 mL) are added to each cuvette in turn. Mix well and place for 20 minutes. After sufficient reaction, perform UV test. The tetraiodine mercuric ions in Nessler's reagent will react with ammonia in the reaction solution to form a brick red precipitate with UV absorption at 420 nm. The ultraviolet absorption of the solution at different reaction times at 420 nm was detected by UV-visible spectrophotometer, and the ammonia concentration of the reaction solution and the ammonia generation rate within 4 h were calculated.
[0030] and TiN / TiO after heat treatment 2 Absorption spectrum and X-ray diffraction pattern characterization Appropriate amounts of TiN and TiN products treated in a muffle furnace for different times were uniformly and tightly attached to the surface of a barium sulfate substrate. Barium sulfate was used as a reference, an integrating sphere accessory was installed, and a Hitachi U-4100 UV-Vis-NIR spectrometer was used to collect the absorption spectrum of the sample. The plasmon effect of TiN made it still absorb after 800 nm, so the absorption spectrum scanning range was 300-1400 nm. After the spectrum test was completed, computer software was used to draw the graph, as shown in the following figure. Figure 1 As shown in a. As can be seen from the figure, with the extension of calcination time, the plasmon resonance absorption intensity of TiN in the long wavelength (λ>600 nm) range gradually decreases, indicating that more TiN is oxidized to TiO 2 When the calcination time is 6 h, the plasmon resonance absorption of TiN becomes less obvious. When the calcination time is extended to 12 h, the plasmon resonance absorption of TiN is no longer observed, indicating that TiN has been completely transformed into TiO 2 .
[0031] An appropriate amount of TiN and its oxide powders were uniformly pressed into a glass groove substrate and characterized by X-ray diffraction patterns using a Bruker D8 Advance instrument. Figure 1 b. For the convenience of comparison, TiN and anatase TiO 2The PDF card is also shown in the figure. As can be seen from the figure, with the increase of calcination time, the TiN content in the sample gradually decreases, and the TiO 2 When the calcination time is 6 h, the diffraction peak of TiN is basically not observed. Figure 1 The absorption spectrum of a shows that TiN is completely transformed into TiO after calcination in a muffle furnace for 12 h. 2 .
[0032] 、TiO 2 、TiN / TiO 2 and TiN / TiO 2-x -N30 absorption spectrum and X-ray diffraction pattern characterization like Figure 2 a is TiN, TiO 2 、TiN / TiO 2 and TiN / TiO 2-x -UV-visible absorption spectrum of N30, compared with TiN / TiO 2 , TiN / TiO rich in oxygen vacancies 2-x -N30 has an enhanced absorption intensity in the long wavelength range, indicating that NaBH 4 The oxygen vacancies introduced by reduction can provide reaction sites for the adsorption and activation of nitrogen molecules, and can also improve the photon capture ability of the catalyst, thereby facilitating the increase in the rate of photo-nitrogen fixation and ammonia synthesis. Figure 2 From the X-ray diffraction pattern of b, it can be seen that after the introduction of oxygen vacancies, the diffraction peak position and intensity of the catalyst did not change significantly, indicating that after the introduction of oxygen vacancies, the catalyst can still maintain a good crystal structure.
[0033] 、TiO 2 、TiN / TiO 2 and TiN / TiO 2-x Scanning electron microscopy characterization of -N30 0.5 mg of catalyst (TiN, TiO 2 、TiN / TiO 2 or TiN / TiO 2-x -N30) was dispersed in 0.5 mL of deionized water and dispersed evenly by ultrasonication for 10 min. Then 20 μL of the solution was added dropwise to the surface of the silicon wafer and dried naturally. The surface morphology was characterized by scanning electron microscopy. The scanning electron microscope model was Quanta 250 FEG FEI. Figure 3 shown. Figure 3 a is a scanning electron microscope image of TiN. It can be seen that the TiN nanostructure is composed of particles with a size of about 20 nm, and the monodispersity is not very good. Figure 3 b, c and d are TiO 2、TiN / TiO 2 and TiN / TiO 2-x -N30 scanning electron microscope image shows that the morphology of TiN does not change significantly after calcination and reduction treatment.
[0034] 、TiO 2 、TiN / TiO 2 and TiN / TiO 2-x Transmission electron microscopy characterization of -N30 The dispersion of the above photocatalyst was added dropwise onto the copper mesh supported by the carbon film and dried naturally. The microstructure was characterized by transmission electron microscopy. The transmission electron microscope was a Tecnai G2 20 model with an accelerating voltage of 200 kV. Figure 4 shown. Figure 4 a, b, c and d are TiN, TiO 2 、TiN / TiO 2 and TiN / TiO 2-x Transmission electron microscopy image of -N30 shows that after in-situ oxidation and NaBH 4 After reduction treatment, the morphology of TiN did not change significantly, which is consistent with the results of scanning electron microscopy.
[0035] TiN / TiO prepared by different reduction methods 2-x Electron paramagnetic resonance spectra of heterojunction and comparison samples The electron paramagnetic spectroscopy characterization of the catalyst powder was carried out at room temperature using a Brucker EMXnano spectrometer. A capillary tube (inner diameter: 0.9-1.1 mm) with one end sealed was filled with sample powder about 1.5 cm high and placed in the sample chamber for testing. When oxygen vacancies are generated on the catalyst surface, free electrons are generated, which appear on the electron paramagnetic spectrum. g =2.003 peak. Figure 5 As shown in a, using H 2 / N 2 When the reduction temperature is 350℃ and 400℃, it is difficult to generate oxygen vacancies on the catalyst surface. Only when the reduction temperature is increased to 450℃, a small amount of oxygen vacancies can be introduced. 4 During reduction, obvious oxygen vacancy signals can be observed after reduction at room temperature (30 °C) for 1 h ( Figure 5 b) shows that at the same temperature NaBH 4 Reduction can be more effective in TiN / TiO 2 Oxygen vacancies are introduced on the surface. With the NaBH 4 As the reduction time increases, the oxygen vacancy content on the catalyst surface gradually increases. 4When the reduction temperature is increased to 60°C, more oxygen vacancies can be created on the surface in the same reaction time (≤ 6h) compared with the reduction at room temperature (30°C). Figure 5 b, c). However, when the reaction time was extended to 24 h, 30℃ NaBH 4 The oxygen vacancy concentration of the reduction product is higher than that at 60 °C, which may be due to the fact that more NaBH 4 Reaction with water (NaBH 4 + 2H 2 O = NaBO 2 + 4H 2 ↑), resulting in less H - Participate in the generation of oxygen vacancies.
[0036] Furthermore, electron paramagnetic spectroscopy was used to compare the TiN and TiO 2 、TiO 2-x (TiO 2 At 30℃NaBH 4 Reduction 4 h), TiN / TiO 2 and TiN / TiO 2-x (i.e. TiN / TiO 2-x -H450, TiN / TiO 2-x -N30 and TiN / TiO 2-x -N60) oxygen vacancy concentration. Figure 5 As shown in d, TiO 2 There are weak oxygen vacancy signals on the surface, which may be caused by a small amount of defects caused by long-term oxidation of TiN, which introduces unpaired electrons. 4 TiO obtained by reduction at room temperature (30°C) 2-x , the electron paramagnetic spectrum signal is enhanced, and the oxygen vacancies increase. By comparison, it is found that under the same reduction conditions (NaBH 4 , 30℃, 4 h), TiN / TiO 2-x The oxygen vacancy concentration of TiO 2-x , which is TiN / TiO 2-x The high nitrogen fixation activity of the heterogeneous structure provides the conditions.
[0037] Test of nitrogen fixation and ammonia synthesis rate of titanium nitride and titanium nitride / titanium oxide under visible light By comparing the generation rate of ammonia under different reduction conditions, it was found that the use of H 2 / N 2 The ammonia generation rate was the highest when the reduction temperature was 450℃ and the reaction time was 2 h. 4 When the reaction time is 4 h, the ammonia generation rate is the highest. 2、TiO 2-x (TiO 2 At 30℃NaBH 4 Reduction 4 h), TiN / TiO 2 、TiN / TiO 2-x -H450(TiN / TiO 2 Yu H 2 / N 2 450℃ reduction for 4 h), TiN / TiO 2-x -N30(TiN / TiO 2 At 30℃NaBH 4 Reduction 4h) and TiN / TiO 2-x -N60(TiN / TiO 2 60℃ NaBH 4 The rate of ammonia synthesis by photo-nitrogen fixation (4 h reduction). Figure 6 As shown, TiN has no obvious ammonia synthesis activity, TiO 2 The ammonia generation rate is also very low. 2 TiO obtained after oxygen vacancies were introduced on the surface 2-x The ammonia synthesis rate is 8.27 µmol g -1 h -1 . Due to TiN / TiO 2 There are not enough sites for nitrogen molecules to be adsorbed and activated on the surface, and the generation rate is low. After oxygen vacancies are introduced on the surface, thanks to the surface plasmon effect of TiN and the adsorption and activation function of oxygen vacancies on nitrogen molecules, TiN / TiO 2-x The ammonia synthesis rate of the heterogeneous structure is significantly improved. 2-x -H450, TiN / TiO 2-x -N30 and TiN / TiO 2-x The ammonia generation rates of -N60 were 12.85 µmol g -1 h -1 、40.35µmolg -1 h -1 and 25.78 µmol g -1 h -1 Although TiN / TiO 2-x -N60 has a higher oxygen vacancy concentration than TiN / TiO 2-x -N30, however, too high oxygen vacancy concentration will become the recombination center of photogenerated carriers, and the catalytic activity will be reduced. Therefore, TiN / TiO 2-x -N60 has a lower ammonia generation rate than TiN / TiO 2-x -N30, while TiN / TiO 2-x -N30 and TiN / TiO 2-x-N60 has a significantly higher ammonia generation rate than TiN / TiO 2-x -H450, NaBH 4 TiN / TiO prepared by reduction method 2-x The heterojunction has a higher ammonia synthesis rate, proving that NaBH 4 Reduction is an effective means to regulate the oxygen vacancy concentration of the catalyst and the rate of ammonia synthesis.
[0038] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A plasmonic TiN / TiO rich in oxygen vacancies 2-x A method for synthesizing a heterostructure, characterized in that: The following steps are involved: (1) Commercial TiN nanoparticles were placed in an alumina crucible and calcined in a muffle furnace at a specific temperature to obtain a TiN / TiO2 heterostructure. (2) The obtained TiN / TiO2 is heat treated in H2 / N2 atmosphere or reduced in NaBH4 aqueous solution to introduce oxygen vacancies on the surface of TiN / TiO2 to obtain TiN / TiO 2-x Heterogeneous structure.
2. The synthesis method according to claim 1, characterized in that In step (1), the calcination temperature is 350-450°C, and the calcination time is 2-12 h.
3. The synthesis method according to claim 1, characterized in that In step (2), the temperature of the heat treatment in the H2 / N2 atmosphere is 350-450°C and the time is 2-12 h.
4. The synthesis method according to claim 1, characterized in that The temperature of NaBH4 reduction treatment in step (2) is 30-60°C, and the reaction time is 1-24 h.
5. The synthesis method according to claim 1, characterized in that The volume ratio of H2 and N2 in the H2 / N2 atmosphere is (5~10):(90~95), the gas flow rate of the H2 / N2 mixed gas is 10~100 mL / min, and the concentration of the NaBH4 aqueous solution is 0.1~0.5 mol / L.
6. Plasmonic TiN / TiO prepared by the synthesis method according to any one of claims 1 to 5 2-x Heterogeneous structure.
7. TiN / TiO according to claim 6 2-x Application of heterostructures as photocatalysts for catalytic nitrogen fixation and ammonia synthesis under light irradiation.
8. The use according to claim 7, characterized in that: According to 1mg~2mg:5mL, TiN / TiO 2-x The heterogeneous structure was added into pure water, and after being uniformly dispersed by ultrasonication, it was irradiated with a light source with a wavelength of 420 nm to 780 nm under nitrogen atmosphere and stirring.
9. The use according to claim 8, characterized in that: The light source is a 300W xenon lamp equipped with a 420 nm cut-off filter.
Citation Information
Cited By
Porous floating type evaporator based on dynamic rotary self-cleaning and preparation method and application of porous floating type evaporator
CN120364784A
Preparation method of catalyst and catalyst
CN120961202A
Process for the preparation of a catalyst and catalyst
CN120961202B