Method for highly selectively preparing 2-cyclohexenol by electrocatalytic oxidation of cyclohexene

By using Co3O4 or Co3O4/PANI catalysts in the electrocatalytic oxidation of cyclohexene, the problem of low solubility of cyclohexene in aqueous electrolytes is solved, efficient electrocatalytic oxidation is achieved, and Faraday efficiency and product selectivity are improved. The separation treatment is simplified and the high selective preparation of cyclohexenol is promoted.

CN119040919APending Publication Date: 2024-11-29ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202253.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the low solubility of cyclohexene in aqueous electrolytes leads to a large-scale oxygen evolution reaction during electrolysis, the Faraday efficiency is low, and the product is difficult to separate from the electrolyte, which limits the practical application of electrocatalytic cyclohexene oxidation.

Method used

A device for electrocatalytic oxidation of cyclohexene is designed, using the catalyst Co3O4 or Co3O4/PANI. By performing electrocatalytic oxidation under mild conditions, it ensures that the catalyst always contacts and participates in the reaction during the organic phase reaction, and realizes organic after the reaction. The separation of phase and aqueous phase avoids separation treatment.

Benefits of technology

It significantly improves the Faraday efficiency of electrocatalytic oxidation of cyclohexene, improves the selectivity and purity of the product, simplifies the post-treatment process, solves the problems of diffusion of insoluble organic matter and product separation, and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040919A_ABST
    Figure CN119040919A_ABST
Patent Text Reader

Abstract

The invention discloses a method for high-selectivity preparation of 2-cyclohexenol by electrocatalytic oxidation of cyclohexene, the method utilizes an electrolysis device for electrocatalytic oxidation of cyclohexene to electrolyze cyclohexene, and the device comprises an electrolytic bath body, a storage part, a counter electrode, a working electrode and a reference electrode. An electrolyte solution is added into the electrolytic cell body, and the electrolytic cell body is sealed by a cell cover body. And cyclohexene is added into the storage part, a material adding opening is sealed through a material adding opening sealing plug, and then cyclohexene is electrolyzed for 2-5 h under the voltage of 1.3-1.8 V. In the device disclosed by the invention, the reaction does not need to separate the cyclohexene oxidation product from the electrolyte solution, so that complicated post-treatment is avoided, manpower and material resources are saved, and the purity of the product is improved; by adopting the device, the Faraday efficiency is improved, the selectivity of cyclohexene is obviously improved, the defects in the prior art are overcome, and the device has a very good application prospect in cyclohexene catalytic oxidation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalysis, and relates to a method for preparing 2-cyclohexenol with high selectivity by electrocatalytic oxidation of cyclohexene, and specifically relates to an electrolysis device for electrocatalytic oxidation of cyclohexene and a method for electrocatalytic oxidation of cyclohexene using the device. Background Art

[0002] With the maturity of the process of selective hydrogenation of benzene to prepare cyclohexene, the downstream applications of cyclohexene have developed rapidly. The CH oxidation of olefins can convert olefin compounds into alcohols, aldehydes, carboxylic acids and epoxides with higher added value. Among them, the selective oxidation of cyclohexene to prepare 2-cyclohexene-1-ol (cyclohexenol) has become a research hotspot. Cyclohexenol is an important raw material in the research fields of medicine, pesticides and materials. It can be used as a raw material for the synthesis of drugs or intermediates such as terpenes, Amaryllis alkaloids galantamine, dihydrocodone, etc. Therefore, the research on the selective oxidation of cyclohexene to prepare cyclohexenol has attracted much attention in recent years.

[0003] At present, the industrial oxidation of cyclohexene to cyclohexenol is usually carried out by catalytic oxidation under high temperature and high pressure, which has the problems of high energy consumption, low efficiency and difficult separation of products. However, the conversion of cyclohexene to cyclohexenol driven by renewable energy can produce valuable products in a mild way with lower energy consumption, so electrochemical synthesis has been widely developed. Electrochemical synthesis reactions can replace traditional redox reagents and do not require other toxic or dangerous redox reagents. In addition, in the process of electrochemical catalytic synthesis, the direction and speed of the reaction can be changed by adjusting the voltage and current of the electrode, and the selectivity of the target product can be significantly increased. At the same time, electrocatalytic synthesis simplifies the separation and purification of the product. In addition, electrochemical catalytic synthesis reactions can usually be carried out at room temperature and pressure, which is very beneficial for saving energy and reducing equipment investment, and the reaction is also safer. However, the low solubility of cyclohexene in aqueous electrolytes leads to a large degree of oxygen evolution reaction (OER) during the electrolysis process, resulting in a low Faraday efficiency (FE); and the product is difficult to separate from the electrolyte. This seriously limits and hinders the practical application of electrocatalytic cyclohexene oxidation. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a device for electrocatalytic oxidation of cyclohexene, which can ensure that the organic phase can always contact the catalyst during the reaction process and can continuously participate in the reaction, and does not use a co-solvent to participate in the reaction. After the reaction, the organic phase and the aqueous phase can be separated without the need for extraction treatment.

[0005] The present invention also provides the application of the device for electrocatalytic oxidation of cyclohexene in the electrocatalytic oxidation of cyclohexene, in which the catalyst Co3O4 or Co3O4 / PANI is used to electrocatalytically oxidize cyclohexene to cyclohexenol. By using the device and the corresponding catalyst, the reaction can be carried out under mild conditions, and the Faraday efficiency of the electrocatalytic oxidation of cyclohexene is significantly improved. The present invention is achieved by the following technical solutions:

[0006] First, the present invention provides an electrolysis device for electrocatalytic oxidation of cyclohexene, the device comprising: An electrolytic cell body, wherein a detachable cell cover for sealing is disposed on the top of the electrolytic cell body, an inner cavity is disposed in the electrolytic cell body, and an electrolyte is disposed in the inner cavity, and a flow hole penetrating the side wall is disposed in the middle and lower part of the side wall of the electrolytic cell body; A storage part, wherein a storage cavity is arranged inside the storage part, and a feeding port with a detachable feeding sealing plug is arranged on the top of the storage cavity; the storage part and the side wall of the electrolytic cell body on which the flow hole is arranged are detachably fitted and fixed; the side wall of the storage part close to the electrolytic cell body is also provided with a flow hole, and the flow holes on the electrolytic cell body and the side wall of the storage part are arranged in a corresponding position; A counter electrode, the counter electrode is fixedly disposed on the cell cover and inserted into the inner cavity of the electrolytic cell through the cell cover; A working electrode, the working electrode comprising carbon paper and copper tape, the carbon paper being sandwiched between the flow holes of the electrolytic cell body and the storage part, and the carbon paper being led out to the periphery of the storage part through the copper tape sandwiched in the gap between the electrolytic cell body and the storage part, and, A reference electrode is fixedly arranged on the cell cover and is inserted through the cell cover into the electrolyte in the inner cavity of the electrolytic cell.

[0007] Furthermore, the counter electrode is a graphite electrode, and the counter electrode is immersed in the electrolyte of the electrolytic cell body; the reference electrode is an Ag / AgCl electrode, and the reference electrode is immersed in the electrolyte of the electrolytic cell body.

[0008] Furthermore, the orthographic projection area of ​​the carbon paper of the working electrode is larger than the orthographic projection area of ​​the flow hole. The flow hole can be in a rectangular, square, circular or other shape.

[0009] Furthermore, the electrolytic cell body, the cell cover and the storage part may all be cylindrical or cubical, and the electrolytic cell body and the cell cover, and the electrolytic cell body and the storage part may be detachably fixedly connected by bolt fasteners.

[0010] Furthermore, a mating boss is integrally provided at the middle of the bottom surface of the cell cover, and the cross-sectional shape of the mating boss matches the cross-sectional shape of the inner cavity of the electrolytic cell. When assembled, the mating boss is inserted into the top of the inner cavity of the electrolytic cell; Preferably, a sealing ring is arranged on the periphery of the mating boss to achieve sealing.

[0011] The present invention provides application of an electrolysis device for electrocatalytic oxidation of cyclohexene in catalytic oxidation of cyclohexene.

[0012] Another object of the present invention is to provide a method for preparing 2-cyclohexenol by electrocatalytic oxidation of cyclohexene with high selectivity using an electrolytic device, comprising the following steps: S1. Preparation of working electrode: The catalyst is dispersed in an ethanol solution, and then Nafion (Nafion perfluorinated resin solution) is added and mixed evenly. Then the solution is dropped onto carbon paper, and a copper tape is taken and its end is bonded to the carbon paper to obtain a working electrode. The ethanol solution is preferably ethanol or an ethanol aqueous solution; S2, connecting an electrolytic device for electrocatalytic oxidation of cyclohexene to perform electrocatalytic oxidation of cyclohexene: (1) Take the electrolytic cell body and storage part of the device, and make the side wall of the electrolytic cell body with the flow hole fit tightly with the side wall of the storage part with the flow hole, and clamp the working electrode between the two side walls. The carbon paper sheet is placed between the two flow holes, and the copper tape bonded to the carbon paper extends upward to the outside of the electrolytic cell body, and then fix the electrolytic cell body and the storage part with bolts; (2) Add electrolyte solution to the electrolytic cell and seal it with a cell cover. Add cyclohexene to the storage unit and seal the filling port with a filling port sealing plug. Then connect the working electrode of the workstation with copper tape, and connect the counter electrode (graphite rod) and reference electrode (Ag / AgCl electrode) to the counter electrode and reference electrode of the workstation respectively, thus completing the connection of the device; (3) Turn on the electrochemical workstation and perform electrolysis at a voltage of 1.3 to 1.8 V for 2 to 5 hours.

[0013] Furthermore, the catalyst described in step S1 can be Co3O4 or Co3O4 / PANI.

[0014] And / or the catalyst is mixed with the ethanol solution by ultrasonic mixing.

[0015] Furthermore, in step (2), the electrolyte solution is a 1 mol / L potassium hydroxide solution, and the volume ratio of the potassium hydroxide solution to cyclohexene is 14-16:1-3; And / or, the usage ratio of the catalyst to cyclohexene is 5 mg: 1-3 ml.

[0016] Furthermore, the preparation method of the above-mentioned catalyst Co3O4 / PANI comprises the following steps: (1) Take aniline monomer, adjust its pH to 1-2 and stir evenly, then add ammonium persulfate, stir for 20-30 h, wash and dry to obtain polyaniline (PANI); (2) Soak Co3O4 and the PANI prepared in step (1) in ethanol, let stand for 20-30 hours, filter and dry to obtain PANI / Co3O4.

[0017] Furthermore, the reagent used to adjust the pH value of the aniline monomer in step (1) is preferably hydrochloric acid.

[0018] Furthermore, in step (1), after adjusting the pH value of the aniline monomer to 1-2, stirring is performed for 1 hour.

[0019] Furthermore, in step (1), the usage ratio of the aniline monomer to the ammonium persulfate is 4-6 ml: 1-1.5 g, and the usage ratio of the aniline monomer to the ammonium persulfate can be any value within this range.

[0020] Furthermore, in step (2), the mass ratio of PANI to Co3O4 is 0.8~1.2:0.8~1.2, wherein the mass ratio of PANI to Co3O4 can be any value within this range, preferably 1:1.

[0021] Furthermore, the drying obtained in step (1) and step (2) is performed at a drying temperature of 60-80° C. and a drying time of 9-15 h. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is one of the schematic diagrams of an electrolytic device for electrocatalytic oxidation of cyclohexene; in the figure, 1 represents an electrolytic cell body, 101 represents a cell body cover, 102 represents an electrolytic cell body cavity, 103 represents an electrolytic cell body flow hole, 2 represents a storage part, 201 represents a filler sealing plug, 202 represents a storage cavity, 203 represents a storage part flow hole, 3 represents a counter electrode, 4 represents a reference electrode, 5 represents a copper tape, and 6 represents a carbon paper sheet; Figure 2 The second schematic diagram of the electrolysis device for electrocatalytic oxidation of cyclohexene; Figure 3 A schematic diagram of a reaction of electrocatalytically oxidizing cyclohexene using an electrolysis device; Figure 4 LSV curves of catalyst Co3O4 and catalyst Co3O4 / PANI with and without cyclohexene; Figure 5This is the NMR spectrum of the sample obtained after catalytic oxidation of cyclohexene by Co3O4 / PANI; Figure 6 This is the Faraday efficiency diagram of the electrolysis of cyclohexene by the catalyst Co3O4 / PANI at different voltages; Figure 7 This is the NMR spectrum of the sample obtained after catalytic oxidation of cyclohexene by catalyst Co3O4; Figure 8 This is the Faraday efficiency diagram of the electrolysis of cyclohexene by catalyst Co3O4 at different voltages; Fig. 9 is the Faraday efficiency of the electrolytic catalytic oxidation of cyclohexene by the catalyst Co3O4 in the electrolysis device of the present invention and in a conventional electrolysis device; Fig.10 The Faraday efficiencies of the electrolytic catalytic oxidation of cyclohexene by the catalysts Co3O4 / PANI and Co3O4 at different voltages in the electrolysis device of the present invention.

[0023] The present invention has the following positive and beneficial effects: the device described in the present invention can effectively control the reaction interface, ensure that the organic phase can always contact the catalyst during the reaction process, and can continuously participate in the reaction, thereby improving the diffusion problem of insoluble organic matter on the electrode surface; and the device does not use a co-solvent to participate in the reaction during the electrocatalytic oxidation of cyclohexene, and the organic phase and the aqueous phase can be separated after the reaction, thereby avoiding the separation treatment of the organic phase and the aqueous phase after the reaction and avoiding the generation of sewage; In the device of the present invention, the reaction does not need to separate the cyclohexene oxidation product from the electrolyte solution, which not only avoids complicated post-treatment, saves manpower and material resources, but also improves the purity of the product; the use of this device improves the Faraday efficiency (reaching 83%), and the selectivity of cyclohexene is significantly improved, which solves the drawbacks of the prior art and has a very good application prospect in the catalytic oxidation of cyclohexene. DETAILED DESCRIPTION

[0024] The present invention is described in more detail below through specific implementation modes to facilitate understanding of the technical solution of the present invention, but is not intended to limit the protection scope of the present invention.

[0025] The reagents used in the experimental part of the present invention are all reagents known to those skilled in the art unless otherwise specified, and a CHI660E electrochemical workstation (Shanghai Chenhua) was used; Example 1 An electrolytic device for electrocatalytic oxidation of cyclohexene, comprising An electrolytic cell body 1, wherein a detachable cell cover 101 for sealing is disposed on the top of the electrolytic cell body, an inner cavity 102 is disposed in the electrolytic cell body, and an electrolyte is disposed in the inner cavity 102, and an electrolytic cell body flow hole 103 penetrating the side wall is disposed in the middle and lower part of the side wall of the electrolytic cell body; A storage part 2, wherein a storage cavity 202 is arranged inside the storage part, and a feeding port with a detachable feeding sealing plug 201 is arranged on the top of the storage cavity; the storage part 2 is detachably fitted and fixed to the side wall of the electrolytic cell body where the electrolytic cell body flow hole 103 is arranged; the storage part flow hole 203 is also arranged on the side wall of the storage part 2 close to the electrolytic cell body, and the flow holes on the electrolytic cell body and the storage part side wall are arranged in a corresponding position; A counter electrode 3, which is fixedly mounted on the cell cover 101 and inserted into the inner cavity 102 of the electrolytic cell through the cell cover 101; A working electrode, the working electrode comprising carbon paper 6 and copper tape 5 (the end of the copper tape is bonded to the carbon paper), the carbon paper 6 is sandwiched between the flow holes of the electrolytic cell body and the storage part, and the carbon paper 6 is led out to the upper part of the periphery of the storage part through the copper tape 5 sandwiched in the gap between the electrolytic cell body and the storage part, and, The reference electrode 4 is fixedly arranged on the cell cover and is inserted into the electrolyte in the inner cavity of the electrolytic cell through the cell cover.

[0026] The orthographic projection area of ​​the carbon paper of the working electrode is larger than the orthographic projection area of ​​the flow hole. The flow holes on the side wall of the electrolytic cell and the storage part are preferably squares with a side length of 1 cm (completely corresponding); the carbon paper sheet is preferably a square with a side length of 1.5 cm, and the thickness of the carbon paper is preferably 0.19 mm.

[0027] Wherein, the electrolytic cell body and the storage part are both cylindrical. Figure 1 As shown, the electrolytic cell body and the cell cover, and the electrolytic cell body and the storage portion are detachably fixedly connected by bolt fasteners.

[0028] In this embodiment, the length of the copper tape for bonding and connecting the carbon paper sheets is 10 cm.

[0029] Example 2 The same points as Example 1 will not be repeated here, except that the electrolytic cell body and the storage part are both cube-shaped, and the electrolytic cell body and the cell cover, and the electrolytic cell body and the storage part are detachably fixedly connected by bolt fasteners.

[0030] Embodiment 3 The same points as Embodiment 1 will not be repeated, except that a mating boss is integrally provided at the middle position of the bottom surface of the cell cover, and the cross-sectional shape of the mating boss matches the cross-sectional shape of the inner cavity of the electrolytic cell. In the assembled state, the mating boss is inserted into the top of the inner cavity of the electrolytic cell; Preferably, a sealing ring is arranged on the periphery of the mating boss to achieve sealing.

[0031] Example 4 One of the methods for preparing 2-cyclohexenol with high selectivity by electrocatalytic oxidation of cyclohexene using an electrolysis device for electrocatalytic oxidation of cyclohexene as described in the above examples comprises the following steps: S1. Preparation of working electrode: Take 5 mg Co3O4 / PANI and disperse it in 980 μL ethanol, then add 20 μL Nafion, mix it by ultrasonic for 15 min, drop the mixed solution on a 1.5 cm * 1.5 cm carbon paper, take a copper tape, stick its end to the carbon paper, and extend it upward for 10 cm to obtain a working electrode; S2, connecting an electrolytic device for electrocatalytic oxidation of cyclohexene to perform electrocatalytic oxidation of cyclohexene: (1) Take the electrolytic cell body and storage part of the device described in Example 1, and closely fit the side wall of the electrolytic cell body with the flow hole and the side wall of the storage part with the flow hole, and clamp the working electrode between the two side walls, and set the carbon paper sheet between the two flow holes. The copper tape bonded to the carbon paper extends upward to the outside of the electrolytic cell body, and then fix the electrolytic cell body and the storage part with bolts; (2) Add 1 mol / L potassium hydroxide solution into the electrolytic cell and seal it with the cell cover; add 1 mol / L potassium hydroxide solution into the storage part and seal the filling port with a filling port sealing plug; then use the copper tape bonded to the carbon paper loaded with Co3O4 catalyst as the working electrode, Ag / AgCl as the reference electrode, and the graphite rod as the counter electrode, and connect them to the corresponding electrode clips of the workstation respectively, turn on the electrochemical workstation, and open the CHI660E software.

[0032] Perform CV (cyclic voltammetry) test in the range of 1-1.8V to activate the catalyst; then perform LSV (linear sweep voltammetry) test in the range of 1-1.8V, and repeat the test until the curve is stable. Figure 4 shown by Figure 4 From the LSV curve, it can be seen that the Co3O4 / PANI catalyst has a current response with or without the addition of cyclohexene, and it can be seen that the current density increases after the addition of cyclohexene.

[0033] (3) Then the potassium hydroxide solution on one side of the reaction cell was sucked out, cyclohexene was added, and CV and LSV tests were performed at 1.0~1.8V. The results are as follows: Figure 4 As shown; then IT test was performed at 1.3~1.8V for 3h; After the reaction, samples were taken for product analysis and testing. The NMR spectrum was as follows: Figure 5 As shown, Figure 5 (Left) is the NMR spectrum of cyclohexenol standard sample. Figure 5(Right) is the NMR spectrum of the electrolyte after electrolysis. It can be seen that the peak shape and position of the NMR spectrum of the electrolyte are the same as those of the cyclohexenol standard sample, that is, the product is cyclohexenol. The Faraday efficiency of the reaction is calculated as Figure 6 As shown in the figure, it can be seen that the Faraday efficiency is highest at 1.5V, which can reach 83%.

[0034] The preparation method of the catalyst Co3O4 / PANI described in this embodiment comprises the following steps: (1) Take 1.5 ml of aniline monomer and add HCl to adjust its pH to 1-2. After stirring for 1 hour, add 0.36 g of ammonium persulfate, stir for 24 hours, wash with water, and dry at 70 °C for 12 hours to obtain PANI; (2) Take 25 mg of Co3O4 and 25 mg of PANI prepared in step (1), soak them in 1 ml of ethanol, let them stand for 24 h, filter them, and dry them at 70 °C for 12 h to obtain PANI / Co3O4.

[0035] Example 5 A second method for preparing 2-cyclohexenol with high selectivity by electrocatalytically oxidizing cyclohexene using an electrolytic device for electrocatalytically oxidizing cyclohexene as described in the above example comprises the following steps: S1. Preparation of working electrode: Take 5 mg Co3O4 and disperse it in 980 μL ethanol, then add 20 μL Nafion, mix it by ultrasonic for 15 min, drop the mixed solution on a 1.5 cm * 1.5 cm carbon paper, take a copper tape, stick its end to the carbon paper, and extend it upward for 10 cm to obtain a working electrode; S2, connecting an electrolytic device for electrocatalytic oxidation of cyclohexene to perform electrocatalytic oxidation of cyclohexene: (1) Take the electrolytic cell body and storage part of the device described in Example 1, and closely fit the side wall of the electrolytic cell body with the flow hole and the side wall of the storage part with the flow hole, and clamp the working electrode between the two side walls, and set the carbon paper sheet between the two flow holes. The copper tape bonded to the carbon paper extends upward to the outside of the electrolytic cell body, and then fix the electrolytic cell body and the storage part with bolts; (2) Add 1 mol / L potassium hydroxide solution into the electrolytic cell and seal it with the cell cover; add 1 mol / L potassium hydroxide solution into the storage part and seal the filling port with a filling port sealing plug; then use the copper tape bonded to the carbon paper loaded with Co3O4 catalyst as the working electrode, Ag / AgCl as the reference electrode, and the graphite rod as the counter electrode, and connect them to the corresponding electrode clips of the workstation respectively, turn on the electrochemical workstation, and open the CHI660E software.

[0036] Perform CV (cyclic voltammetry) test in the range of 1-1.8V to activate the catalyst; then perform LSV (linear sweep voltammetry) test in the range of 1-1.8V, and repeat the test until the curve is stable. Figure 4 shown by Figure 4 The LSV curve shows that the Co3O4 catalyst has a current response with or without cyclohexene, and the current density increases after the addition of cyclohexene. In addition, it can be seen that the performance of the Co3O4 / PANI catalyst is significantly improved compared with the current density of Co3O4 when cyclohexene is added, which shows that the introduction of PANI is beneficial to the electrocatalytic oxidation of cyclohexene.

[0037] (3) Then the potassium hydroxide solution on one side of the reaction tank was sucked out, cyclohexene was added, and CV and LSV tests were performed under the conditions of 1.0~1.8. The results are as follows: Figure 4 As shown; then cyclohexene was catalytically oxidized at 1.3~1.8V for 3h.

[0038] After the reaction, samples were taken for product analysis and testing. The NMR spectrum was as follows: Figure 7 As shown, Figure 7 (Left) is the NMR spectrum of cyclohexenol standard sample. Figure 7 (Right) is the NMR spectrum of the electrolyte after electrolysis. It can be seen that the peak shape and position of the NMR spectrum of the electrolyte are the same as those of the cyclohexenol standard sample, that is, the product is cyclohexenol. The Faraday efficiency of the reaction is calculated as Figure 8 shown.

[0039] Comparative Example Using Co3O4 as a catalyst, cyclohexene was electrolytically oxidized in a conventional reaction cell (conventional H-type reaction cell), and its Faraday efficiency (FE) at different voltages was measured. The results are as follows: Fig. 9 As shown. Fig. 9 It can be seen that under the condition of voltage 1.3-1.8 V, the Faraday efficiency of the reaction cell of the present invention for electrolytic catalytic oxidation of cyclohexene is much better than that of the conventional reaction cell. Therefore, the electrocatalytic oxidation of cyclohexene by the reaction cell of the present invention breaks through the bottleneck of the prior art, and the post-processing is simple and easy.

[0040] Fig.10 The IT test was carried out for 3 hours at different voltages for the catalysts Co3O4 / PANI and Co3O4, and the Faraday efficiency of the reaction was calculated. It can be seen that the Faraday efficiency of Co3O4 / PANI is higher than that of Co3O4 in the voltage range of 1.3-1.8V. It can also be seen that the Faraday efficiency of both catalysts is the highest at 1.5V, which can reach 83%.

Claims

1. An electrolysis device for electrocatalytic oxidation of cyclohexene, characterized in that: include An electrolytic cell body, wherein a detachable cell cover for sealing is disposed on the top of the electrolytic cell body, an inner cavity is disposed in the electrolytic cell body, and an electrolyte is disposed in the inner cavity, and a flow hole penetrating the side wall is disposed in the middle and lower part of the side wall of the electrolytic cell body; A storage part, wherein a storage cavity is arranged inside the storage part, and a feeding port with a detachable feeding sealing plug is arranged on the top of the storage cavity; the storage part and the side wall of the electrolytic cell body on which the flow hole is arranged are detachably fitted and fixed; the side wall of the storage part close to the electrolytic cell body is also provided with a flow hole, and the flow holes on the electrolytic cell body and the side wall of the storage part are arranged in a corresponding position; A counter electrode, the counter electrode is fixedly arranged on the cell cover and inserted into the inner cavity of the electrolytic cell through the cell cover; A working electrode, the working electrode comprising carbon paper and copper tape, the carbon paper being sandwiched between the flow holes of the electrolytic cell body and the storage part, and the carbon paper being led out to the periphery of the storage part through the copper tape sandwiched in the gap between the electrolytic cell body and the storage part, and, A reference electrode is fixedly arranged on the cell cover and is inserted through the cell cover into the electrolyte in the inner cavity of the electrolytic cell.

2. The electrolysis device for electrocatalytic oxidation of ethylene according to claim 1, characterized in that: The orthographic projection area of ​​the carbon paper of the working electrode is larger than the orthographic projection area of ​​the flow hole.

3. The electrolysis device for electrocatalytic oxidation of cyclohexene according to claim 1, characterized in that: The electrolytic cell body, the cell cover and the storage part can all be cylindrical or cubical, and the electrolytic cell body and the cell cover, and the electrolytic cell body and the storage part are detachably fixedly connected by bolt fasteners.

4. The electrolysis device for electrocatalytic oxidation of cyclohexene according to claim 8, characterized in that: A mating boss is integrally provided at the middle of the bottom surface of the cell cover, and the cross-sectional shape of the mating boss matches the cross-sectional shape of the inner cavity of the electrolytic cell. When assembled, the mating boss is inserted into the top of the inner cavity of the electrolytic cell; Preferably, a sealing ring is arranged on the periphery of the mating boss to achieve sealing.

5. A method for preparing 2-cyclohexenol with high selectivity by electrocatalytic oxidation of cyclohexene using the electrolysis device according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: S1. Preparation of working electrode: The catalyst is dispersed in an ethanol solution, and then Nafion is added and mixed evenly, and the mixed solution is dropped on carbon paper, and a copper tape is taken and its end is bonded to the carbon paper to obtain a working electrode; S2, connecting an electrolytic device for electrocatalytic oxidation of cyclohexene to perform electrocatalytic oxidation of cyclohexene: (1) Take the electrolytic cell body and the storage part of the device, and closely fit the side wall of the electrolytic cell body with the flow hole and the side wall of the storage part with the flow hole, and clamp the working electrode between the two side walls, and set the carbon paper sheet between the two flow holes. The copper tape bonded to the carbon paper extends upward to the outside of the electrolytic cell body, and then fix the electrolytic cell body and the storage part with bolts; (2) Add electrolyte solution into the electrolytic cell body and seal it with the cell cover; add cyclohexene into the storage part and seal the filling port with a filling port sealing plug; then connect the working electrode of the workstation with copper tape, and connect the counter electrode and reference electrode to the counter electrode and reference electrode of the workstation respectively, thus completing the connection of the device; (3) Turn on the electrochemical workstation and perform electrolysis at a voltage of 1.3 to 1.8 V for 2 to 5 hours.

6. The method according to claim 5, characterized in that The catalyst described in step S1 can be Co3O4 or Co3O4 / PANI.

7. The method according to claim 5, characterized in that The electrolyte solution in step (2) is a 0.8-1.2 mol / L potassium hydroxide solution, and the volume ratio of the potassium hydroxide solution to cyclohexene is 13-17:1-3; And / or, the usage ratio of the catalyst to cyclohexene is 5 mg: 1-3 ml.

8. The method according to any one of claims 5 to 7, characterized in that: The preparation method of the catalyst Co3O4 / PANI comprises the following steps: (1) Take aniline monomer, adjust its pH to 1-2 and stir evenly, then add ammonium persulfate, stir for 20-30 h, wash and dry to obtain PANI; (2) Soak Co3O4 and the PANI prepared in step (1) in ethanol, let stand for 20-30 hours, filter and dry to obtain PANI / Co3O4.

9. The preparation method according to claim 8, characterized in that: The dosage ratio of the aniline monomer to ammonium persulfate in step (1) is 4-6 ml: 1-1.5 g; the mass ratio of PANI to Co3O4 in step (2) is 0.8-1.2: 0.8-1.

2.