Lithium iron phosphate conductive aerogel as well as preparation method and application thereof

By using high-degree-diameter conducting agents in lithium iron phosphate positive electrode materials to construct three-dimensional conductive paths, the problems of low conductivity and easy agglomeration of conductive agents are solved, and high-performance and stable lithium iron phosphate conductive aerogels are achieved, suitable for High-speed charging scenario.

CN119059507APending Publication Date: 2024-12-03CHINA FAW CO LTD

Patent Information

Application Number
CN202411359780.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Due to the low conductivity of lithium iron phosphate positive electrode materials, due to the problems of low conductivity and easy agglomeration of conductive agents, the performance of lithium iron phosphate cathode materials is insufficient in high-rate charging scenarios, and the existing processes are complex and difficult to achieve mass production.

Method used

A three-dimensional conductive path is constructed with a sheet or linear conductive agent with a high aspect ratio. Through the defoaming, heat treatment, dialysis and freeze-drying of the suspension, a stable gel lithium iron phosphate conductive aerogel is formed to ensure iron phosphate Lithium is uniformly loaded on the conductive agent aerogel network to form a continuous conductive pathway.

Benefits of technology

It improves the conductivity and structural stability of lithium iron phosphate positive electrode material, enhances circulation and storage life, adapts to high-rate fast charging scenarios, and reduces the risk of aggregation of conductive agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059507A_ABST
    Figure CN119059507A_ABST
Patent Text Reader

Abstract

The invention provides lithium iron phosphate conductive aerogel as well as a preparation method and application thereof, and relates to the technical field of lithium ion batteries. Specifically, the method comprises the following steps: preparing a suspension containing lithium iron phosphate, a conductive agent and a dispersing agent, and carrying out defoaming treatment and heat treatment on the suspension to obtain a gel precursor; and carrying out dialysis treatment and freeze drying treatment on the gel precursor to obtain the lithium iron phosphate conductive aerogel. The lithium iron phosphate conductive aerogel prepared by the invention can be used as a self-supporting positive electrode, has excellent electrochemical performance and structural stability, solves the problems of low intrinsic conductivity and insufficient fast charging performance of lithium iron phosphate, can effectively avoid the agglomeration of the conductive agent, enhances the structural stability, prolongs the cycle and storage life of the positive electrode material, and has a good application prospect. A plurality of defects when the lithium iron phosphate aerogel is used for the positive electrode are effectively improved, and the lithium iron phosphate aerogel has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium iron phosphate conductive aerogel and a preparation method and application thereof. Background Art

[0002] Lithium iron phosphate has good electrical properties and extremely high safety, and is one of the most promising positive electrode materials for lithium-ion power batteries. However, due to its low lithium ion diffusion coefficient and poor intrinsic conductivity, lithium iron phosphate is limited in current application scenarios requiring high-rate charging. There are two main solutions at present: First, nano-size lithium iron phosphate particles to increase the specific surface area of ​​the material, shorten the migration path of lithium ions and electrons, and increase its charging and discharging speed; second, the surface of lithium iron phosphate is carbon-coated or the content ratio of the conductive agent in the formula is increased to improve its conductivity. However, the nano-size of lithium iron phosphate cannot change its low intrinsic conductivity, and excessive conductive agents are prone to agglomeration, shortening the life of the battery cell and not conducive to capacity utilization.

[0003] CN107170977A discloses a method for preparing a lithium iron phosphate / graphene composite material. The three-dimensional reduced graphene oxide is soaked in a soaking solution containing an iron source, a phosphate source, a lithium source and a reducing agent, and then freeze-dried, pre-decomposed and roasted under the protection of an inert gas to obtain the composite material. The lithium iron phosphate / graphene composite material prepared by the present invention is applied to lithium-ion batteries and has excellent properties such as high capacity, long cycle life, low cost and easy large-scale production. However, this preparation process belongs to the conventional calcination method, and has the inherent defects of uneven dispersion of positive electrode materials and insufficient mechanical strength. The prepared composite material still needs to be compounded with a current collector before being used for the positive electrode. The prior art has also made further improvements to the above defects, such as introducing an aerogel structure into the electrode material.

[0004] CN106920931A discloses a method for preparing a graphene aerogel-loaded mesoporous lithium iron phosphate nanosheet composite material. The graphene aerogel is prepared by subjecting a graphene oxide solution of appropriate concentration to hydrothermal reaction, cooling and drying in sequence; a phosphate source, an iron source and a lithium source are then prepared into a mixed sol in an appropriate molar ratio; the sol is then dripped onto the surface of the graphene aerogel until adsorption saturation and dried to obtain a gel precursor; and finally, a graphene aerogel-loaded mesoporous lithium iron phosphate nanosheet composite material is obtained by high-temperature calcination. The process of the present invention is simple, and the obtained material has excellent specific capacity, rate and cycle performance. However, in this method, in order to ensure its liquid absorption efficiency, the amount of graphene used in the positive electrode material accounts for a very high proportion, which is not conducive to the capacity of the positive electrode material and shortens the cycle life; moreover, lithium iron phosphate is synthesized in the graphene aerogel framework, and the aerogel structure is easily damaged during the calcination process, and it is not easy to maintain the overall structural stability.

[0005] CN108232180A discloses a graphene / titanium dioxide / lithium iron phosphate aerogel battery positive electrode material and a preparation method thereof. The material uses nanographene as a core, first loads nanotitanium dioxide, then coats a lithium iron phosphate layer, and finally undergoes aging and drying treatment to obtain a graphene / titanium dioxide / lithium iron phosphate aerogel battery positive electrode material. The positive electrode material has ultra-low density, ultra-large pores, ultra-large internal surface area, ultra-low thermal conductivity, ultra-low sound velocity, and excellent thermal stability and mechanical properties, and is more flexible, high-strength, high heat resistance, high conductivity, high specific capacity, high rate characteristics, fast charge and discharge, and long cycle life, and can be widely used in the fields of batteries, catalysis, aerospace, and advanced materials. However, it was found through actual production tests that due to its complex synthesis conditions and high raw material requirements, its three-layer coating structure may not be obtained as smoothly as imagined, and has the defects of low product qualification rate and low quality stability.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The first purpose of the present invention is to provide a method for preparing lithium iron phosphate conductive aerogel, which is mainly used to solve the defects of the existing lithium iron phosphate positive electrode having low conductivity and easy agglomeration of the conductive agent; at the same time, it is used to solve the defects of the existing gel-state lithium iron phosphate positive electrode having excessive amount of carbon conductive agent, easy destruction of the gel structure by heat treatment, complex process or difficulty in mass production.

[0008] The second purpose of the present invention is to provide a lithium iron phosphate conductive aerogel, which can change the electrical contact of the electron transmission path between lithium iron phosphates into line contact through a sheet-like or linear conductive agent with a high aspect ratio, and construct a denser three-dimensional conductive path based on the gel structure; the obtained three-dimensional nanoporous aerogel positive electrode material has the characteristics of low density, high specific surface area, high porosity and strong mechanical properties.

[0009] A third object of the present invention is to provide a lithium ion battery.

[0010] A fourth object of the present invention is to provide an electrical device.

[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0012] A method for preparing lithium iron phosphate conductive aerogel comprises the following steps:

[0013] preparing a suspension containing lithium iron phosphate, a conductive agent, and a dispersant, and performing a defoaming treatment and a heat treatment on the suspension to obtain a gel precursor;

[0014] The gel precursor is dialyzed and freeze-dried to obtain lithium iron phosphate conductive aerogel.

[0015] A lithium iron phosphate conductive aerogel is prepared by adopting the preparation method of the lithium iron phosphate conductive aerogel.

[0016] A lithium ion battery comprises the lithium iron phosphate conductive aerogel.

[0017] An electrical device comprises the lithium-ion battery.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present invention proposes a novel method for preparing lithium iron phosphate conductive aerogel, by limiting the type of carbon conductive agent, introducing a conductive agent with a high aspect ratio or a linear configuration, and in the process of configuring it into a suspension, by controlling the appropriate mass fraction to form a state in which the sheets are overlapped with each other in a well-dispersed state, and finally forming a stable gel state. In this state, a continuous and uniform conductive agent gel network has excellent conductivity; further, the present invention realizes that after removing the solvent, lithium iron phosphate is uniformly loaded on the conductive agent aerogel network and a continuous conductive path is formed through the process of defoaming, heat treatment, dialysis and freeze drying.

[0020] (2) The lithium iron phosphate / conductive aerogel positive electrode material prepared by the present invention has excellent electrical properties and structural stability, which solves the problems of low intrinsic conductivity and insufficient fast charging performance of lithium iron phosphate. At the same time, it can effectively avoid the agglomeration of the conductive agent, enhance the structural stability, and further improve the cycle and storage life of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] like Figure 1 The figure shows a schematic diagram of the structure of the lithium iron phosphate conductive aerogel of the present invention. DETAILED DESCRIPTION

[0023] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. In addition, the terms "first", "second" and "third" are only used for descriptive purposes and cannot be interpreted as indicating or implying relative importance.

[0024] A first aspect of the present invention is to provide a method for preparing lithium iron phosphate conductive aerogel.

[0025] The preparation method mainly comprises the following steps: preparing a suspension containing lithium iron phosphate, a conductive agent and a dispersant, degassing and heat-treating the suspension to obtain a gel precursor; and dialyzing and freeze-drying the gel precursor to obtain a lithium iron phosphate conductive aerogel.

[0026] As a preferred embodiment, the lithium iron phosphate described in the present invention is nano-scale; in some more preferred cases, the particle size of the lithium iron phosphate is 300nm to 500nm, and the purity of the lithium iron phosphate should be higher than 99.5%.

[0027] It is understandable that those skilled in the art can obtain suitable lithium iron phosphate raw materials through commercial channels or through self-synthesis. However, when high-purity nano-scale lithium iron phosphate is used as the raw material of the lithium iron phosphate conductive aerogel of the present invention, the aerogel product will have better conductive performance; therefore, the present invention also provides a suitable preparation method of lithium iron phosphate, comprising the following steps:

[0028] (1) preparing a first mixed solution containing a lithium source and a phosphorus source, adjusting the pH to 11 to 13, performing a sufficient reaction, and performing solid-liquid separation to obtain a lithium phosphate precipitate;

[0029] (2) preparing a second mixed solution containing an iron source and ascorbic acid, adding the lithium phosphate precipitate to the second mixed solution, adjusting the pH to 6 to 8, and then reacting fully under a protective gas environment, separating the solid and the liquid to obtain lithium iron phosphate.

[0030] As a more preferred embodiment, the lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium chloride or lithium acetate.

[0031] As a more preferred embodiment, the phosphorus source includes at least one of phosphoric acid, diammonium phosphate, iron phosphate or lithium phosphate.

[0032] As a more preferred embodiment, the iron source includes at least one of ferrous sulfate, ferrous nitrate, ferrous phosphate, ferrous oxalate or ferrous oxide.

[0033] As a more preferred embodiment, in the first mixed solution, the molar ratio of the lithium element in the lithium source to the phosphorus element in the phosphorus source is (2.5-3.5):1, and more preferably 3:1.

[0034] As a more preferred embodiment, the pH is adjusted by lithium hydroxide in step (1).

[0035] As a more preferred embodiment, the pH value adjusted in step (1) includes but is not limited to any one of 11, 11.2, 11.5, 11.8, 12, 12.2, 12.5, 12.8, 13 or a numerical range consisting of any two of them.

[0036] As a more preferred embodiment, the full reaction involved in steps (1) and (2) can be achieved by applying any one or two of the treatment conditions such as stirring, shaking, centrifugation, ultrasound, and heat treatment to ensure the full implementation of the chemical reaction.

[0037] As a more preferred embodiment, in the solid-liquid separation involved in steps (1) and (2), the solid phase product is washed with clean water 2 to 3 times after being obtained.

[0038] As a more preferred embodiment, in the second mixed solution, the molar ratio of the iron element in the iron source to the phosphorus element in the lithium phosphate precipitate is (2.5-3.5):1, and more preferably 3:1.

[0039] As a more preferred embodiment, in the second mixed solution, the concentration of ascorbic acid is 0.2 mol / L to 0.3 mol / L.

[0040] As a more preferred embodiment, in step (2), the pH is adjusted by lithium hydroxide or phosphoric acid.

[0041] As a more preferred embodiment, the pH value adjusted in step (2) includes but is not limited to any one of 6, 6.2, 6.5, 6.8, 7, 7.2, 7.5, 7.8, 8, or a numerical range consisting of any two of them.

[0042] As a more preferred embodiment, the protective gas environment includes but is not limited to nitrogen, helium, neon, argon, etc.; the protective gas is replaced at least 3 to 5 times during the reaction process of step (2).

[0043] As a more preferred embodiment, in step (2), the temperature of the full reaction is 180°C to 190°C, and the holding time of the full reaction is 10h to 12h. In the present invention, by controlling the temperature and time characteristics of the hydrothermal reaction and the hydrothermal synthesis conditions, lithium iron phosphate nanoparticles with good morphology and uniform size distribution are prepared.

[0044] As a more preferred embodiment, after step (2), the method further comprises: vacuum drying at 60° C. to 80° C. for 5 h to 7 h to obtain the lithium iron phosphate.

[0045] As a preferred embodiment, the conductive agent includes graphene nanosheets, single-walled carbon nanotubes, multi-walled carbon nanotubes, graphitized carbon fibers, etc.; it can be understood that in addition to any one or more of the materials listed above, the present invention can also adopt any amorphous carbon material with a flaky structure having a high aspect ratio.

[0046] In the present invention, a high aspect ratio sheet / wire-shaped conductive agent is innovatively used as the aerogel matrix skeleton, and the sheet layers are overlapped to construct a stable three-dimensional network structure of the aerogel, and the lithium iron phosphate is loaded on the conductive agent network through hydrogen bonds and van der Waals forces, and the prepared positive electrode material has good mechanical properties; further, the proportion of active materials in the positive electrode material is increased under the premise of eliminating the current collector and the binder, and the prepared self-supporting lithium iron phosphate conductive aerogel material can be independently used for the positive electrode of a lithium-ion battery, and has good conductivity and cycle life, and is suitable for high-rate fast charging scenarios of 6C and above.

[0047] As a preferred embodiment, the aspect ratio of the conductive agent is 1000-5000, including but not limited to any one of 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000 or a numerical range consisting of any two of them.

[0048] As a preferred embodiment, the dispersant includes at least one of ascorbic acid, glucose, hydrazine hydrate or hydroxylamine hydrochloride.

[0049] As a preferred embodiment, the conductive agent includes the following pretreatment steps: ball milling for 7 minutes to 10 minutes to obtain small particles of the conductive agent at the nanoscale; in some more preferred embodiments, the particle size of the conductive agent is 30nm to 40nm, and the sheet length of the conductive agent is 40μm to 60μm.

[0050] As a preferred embodiment, the preparation of the suspension includes the following steps: first preparing an aqueous solution of the conductive agent and performing a first homogenization treatment; then adding the lithium iron phosphate and performing a second homogenization treatment; and finally adding the dispersant and performing a third homogenization treatment to obtain the suspension.

[0051] As a more preferred embodiment, the first homogenization treatment, the second homogenization treatment and the third homogenization treatment are all carried out by mechanical stirring, and the stirring frequency is 300rpm to 500rpm; wherein, the time of the first homogenization treatment is 10min to 15min, the time of the second homogenization treatment is 35min to 40min, and the time of the third homogenization treatment is 15min to 20min.

[0052] As a preferred embodiment, in the suspension, the mass ratio of the lithium iron phosphate, the conductive agent and the dispersant is (10-15): (1-1.5):200.

[0053] As a preferred embodiment, the defoaming treatment comprises the following steps: evacuating the suspension to a vacuum and maintaining the vacuum for 10 to 12 minutes.

[0054] As a preferred embodiment, the heat treatment temperature is 10°C to 80°C, and the heat treatment time is 8h to 12h; in some more preferred embodiments, the heat treatment temperature includes but is not limited to any one of 10, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80 (°C) or a numerical range consisting of any two of them. In some optional embodiments, the heat treatment can be carried out by water bath, oven, electric heating, etc.

[0055] As a preferred embodiment, the dialysis treatment can be performed according to conventional dialysis equipment and conventional methods; the medium of the dialysis treatment is deionized water, and the dialysis treatment time is 18h to 24h. The present invention can effectively remove the small-particle dispersant ions in the gel precursor through the dialysis treatment without losing nano-lithium iron phosphate and conductive agent molecules, thereby obtaining a relatively pure aerogel product.

[0056] As a more preferred embodiment, the treatment temperature of the dialysis treatment is 25°C±3°C; the flow rate of the medium (dialysis fluid) of the dialysis treatment is not strictly limited in the present invention, but the dialysate is usually replaced every 5 to 8 hours.

[0057] As a preferred embodiment, the freeze-drying process includes pre-freezing and vacuum freezing performed in sequence; the pre-freezing temperature is 1°C to 5°C, the pre-freezing duration is 6h to 8h, the vacuum freezing temperature is -55°C to -45°C, and the vacuum freezing duration is 42h to 48h.

[0058] It is worth noting that the present invention innovatively applies a pre-freezing process to control the growth of ice crystals during freeze-drying, achieve small and uniform pores in the lithium iron phosphate conductive aerogel, construct a fast ion transfer channel, and improve the rate performance of the material; at the same time, it avoids the re-agglomeration of the conductive agent during the freeze-drying process, and effectively improves the stability and consistency of the conductive network.

[0059] A second aspect of the present invention is to provide a lithium iron phosphate conductive aerogel.

[0060] The lithium iron phosphate conductive aerogel is prepared according to the preparation method of the lithium iron phosphate conductive aerogel as described in the first aspect. Figure 1 The structure diagram of the lithium iron phosphate conductive aerogel of the present invention is provided as shown in FIG. Figure 1 It can be seen that the composite conductive aerogel obtained by the present invention presents a three-dimensional continuous porous network structure with a pore size ranging from hundreds of nanometers to micrometers; nano-scale lithium iron phosphate is evenly dispersed by van der Waals forces and tightly wrapped by the conductive agent layer, and the conductive network formed by overlapping the conductive agent layers can significantly improve the conductivity of the aerogel.

[0061] It is understandable that the lithium iron phosphate conductive aerogel of the present invention can be directly used as a self-supporting positive electrode of a lithium ion battery, obtaining an electrode structure without the need for additional binders, conductive agents and current collectors.

[0062] A third aspect of the present invention is to provide a lithium ion battery.

[0063] The lithium-ion battery should include the lithium iron phosphate conductive aerogel as described in the second aspect, and the lithium-ion battery includes but is not limited to primary or secondary batteries such as button batteries, soft-pack batteries, and square batteries.

[0064] It can be understood that, in addition to the lithium iron phosphate conductive aerogel, the lithium ion battery should include a negative electrode, an electrolyte, a diaphragm, and other necessary or unnecessary functional elements or packaging components, etc., and those skilled in the art can arbitrarily select and combine them; when the lithium iron phosphate conductive aerogel of the present invention is included in the lithium ion battery, whether or not other positive electrode functional components or structures are used in the lithium ion battery, it can be regarded as an embodiment of the present invention.

[0065] A fourth aspect of the present invention is to provide an electrical device.

[0066] The electrical equipment includes the lithium-ion battery as described in the third aspect. It is understandable that the electrical equipment can be any equipment or device that relies on electric energy to work or operate, including but not limited to new energy vehicles, building electrical equipment, industrial electrical appliances, household and agricultural electrical appliances, etc.; when including the lithium-ion battery, any electrical equipment equipped with the lithium-ion battery can belong to an embodiment of the present invention.

[0067] Example 1

[0068] (1) Preparation of high-purity nanoscale lithium iron phosphate.

[0069] S1: Take 500g of 1mol / L lithium hydroxide solution, add 500g of 0.33mol / L phosphoric acid and stir evenly, introduce a small amount of lithium hydroxide to adjust the pH to 11, and mechanically stir at 500r / min for 40min to obtain a white precipitate of lithium phosphate;

[0070] S2: After filtering the precipitate, wash it with deionized water for 3 times and set aside;

[0071] S3: Take 500 g of 1 mol / L ferrous sulfate solution and 100 g of 0.3 mol / L ascorbic acid, mix the two and stir briefly, then slowly add the mixed solution into the lithium phosphate precipitate and stir at 500 r / min for 12 min;

[0072] S4: lithium hydroxide or phosphoric acid is added dropwise to the mixed solution to adjust the pH to 8, the mixed solution is transferred to an autoclave, argon is replaced 4 times, the reaction temperature is controlled at 185°C, and the temperature is kept for 11 hours;

[0073] S5: After the autoclave is naturally cooled to room temperature, the solid sample is centrifuged at 1000 r / min for 10 min to obtain the solid sample, which is washed with deionized water and anhydrous ethanol for 3 times respectively, and vacuum dried at 70° C. for 6 h to obtain lithium iron phosphate.

[0074] (2) Preparation of lithium iron phosphate / conductive gel precursor.

[0075] S6: Take 5 g of graphene nanosheets, add deionized water to prepare 1 L of mixed solution, and mechanically stir at 400 r / min for 12 min to obtain a graphene suspension;

[0076] S7: Take 50 g of the lithium iron phosphate prepared in step S5, add it to the suspension in step S6, and mechanically stir at 400 r / min for 38 min to obtain a suspension a;

[0077] S8: Take 10 mL of ascorbic acid solution and add it to suspension a, and stir mechanically at 400 r / min for 15 min to obtain suspension b;

[0078] S9: Place the suspension b in a vacuum oven for evacuation for 10 minutes. After the bubbles are eliminated, place it in a water bath and heat it at 75°C for 10 hours to obtain a lithium iron phosphate / conductive gel precursor.

[0079] (3) Preparation of self-supporting lithium iron phosphate conductive aerogel positive electrode.

[0080] S10: placing the gel precursor prepared in step S9 into a dialysis bag, dialyzing it with deionized water for 20 hours, and then taking it out;

[0081] S11: placing the dialyzed gel precursor in a freeze dryer cold trap, adjusting the temperature to 2°C for pre-freezing for 6 hours, then adjusting the cold trap temperature to -50°C, and continuing vacuum freeze drying for 48 hours, until the solvent is completely sublimated to obtain the lithium iron phosphate-graphene aerogel positive electrode of this embodiment.

[0082] Example 2

[0083] The method is basically the same as Example 1, except that the 500 g lithium hydroxide in step S1 is replaced by the same molar amount of lithium carbonate.

[0084] Example 3

[0085] The method is basically the same as Example 1, except that 500 g of lithium hydroxide in step S1 is replaced by the same molar amount of lithium nitrate.

[0086] Example 4

[0087] The method is basically the same as Example 1, except that the pH is adjusted to 13 in step S1 and the pH is adjusted to 6 in step S4.

[0088] Example 5

[0089] The method is substantially the same as Example 1, except that 500 g of ferrous sulfate in step S3 is replaced by the same molar amount of ferrous nitrate.

[0090] Example 6

[0091] The method is substantially the same as Example 1, except that 500 g of ferrous sulfate in step S3 is replaced by the same molar amount of ferrous phosphate.

[0092] Example 7

[0093] The method is basically the same as Example 1, except that 500 g of phosphoric acid in step S1 is replaced by the same molar amount of diammonium phosphate.

[0094] Example 8

[0095] The method is basically the same as Example 1, except that the graphene nanosheets in step S6 are replaced by single-walled carbon nanotubes.

[0096] Example 9

[0097] The method is basically the same as Example 1, except that the graphene nanosheets in step S6 are replaced by graphitized carbon fibers.

[0098] Comparative Example 1

[0099] The method is basically the same as Example 1, except that the pH value is controlled to 9 in step S4.

[0100] Comparative Example 2

[0101] The method is basically the same as Example 1, except that the pH value is controlled to 5 in step S4.

[0102] Comparative Example 3

[0103] The process is basically the same as Example 1, except that the reaction temperature is controlled to 160° C. in step S4 .

[0104] Comparative Example 4

[0105] The process is basically the same as Example 1, except that the reaction temperature is controlled to 200° C. in step S4 .

[0106] Comparative Example 5

[0107] The method is basically the same as Example 1, except that the graphene nanosheets in step S6 are replaced by conductive carbon black.

[0108] Comparative Example 6

[0109] The method is basically the same as Example 1, except that the amount of graphene nanosheets in step S6 is replaced to 15 g.

[0110] Comparative Example 7

[0111] The method is basically the same as Example 1, except that the amount of graphene nanosheets in step S6 is replaced to 7 g.

[0112] Comparative Example 8

[0113] The method is basically the same as Example 1, except that the operation step of "adjusting the temperature to 2° C. and pre-freezing for 6 hours" is omitted in step S11.

[0114] Test Example 1

[0115] The aerogel positive electrodes prepared in each embodiment and comparative example were subjected to conductivity test and tensile strength test in turn, and the results are recorded in Table 1.

[0116] (a) Conductivity test: The volume resistance of the aerogel cathode was tested by the AC impedance method, and the conductivity of the aerogel cathode was calculated according to the following formula (σ, S·cm -1);

[0117] σ=L / (R b A); where L represents the thickness of the aerogel cathode in cm; R b is the measured volume resistance of the aerogel positive electrode, in Ω; A is the actual effective contact area between the aerogel positive electrode and the stainless steel sheet, in cm 2 .

[0118] (b) Tensile strength test: Each aerogel cathode was cut into dumbbell-shaped samples with a thickness of 2 mm and a width of 6 mm. The tensile speed of the tensile testing machine was controlled to be 10 mm / min and the test temperature was 25°C ± 2°C. The average tensile strength of 5 sets of parallel samples was taken for each sample.

[0119] Test Example 2

[0120] The gel-state positive electrodes prepared in the examples and comparative examples were used to prepare button-type half-cells, and the specific steps were as follows: graphite was used as the negative electrode, and nickel foam was used as a buffer gasket; the electrolyte components included solvent (EC 20 parts, PC 5 parts, DEC 10 parts, EMC 65 parts), lithium salt (LiPF 6 1.1mol / L), additives (LIFSI 2%, PS 0.5%, DTD 1%, LiPO 2 F 2 1%, LiDFOB0.5%, PST 0.3%, TMSP 0.5%, GN15 0.2%, VC 0.3%).

[0121] (1) Carry out the first charge and discharge test, record the battery capacity in grams during the first charge and the coulomb efficiency during the first discharge; the test conditions are 0.1C charge and discharge, and the voltage is 2.0V~3.6V.

[0122] (2) Perform rate performance test: adjust the ambient temperature to 25℃±2℃, perform standard charging (0.33C constant current charging to the upper limit voltage of the battery 3.6V, adjust to constant voltage charging to 0.05C), let it stand for 30 minutes, and then discharge it at 0.2C constant current to the lower limit voltage 2.0V, and record the discharge capacity C1; perform standard charging again, let it stand for 30 minutes, and then discharge it at 2C constant current to the lower limit voltage 2.0V, and record the discharge capacity C2; calculate the rate performance (2C / 0.2C) and the result is C2 / C1.

[0123] (3) Perform cycle life test: adjust the ambient temperature to 25℃±2℃, first discharge the battery at 0.33C to the lower limit voltage of 2.0V; the first cycle and capacity calibration: 0.5C constant current charge to the upper limit voltage of 3.6V, constant voltage charge to 0.05C, let it stand for 30 minutes, then discharge at 1C constant current to the lower limit voltage of 2.0V, record the discharge capacity C1; the nth cycle process is the same as the first cycle, record the discharge capacity Cn. When Cn / C1≤80%, the life is determined to be terminated, and n (number of cycles) is recorded as the cycle life of the battery.

[0124] Table 1

[0125]

[0126] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A method for preparing lithium iron phosphate conductive aerogel, characterized in that: The steps include: preparing a suspension containing lithium iron phosphate, a conductive agent, and a dispersant, and performing a defoaming treatment and a heat treatment on the suspension to obtain a gel precursor; The gel precursor is dialyzed and freeze-dried to obtain lithium iron phosphate conductive aerogel.

2. The method for preparing lithium iron phosphate conductive aerogel according to claim 1, characterized in that: The preparation method comprises at least one of the following features (a) to (d): (a) the particle size of the lithium iron phosphate is 300nm to 500nm, and the purity of the lithium iron phosphate is ≥99.5%; (b) the conductive agent comprises at least one of graphene nanosheets, single-walled carbon nanotubes, multi-walled carbon nanotubes or graphitized carbon fibers; (c) the dispersant comprises at least one of ascorbic acid, glucose, hydrazine hydrate or hydroxylamine hydrochloride; (d) The particle size of the conductive agent is 30 nm to 40 nm; the aspect ratio of the conductive agent is 1000 to 5000; and the sheet length of the conductive agent is 40 μm to 60 μm.

3. The method for preparing lithium iron phosphate conductive aerogel according to claim 1, characterized in that: In the suspension, the mass ratio of the lithium iron phosphate, the conductive agent and the dispersant is (10-15): (1-1.5): 200; And / or, in the suspension, the concentration of the conductive agent is 5 g / L to 6 g / L.

4. The method for preparing lithium iron phosphate conductive aerogel according to claim 1, characterized in that: The temperature of the heat treatment is 10°C to 80°C, and the time of the heat treatment is 8h to 12h; And / or, the defoaming treatment includes: evacuating the suspension to a vacuum state and maintaining the vacuum state for 10 to 12 minutes.

5. The method for preparing lithium iron phosphate conductive aerogel according to claim 1, characterized in that: The dialysate for the dialysis treatment is deionized water; and the dialysis treatment time is 18h to 24h.

6. The method for preparing lithium iron phosphate conductive aerogel according to claim 1, characterized in that: The freeze-drying process includes pre-freezing and vacuum freezing performed sequentially; The pre-freezing temperature is 1°C to 5°C, and the pre-freezing duration is 6h to 8h; The temperature of the vacuum freezing is -55°C to -45°C, and the duration of the vacuum freezing is 42h to 48h.

7. The method for preparing lithium iron phosphate conductive aerogel according to claim 1, characterized in that: The preparation method of lithium iron phosphate comprises the following steps: A first mixed solution containing a lithium source and a phosphorus source is prepared, and the pH value is adjusted to 11 to 13, followed by a first reaction, solid-liquid separation, and lithium phosphate precipitation is obtained; A second mixed solution containing an iron source and ascorbic acid is prepared, the lithium phosphate precipitate is added to the second mixed solution, the pH is adjusted to 6-8, a second reaction is carried out under a protective gas environment, and solid-liquid separation is performed to obtain lithium iron phosphate.

8. A lithium iron phosphate conductive aerogel, characterized in that: The lithium iron phosphate conductive aerogel is prepared by the preparation method of any one of claims 1 to 7.

9. A lithium ion battery, characterized in that: Comprising the lithium iron phosphate conductive aerogel as described in claim 8.

10. An electrical device, characterized in that: Comprising the lithium ion battery as claimed in claim 9.

Citation Information

Patent Citations

  • Graphene aerogel-loaded mesoporous lithium iron phosphate nanosheet composite material and preparation method thereof

    CN106920931A

  • Preparation method of lithium iron phosphate / graphene composite material, lithium ion battery cathode, and lithium ion battery

    CN107170977A

  • Graphene / titanium dioxide / lithium ion phosphate aerogel battery anode material and preparation method thereof

    CN108232180A

Cited By

  • Self-supporting negative electrode material and preparation method and application thereof

    CN119905546A