Method for reducing content of resin acid in softwood chemical-mechanical pulp wastewater

By using twin screw extrusion process and chemical agent treatment in the pulping process of needle pulping, combined with biological treatment, the problem of high resin acid content in wastewater is solved, and the source control of pollutants and effective reduction of wastewater treatment is achieved. , reducing costs and sludge expansion problems.

CN119041230AActive Publication Date: 2024-11-29INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411293930.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-29
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The high resin acid content in the wastewater of needle slurry is caused by the problems of sludge expansion, poor treatment effect and high cost during biological treatment.

Method used

The double-screw extrusion process is used to reduce the source of resin acid during the pulping process, and combine chemical agents and biological treatment. The biological treatment is carried out by mixing precipitation and filtrate to reduce the resin acid content in the wastewater.

Benefits of technology

It effectively reduces the resin acid content in the wastewater of needle pulp, simplifies the subsequent biological treatment process, reduces costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041230A_ABST
    Figure CN119041230A_ABST
Patent Text Reader

Abstract

The invention discloses a method for reducing the content of resin acid in softwood chemimechanical pulp wastewater. The method comprises the steps of reducing the source of resin acid and treating the tail end of wastewater through a twin-screw extrusion process. By means of the characteristics of efficient mixing and reaction of chemical agents in the twin-screw extrusion technology, the content of resin acid in wastewater in the coniferous wood chemical-mechanical pulping process is effectively reduced, secondary pollution is not generated in the treatment process, the environment-friendly effect is good, operation is easy, cost is low, and the method is suitable for large-scale industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of pulping wastewater treatment, and in particular to a method for reducing the resin acid content in coniferous wood chemical-mechanical pulping wastewater and its application. Background Art

[0002] In the pulping and papermaking industry, Chemimechanical Pulping (CMP) for coniferous wood is a common pulping method. This method has high production efficiency and low cost, but it will produce a large amount of wastewater containing resin acid during the production process. Resin acid mainly comes from the resin component in coniferous wood. Its chemical properties are stable and difficult to be naturally degraded, causing serious pollution to the environment. The current chemimechanical pulping production process is mainly designed for broad-leaved wood, and there is no targeted pretreatment method for resin acid in the whole process. Therefore, it is difficult to treat it using conventional processes, which seriously affects the subsequent pulping, papermaking and wastewater treatment processes.

[0003] Existing wastewater treatment methods mainly include physical treatment, chemical treatment and biological treatment. However, these methods have obvious limitations in removing resin acids. For example, physical treatment methods (such as precipitation, filtration, etc.) can only remove suspended solids and have limited effects on dissolved resin acids; although chemical treatment methods (such as coagulation, oxidation, etc.) can remove some resin acids, they are costly and prone to secondary pollution; biological treatment methods (such as activated sludge method, anaerobic treatment, etc.) have poor removal effects on resin acids and low treatment efficiency. At present, pulping wastewater containing resin acids is mainly removed in the wastewater treatment section, and there is currently no process method to effectively reduce the source of resin acids in the pulping process. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to solve the problems of high resin acid content in coniferous wood pulping wastewater, sludge swelling during biological treatment, poor treatment effect and high cost, and to provide a method and application for reducing the resin acid content in coniferous wood chemical-mechanical pulping wastewater.

[0005] Technical solution: To achieve the above objectives, the present invention provides a method and application for reducing the resin acid content in the wastewater of coniferous wood chemical-mechanical pulping, which mainly includes a twin-screw extrusion process to achieve the reduction of the resin acid source and the end treatment of the wastewater. The specific steps are as follows:

[0006] (1) Twin-screw extrusion process to achieve the reduction of resin acid source: cut softwood chips into 3-5 cm thin slices, wash with water, dehydrate and then steam, preferably steam at 105°C, to soften the fiber raw material and improve the subsequent liquid penetration effect; add the steamed chips to the first-stage twin-screw extruder (TSPI-I), add chemical agents for extrusion, and collect the first-stage extrusion wastewater; the extruded material is subjected to a first-stage chemical impregnation, and after the impregnation is completed, it is subjected to a second-stage twin-screw extrusion (TSPI-II), and the second-stage extrusion wastewater is collected; the material after the second-stage extrusion is subjected to a second-stage chemical impregnation with chemicals, and then the obtained material is subjected to normal pressure high-concentration pulping, washed with water, the pulp is dried and the pulp washing wastewater is collected, wherein a certain concentration is adjusted according to the actual situation on site to wash the pulp;

[0007] (2) Collect the first-stage squeezing wastewater, the second-stage squeezing wastewater and the pulp washing wastewater in step (1), configure the collected wastewater into comprehensive wastewater in proportion to the amount of wastewater generated in the pulping process, let the wastewater settle, and the obtained precipitate enters a plate and frame filter press for mud pressing. The filtrate obtained after mud pressing is mixed with the supernatant of the settled sedimentation and then subjected to biological treatment.

[0008] Preferably, in step (1), the coniferous wood raw material is pine or fir, and the coniferous wood raw material contains a high content of resin acid.

[0009] Preferably, in step (1), the pre-steaming time is 20-60 min.

[0010] In step (1), the chemical agent in the first twin-screw extruder section is any one or two of NaOH, aluminum sulfate and calcium hydroxide, wherein the total amount of chemical agents is 0.01-0.1wt% of the absolute dry material, preferably 0.03-0.08wt%.

[0011] Preferably, the chemical agents in the first twin-screw extruder section are NaOH and aluminum sulfate or NaOH and calcium hydroxide.

[0012] More preferably, the chemical agents in the first twin-screw extruder section are NaOH and aluminum sulfate, wherein the amount of sodium hydroxide is 0.01-0.03wt% of the absolute dry material, and the amount of aluminum sulfate is 0.02-0.05wt% of the absolute dry material. In a preferred embodiment, the amount of sodium hydroxide is 0.02wt% and the amount of aluminum sulfate is 0.03wt%.

[0013] NaOH is mainly used to soften the fiber and promote the absorption of aluminum sulfate or calcium hydroxide solution, so as to facilitate full reaction with resin acid.

[0014] Preferably, in step (1), the current of the first-stage twin-screw extruder and the second-stage screw extruder does not exceed 100A, and the rotation speed is 1000-1500 rpm.

[0015] The chemical impregnation chemicals are (NaOH), hydrogen peroxide (H2O2), sodium silicate (Na2SiO3) and diethylenetriaminepentaacetic acid (DTPA) chelating agent, and the dosage is 0.5-5wt%, 0.5-5wt%, 0.1-1wt% and 0.1-0.5wt% of the absolute dry material respectively.

[0016] The second-stage chemical impregnation chemicals are sodium hydroxide, hydrogen peroxide, sodium silicate and diethylenetriaminepentaacetic acid (DTPA) chelating agent, and the dosages are 1-10wt%, 1-10wt%, 1-6wt% and 0.1-1wt% of the absolute dry material respectively.

[0017] Preferably, in step (2), the biological method is upflow anaerobic sludge (UASB) treatment and sequencing batch activated sludge (SBR) treatment.

[0018] In a specific embodiment, conventional upflow anaerobic sludge (UASB) treatment and sequencing batch activated sludge (SBR) treatment conditions can be used for treatment. In a specific embodiment, the UASB anaerobic treatment conditions are: volumetric load of 7gCOD / (L·d), hydraulic retention time of 14.42h, temperature of 38±0.5℃, and rising flow rate of 1.68m / h.

[0019] The SBR aerobic treatment conditions are: initial activated sludge concentration of 4-5 g / L, temperature of 25±1° C., and dissolved oxygen of 2-3 mg / L.

[0020] The twin-screw extrusion process is a highly efficient mixing and reaction technology, which is widely used in the fields of food processing, plastic processing, etc. This process utilizes the rotation and shearing action of the twin screws to allow the materials to be fully mixed and reacted during the extrusion process, thereby improving the processing efficiency and effect. At the same time, the twin-screw kneading and extrusion treatment can not only moderately destroy the biological tissue structure of the material and increase the specific surface area of ​​the material, but also remove the air and soluble extracts in the cellular structure and improve the liquid absorption capacity. Therefore, the present application applies the twin-screw extrusion process to the source reduction of the resin acid content in the chemical-mechanical pulping process of coniferous wood, and by coordinating with chemical agents, it reduces the difficulty and cost of pulping wastewater treatment, which has important research significance and application prospects. Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0021] (1) Utilizing the efficient mixing and washing displacement functions of the twin-screw extrusion process, the wood fibers are softened by sodium hydroxide to dissolve the resin acid, which is then reacted with aluminum sulfate or calcium hydroxide to form a precipitate. The precipitate is then separated by plate and frame filter press, and the sludge containing the resin acid is discharged, thereby reducing the resin acid content in the wastewater, effectively reducing the resin acid content in the wastewater during the chemical-mechanical pulping process of coniferous wood, and facilitating subsequent further biological treatment.

[0022] (2) In the softwood pulping process, the source control of resin acid in wastewater is achieved, avoiding its adverse effects on subsequent wastewater treatment, thereby achieving a combination of source control and terminal treatment of pollutants;

[0023] (3) Simple operation, low cost, and suitable for large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a process flow chart for an example of this application. DETAILED DESCRIPTION

[0025] The present invention provides a method and application for reducing the resin acid content in coniferous wood chemical-mechanical pulping wastewater. Figure 1 As shown, the process includes the following: (1) cutting the softwood chips into 3-5 cm thin slices, washing with water, dehydrating and pre-steaming to soften the fiber raw materials and improve the subsequent liquid penetration effect; adding the steamed wood chips to the first-stage twin-screw extruder (TSPI-I), adding chemical agents for extrusion, and collecting the first-stage extrusion wastewater; the extruded material is subjected to a first-stage chemical impregnation, and after the impregnation is completed, it is subjected to a second-stage twin-screw extrusion (TSPI-II), and the second-stage extrusion wastewater is collected; the material after the second-stage extrusion is subjected to a second-stage chemical impregnation by adding chemicals, and then the obtained material is subjected to normal pressure high-concentration pulping, washed with water, the pulp is dried and the pulp washing wastewater is collected, and the treated pulp is subjected to conventional steps such as de-latency, screening, sheet making, and pulp performance testing;

[0026] (2) collecting the first-stage squeezing wastewater, the second-stage squeezing wastewater and the pulp washing wastewater in step (1), configuring the collected wastewater into comprehensive wastewater in proportion to the amount of wastewater generated in the pulping section, allowing the wastewater to settle in a primary sedimentation tank, and the obtained precipitate entering a plate and frame filter press for mud pressing. The filtrate obtained after mud pressing is mixed with the supernatant of the static sedimentation and then subjected to biological treatment, including UASB and SBR treatment in sequence. The treated water meets the discharge standards, and at the same time, collecting the sludge obtained in the primary sedimentation tank, UASB and SBR sections, further concentrating the sludge, and discharging the obtained dry mud.

[0027] The technical solution of the present invention is further described in detail below through embodiments.

[0028] Example 1 Single screw extruder processing effect.

[0029] The pine wood raw material was cut into 3-5 cm pieces, washed, dehydrated and pre-steamed at 105°C for 20 minutes. The steamed wood chips were added to a single screw extruder (MSD) for extrusion, and the extruded materials were chemically impregnated, wherein the amounts of NaOH, H2O2, Na2SiO3 and DTPA were 7wt%, 10wt%, 2wt% and 0.5wt% respectively, the impregnation temperature was 90°C, and the time was 90 minutes. After the pre-impregnation, the materials were pulped at high concentration under normal pressure, washed with water, and the pulp was dried and the waste water from the pulp washing section was collected. Wastewater from each section was collected, and chemical mechanical pulping comprehensive wastewater was prepared in proportion. The water sample was allowed to stand for 4 hours for precipitation, and the precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate and supernatant were mixed and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. Among them, the UASB anaerobic treatment conditions were: volume load of 7gCOD / (L·d), hydraulic retention time of 14.42h, temperature of 38±0.5℃, and rising flow rate of 1.68m / h; SBR aerobic treatment conditions were: initial activated sludge concentration of 4g / L, temperature of 25±1℃, and dissolved oxygen of 2-3mg / L. Changes in resin acid, COD and sludge properties in the wastewater were measured.

[0030] Example 2 Treatment effect of single screw extruder + NaOH.

[0031] The pine wood raw material was cut into 3-5cm pieces, washed, dehydrated and pre-steamed at 105℃ for 20min. The steamed wood chips were added to a single screw extruder (MSD) for extrusion, and NaOH was added at the drug inlet, with an amount of 0.05wt%; the extruded material was chemically impregnated, wherein the amount of NaOH, H2O2, Na2SiO3 and DTPA was 7wt%, 10wt%, 2wt% and 0.3wt%, the impregnation temperature was 90℃, and the time was 90min. After the pre-impregnation, the material was subjected to normal pressure high-concentration pulping, washed with water, the pulp was dried and the pulp washing section wastewater was collected. Wastewater from each section was collected, and the chemical mechanical pulp comprehensive wastewater was configured according to the proportion, and the water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0032] Example 3 Treatment effect of the twin-screw extruder.

[0033] The pine wood raw material is cut into 3-5cm pieces, washed, dehydrated and pre-steamed at 105°C for 20min. The steamed wood chips are added to the first stage twin screw extruder (TSPI-I) for extrusion. The extruded material is subjected to a first stage of chemical impregnation, wherein the amount of NaOH, H2O2, Na2SiO3 and DTPA is 3wt%, 4wt%, 0.8wt% and 0.2wt%, the impregnation temperature is 90°C, and the time is 30min. After the pre-impregnation is completed, the second stage of twin screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA are added for a second stage of chemical impregnation, the amount is 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature is 90°C, and the time is 60min. After the second stage of impregnation, the material is subjected to normal pressure high-concentration pulping, washed with water, and the pulp is dried and the waste water of the pulp washing stage is collected. Wastewater from each process section was collected, and chemical mechanical pulping comprehensive wastewater was prepared in proportion. The water sample was allowed to stand for 4 hours for sedimentation, and the sediment entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as in Example 1, and the changes in resin acid, COD and sludge performance in the wastewater were measured.

[0034] Example 4 Treatment effect of twin-screw extruder + NaOH.

[0035] The pine wood raw material is cut into 3-5 cm pieces, washed, dehydrated and pre-steamed at 105°C for 30 minutes. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and NaOH is added at the drug inlet in an amount of 0.05wt%, and the drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein the amount of NaOH, H2O2, Na2SiO3 and DTPA is 3wt%, 4wt%, 0.8wt% and 0.2wt%, the impregnation temperature is 90°C, and the time is 30 minutes. After the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and the chemical mechanical pulping comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0036] Example 5 Twin-screw extruder + Al2(SO4)3 treatment effect

[0037] The pine wood raw material is cut into 3-5cm pieces, washed, dehydrated and pre-steamed at 105°C for 30min. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and Al2(SO4)3 is added at the drug inlet in an amount of 0.05wt%. The drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein NaOH, H2O2, Na2SiO3 and DTPA are used in amounts of 3wt%, 4wt%, 0.8wt% and 0.2wt%, the impregnation temperature is 90°C, the time is 30min, and after the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and the chemical mechanical pulping comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0038] Example 6 Treatment effect of twin-screw extruder + calcium hydroxide.

[0039] The pine wood raw material is cut into 3-5 cm pieces, washed, dehydrated and pre-steamed at 105°C for 30 minutes. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and calcium hydroxide is added at the drug inlet in an amount of 0.05wt%, and the drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein NaOH, H2O2, Na2SiO3 and DTPA are used in amounts of 3wt%, 4wt%, 0.8wt% and 0.2wt%, the impregnation temperature is 90°C, and the time is 30 minutes. After the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and the chemical mechanical pulping comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0040] Example 7 Treatment effect of twin-screw extruder + sodium hydroxide + calcium hydroxide.

[0041] The pine wood raw material is cut into 3-5 cm pieces, washed, dehydrated and pre-steamed at 105°C for 30 minutes. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and sodium hydroxide and calcium hydroxide are added at the drug inlet in an amount of 0.02wt% and 0.03wt%, respectively. The drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein NaOH, H2O2, Na2SiO3 and DTPA are used in an amount of 3wt%, 4wt%, 0.8wt% and 0.2wt%, respectively, at an impregnation temperature of 90°C for 30 minutes. After the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and the chemical mechanical pulping comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0042] Example 8 Treatment effect of twin-screw extruder + sodium hydroxide + aluminum sulfate.

[0043] The pine wood raw material is cut into 3-5 cm pieces, washed, dehydrated and pre-steamed at 105°C for 30 minutes. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and sodium hydroxide and aluminum sulfate are added at the drug inlet in an amount of 0.02wt% and 0.03wt%, respectively. The drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein NaOH, H2O2, Na2SiO3 and DTPA are used in an amount of 3wt%, 4wt%, 0.8wt% and 0.2wt%, respectively, at an impregnation temperature of 90°C for 30 minutes. After the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and the chemical mechanical pulping comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0044] Example 9 Treatment effect of twin screw extruder + sodium hydroxide + aluminum sulfate

[0045] The pine wood raw material is cut into 3-5 cm pieces, washed, dehydrated and pre-steamed at 105°C for 30 minutes. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and sodium hydroxide and aluminum sulfate are added at the drug inlet in an amount of 0.01wt% and 0.04wt%, respectively. The drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein NaOH, H2O2, Na2SiO3 and DTPA are used in an amount of 3wt%, 4wt%, 0.8wt% and 0.2wt%, respectively, at an impregnation temperature of 90°C for 30 minutes. After the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and chemical mechanical pulp comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the wastewater was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0046] Example 10 Treatment effect of twin-screw extruder + sodium hydroxide + aluminum sulfate.

[0047] The pine wood raw material is cut into 3-5 cm pieces, washed, dehydrated and pre-steamed at 105°C for 30 minutes. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and sodium hydroxide and aluminum sulfate are added at the drug inlet in an amount of 0.04wt% and 0.01wt%, and the drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein NaOH, H2O2, Na2SiO3 and DTPA are used in an amount of 3wt%, 4wt%, 0.8wt% and 0.2wt%, the impregnation temperature is 90°C, and the time is 30 minutes. After the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and chemical mechanical pulp comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the wastewater was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0048] Example 11 Treatment effect of twin screw extruder + sodium hydroxide + aluminum sulfate

[0049] The pine wood raw material is cut into 3-5cm, washed, dehydrated and pre-steamed at 105℃ for 30min. The steamed wood chips are added to the first stage twin-screw extruder (TSPI-I), and sodium hydroxide and aluminum sulfate are added at the drug inlet in an amount of 0.03wt% and 0.02wt%. The drug liquid will mix and react at high speed during the TSPI extrusion process; the extruded material is subjected to a chemical impregnation, wherein NaOH, H2O2, Na2SiO3 and DTPA are used in an amount of 3wt%, 4wt%, 0.8wt% and 0.2wt%, the impregnation temperature is 90℃, the time is 30min, and after the pre-impregnation is completed, the second stage twin-screw extrusion (TSPI-II) is carried out to extract the residual liquid. NaOH, H2O2, Na2SiO3 and DTPA were added for two-stage chemical impregnation, with the dosage of 4wt%, 6wt%, 1.2wt% and 0.3wt%, the impregnation temperature was 90℃, the time was 60min, and the material was subjected to normal pressure high-concentration pulping after the two-stage impregnation, and water was added for washing. The pulp was dried and the wastewater from the pulp washing section was collected. Wastewater from each section was collected, and the chemical mechanical pulping comprehensive wastewater was prepared according to the proportion. The water sample was allowed to stand for 4h before precipitation. The precipitate entered the plate and frame filter press for mud pressing. After mud pressing, the filtrate was mixed with the supernatant and entered the "UASB anaerobic-SBR aerobic" reactor for treatment. The treatment conditions were the same as those in Example 1, and the changes in resin acid, COD and sludge properties in the wastewater were measured.

[0050] Among the 11 implementation cases, the basic indicators of Songmu's comprehensive wastewater and treatment are shown in the following table:

[0051]

[0052] Among them, the determination method of resin acid content, the calculation method of COD content and COD removal rate, and the calculation method of VFA and SVI are as follows:

[0053] (1) Determination of resin acid content: The resin acid content was determined by gas chromatography. For details, see Water Research, 2006, 40 (18): 3439-3446 and J. Chromatogr. 346, 205-214.

[0054] (2) Chemical oxygen demand (COD) was determined using the GB11914-89 method.

[0055] The COD removal rate calculation formula is as follows:

[0056]

[0057] (3) Volatile fatty acids (VFA) were determined by a simple acidometer method. For details, see: He Yanling, Anaerobic Biological Treatment of Wastewater, China Light Industry Press, 1998, 344-345.

[0058] (4) Calculation method of sludge index SVI:

[0059]

[0060] Among them: SV 30 MLSS is the sludge volume (mL) of the mixed liquor after sedimentation for 30 minutes and the activated sludge concentration (g / L).

Claims

1. A method for reducing the resin acid content in coniferous wood chemical-mechanical pulping wastewater, characterized in that: The steps include: (1) Cut the softwood chips into 3-5 cm thin slices, wash them with water, dehydrate them and then steam them. Add the steamed chips into the first-stage twin-screw extruder and add chemicals to extrude them. Collect the first-stage extrusion wastewater. Perform a first-stage chemical impregnation on the extruded materials. After the impregnation is completed, perform a second-stage twin-screw extrusion and collect the second-stage extrusion wastewater. Add chemicals to the extruded materials for a second-stage chemical impregnation and then perform high-concentration pulping at normal pressure. Wash them with water, spin dry the pulp and collect the wastewater from the pulp washing stage. The first-stage squeezing wastewater, the second-stage squeezing wastewater and the pulp washing wastewater in step (1) are collected, and the collected wastewater is configured as comprehensive wastewater in proportion to the amount of wastewater generated in the pulping process. The wastewater is allowed to settle, and the obtained precipitate is sent to a plate and frame filter press for mud pressing. The filtrate after mud pressing is mixed with the supernatant of the settled sedimentation and then subjected to biological treatment.

2. The method according to claim 1, characterized in that In step (1), the coniferous wood raw material is pine or fir.

3. The method according to claim 1, characterized in that In step (1), the pre-steaming time is 20-60 minutes.

4. The method according to claim 1, characterized in that: In step (1), the chemical agent in the first twin-screw extruder section is any one or two of NaOH, aluminum sulfate and calcium hydroxide, wherein the total amount of chemical agents is 0.01-0.1wt% of the absolute dry material, preferably 0.03-0.08wt%.

5. The method according to claim 1, characterized in that In step (1), the current of the first-stage twin-screw extruder and the second-stage screw extruder does not exceed 100A, and the rotation speed is 1000-1500 rpm.

6. The method according to claim 1, wherein in step (1), the first-stage chemical impregnation chemicals are sodium hydroxide, hydrogen peroxide, sodium silicate and diethylenetriaminepentaacetic acid chelating agent, and the amounts used are 0.5-5 wt%, 0.5-5 wt%, 0.1-1 wt% and 0.1-0.5 wt% of the absolute dry material, respectively.

7. The method according to claim 1, wherein in step (1), the temperature of the first stage chemical impregnation is 80-100°C, and the reaction time is 20-60 min.

8. The method according to claim 1, wherein in step (1), the second-stage chemical impregnation chemicals are sodium hydroxide, hydrogen peroxide, sodium silicate and diethylenetriaminepentaacetic acid chelating agent, and the amounts used are 1-10 wt%, 1-10 wt%, 1-6 wt% and 0.1-1 wt% of the absolute dry material, respectively.

9. The method according to claim 1, wherein in step (1), the second-stage chemical impregnation temperature is 80-100°C and the reaction time is 30-90 min.

10. The method according to claim 1, characterized in that In step (2), the biological method is upflow anaerobic sludge treatment and sequencing batch activated sludge treatment.