Heat-conducting SiC ceramic-based composite material and preparation method thereof

By using alternate stacking of two-dimensional fiber cloth and graphene films in SiC ceramic matrix composite materials, and high-temperature debonding and chemical vapor permeation treatment, a material with ultra-high thermal anisotropy is formed, and the thermal conductivity of SiC ceramic matrix composite materials is solved. The problem of insufficient performance achieves rapid heat dissipation in the thermal conductivity direction and thermal insulation in the non-thermal conductivity direction.

CN119059822AInactive Publication Date: 2024-12-03WUZHEN LABORATORY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411572448.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

SiC ceramic matrix composites have insufficient thermal conductivity in high temperature environments, resulting in local high temperature damage to internal components. Common carbon fibers have low thermal conductivity, making it difficult to form an effective thermal conductivity path.

Method used

The graphene films with two-dimensional fiber cloth and high-temperature graphitization are alternately stacked, and the SiC with ultra-high thermal anisotropy is formed by fibre thread suture, high-temperature debonding treatment, chemical vapor permeation treatment and polycarbonsilane impregnation and cross-linking. Ceramic matrix composite material.

Benefits of technology

Fast heat dispersion in the thermal conductivity direction and thermal insulation in the non-thermal conductivity direction are achieved, reducing the temperature gradient and preventing high temperature from damaging other components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of heat-conducting materials, in particular to a heat-conducting SiC ceramic-based composite material and a preparation method thereof. The preparation method of the composite material comprises the following steps: A) alternately stacking two-dimensional fiber cloth made of a specific material and a graphene film subjected to high-temperature graphitization treatment, and sewing with fiber threads to obtain a preform; b) performing high-temperature debonding treatment on the preform; c) performing chemical vapor infiltration treatment on the treated prefabricated body to obtain a prefabricated body with an interface phase; d) impregnating the preform obtained in the step C) with polycarbosilane, and then carrying out crosslinking and high-temperature cracking; e, the step D is repeated until the weight gain rate of the composite material is smaller than 3%, and the heat-conducting SiC ceramic-based composite material is obtained.The prepared heat-conducting SiC ceramic-based composite material has ultrahigh heat-conducting anisotropy, that is, the heat-conducting SiC ceramic-based composite material has ultrahigh heat conductivity in the plane direction but is almost insulated in the thickness direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermal conductive materials, and in particular to a thermal conductive SiC ceramic-based composite material and a preparation method thereof. Background Art

[0002] SiC ceramic-based composite materials have outstanding advantages in low density, low thermal expansion coefficient, high strength and high temperature oxidation resistance, and are of great value in the field of thermal protection systems and thermal protection structural materials. For example, in the field of nuclear energy, cladding materials need to be in harsh service environments such as radiation, high temperature and high pressure, and particle sputtering for a long time; in the field of hypersonic aircraft, the leading edge of the wing of the flying chess tip can reach more than 1800℃ due to the rise in temperature due to aerodynamic friction; in the civilian field, friction brake materials need to have good friction resistance and excellent thermal and mechanical properties.

[0003] In practical applications, SiC ceramic-based composite materials need to face the problem of local high temperature, which requires higher and higher temperature for use as hot-end materials. One solution is to develop SiC ceramic-based composite materials with higher thermal conductivity to reduce the temperature gradient. In addition, due to the diffusion of high temperature along the thickness direction, it is easy to damage other non-hot-end components inside, which is also a problem that needs to be solved urgently.

[0004] Continuous carbon fiber reinforced SiC composites can overcome the poor toughness of SiC composites and are therefore widely used. However, the thermal conductivity of ordinary carbon fibers is less than 20 W / (m·K), making it difficult to form an effective heat conduction path. Therefore, the thermal conductivity of common SiC composites is poor. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a thermally conductive SiC ceramic-based composite material and a preparation method thereof. The thermally conductive SiC ceramic-based composite material prepared by the present invention has ultra-high thermal conductivity anisotropy, that is, it has ultra-high thermal conductivity in the plane direction, but is almost heat-insulating in the thickness direction.

[0006] The present invention provides a method for preparing a thermally conductive SiC ceramic-based composite material, comprising the following steps:

[0007] A) alternately stacking a two-dimensional fiber cloth and a graphene film after high-temperature graphitization treatment, and sewing them with fiber threads to obtain a preform; the material of the two-dimensional fiber cloth includes polyacrylonitrile-based carbon fiber;

[0008] B) subjecting the preform to a high temperature debonding treatment;

[0009] C) subjecting the preform treated in step B) to chemical vapor infiltration treatment to obtain a preform with an interface phase;

[0010] D) impregnating the preform obtained in step C) with polycarbosilane, then cross-linking and pyrolyzing at high temperature;

[0011] E) Repeat step D) until the weight gain of the composite material is less than 3%, thereby obtaining a thermally conductive SiC ceramic-based composite material.

[0012] Preferably, in step A), the material of the fiber line includes polyacrylonitrile-based carbon fiber.

[0013] Preferably, in step A), the temperature of the high temperature graphitization treatment is above 2800°C;

[0014] The thickness of the graphene film after high-temperature graphitization treatment is 10-100 μm.

[0015] Preferably, in step A), the suturing density of the suturing process is 0.3-1 suture thread / cm.

[0016] Preferably, in step B), the temperature of the high temperature debonding treatment is 900-1200°C;

[0017] The high-temperature debonding treatment is carried out under the protection of an inert gas.

[0018] Preferably, in step C), the temperature of the chemical vapor infiltration treatment is 600-1300°C, the time is 10-16 h, and the gas source is C 3 H 6 Gas or CH 3 SiCl gas, gas flow rate is 200~1000 mL / min, deposition pressure is 4~12 kPa, and deposition interface thickness is 100~1500 nm.

[0019] Preferably, in step D), the immersion pressure is less than 10 Pa and the immersion time is 10 to 14 h.

[0020] Preferably, in step D), the crosslinking is carried out under the protection of an inert gas; the temperature is 120-200° C.; the rate of heating to the crosslinking temperature is 2-10° C. / min; and the crosslinking time is 20-60 min.

[0021] Preferably, in step D), the cracking is carried out under the protection of an inert gas; the temperature is 1000-1400°C; the rate of heating to the cracking temperature is 2-10°C / min; and the cracking time is 60-120 min.

[0022] The present invention also provides a thermally conductive SiC ceramic-based composite material prepared by the preparation method described above.

[0023] The present invention provides a method for preparing a heat-conducting SiC ceramic-based composite material, comprising the following steps: A) alternately stacking a two-dimensional fiber cloth and a graphene film after high-temperature graphitization treatment, and sewing them with fiber lines to obtain a preform; the material of the two-dimensional fiber cloth includes polyacrylonitrile-based carbon fiber; B) performing a high-temperature debonding treatment on the preform; C) performing a chemical vapor infiltration treatment on the preform after the treatment in step B) to obtain a preform with an interface phase; D) impregnating the preform obtained in step C) with polycarbosilane, and then cross-linking and high-temperature cracking; E) repeating step D) until the weight gain rate of the composite material is less than 3%, thereby obtaining a heat-conducting SiC ceramic-based composite material. The heat-conducting SiC ceramic-based composite material prepared by the present invention has a significantly anisotropic thermal conductivity. In the heat-conducting direction, the heat of the local high-temperature area can be quickly and directionally diverted to the low-temperature area, while in the non-heat-conducting direction, the material is almost heat-insulating, and can also effectively prevent high temperature from damaging other internal components. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The present invention provides a method for preparing a thermally conductive SiC ceramic-based composite material, comprising the following steps:

[0026] A) After the two-dimensional fiber cloth and the graphene film after high-temperature graphitization are alternately stacked, they are sewn with fiber threads to obtain a preform;

[0027] B) subjecting the preform to a high temperature debonding treatment;

[0028] C) subjecting the preform treated in step B) to chemical vapor infiltration treatment to obtain a preform with an interface phase;

[0029] D) impregnating the preform obtained in step C) with polycarbosilane, then cross-linking and pyrolyzing at high temperature;

[0030] E) Repeat step D) until the weight gain of the composite material is less than 3%, thereby obtaining a thermally conductive SiC ceramic-based composite material.

[0031] Regarding step A):

[0032] The two-dimensional fiber cloth and the graphene film after high-temperature graphitization are alternately stacked and then sewn with fiber threads to obtain a preform.

[0033] In certain embodiments of the present invention, the material of the two-dimensional fiber cloth is polyacrylonitrile-based carbon fiber, which can be T300-3K fiber cloth and / or T700-7k fiber cloth. The material of the fiber line is polyacrylonitrile-based carbon fiber, which can be T300-3K fiber cloth and / or T700-7k fiber cloth.

[0034] In certain embodiments of the present invention, the temperature of the high-temperature graphitization treatment is above 2800°C, such as 3000°C. The thickness of the graphene film after the high-temperature graphitization treatment is 10~100 μm, such as 20 μm. The method for preparing the graphene film after the high-temperature graphitization treatment comprises the following steps: under the protection of an inert gas, heat-treating the graphene film at a high temperature of above 2800°C to obtain a graphene film after the high-temperature graphitization treatment. The inert gas may be argon. Before the heat treatment, it also includes: under the protection of an inert gas, heating the graphene film to a high temperature of above 2800°C. The heating rate is 1~10°C / min, such as 5°C / min. The time for heat treatment of the graphene film at a high temperature of above 2800°C is 60~240 min, such as 120 min.

[0035] In certain embodiments of the present invention, after the alternating stacking, the number of layers of the two-dimensional fiber cloth is 2 to 20 layers, such as 11 layers; the number of layers of the graphene film after high-temperature graphitization treatment is 1 to 19 layers, such as 10 layers.

[0036] The suture density of the suture process is 0.3-1 suture thread / cm, such as 0.4 suture thread / cm, 0.6 suture thread / cm.

[0037] Regarding step B):

[0038] The preform is subjected to a high-temperature debonding treatment to obtain a debonded preform.

[0039] In certain embodiments of the present invention, the temperature of the high-temperature debonding treatment is 900-1200°C, such as 900°C, 1200°C; the time is 30-120 min, such as 120 min, 90 min, 40 min. The high-temperature debonding treatment is carried out under the protection of an inert gas. The inert gas may be argon. The purpose of carrying out the treatment under the protection of an inert gas is to decompose the tackifying resin on the surface of the carbon fiber and carry it away with the air flow. The high-temperature debonding treatment is carried out in a tubular furnace.

[0040] Carbon fiber is usually treated with adhesive before leaving the factory. The main purpose of this is to enhance the bonding performance between carbon fiber materials and other materials (such as resin or concrete). The adhesive materials are usually some resin materials, and the preparation and application scenarios of ceramic-based composite materials are accompanied by high temperatures. If debonding treatment is not performed, these resin materials will decompose and produce defects, reducing the performance of the composite material. The high-temperature debonding treatment can separate the carbon fiber in the preform and restore its original mechanical properties.

[0041] Regarding step C):

[0042] The preform treated in step B) is subjected to chemical vapor infiltration treatment (CVI treatment) to deposit an interface phase, thereby obtaining a preform with an interface phase.

[0043] In certain embodiments of the present invention, the chemical vapor infiltration treatment temperature is 600-1300°C, the time is 10-16 h, and the gas source is C 3 H 6 Gas or CH 3 SiCl gas, gas flow rate is 200-1000 mL / min, deposition pressure is 4-12 kPa, deposition interface thickness is 100-1500 nm. The chemical vapor infiltration treatment is carried out in a chemical vapor deposition furnace.

[0044] Specifically, the temperature of the chemical vapor infiltration treatment is 900°C and 1200°C. The time of the chemical vapor infiltration treatment is 12 h, 16 h, and 10 h. The gas flow rate is 200 mL / min and 900 mL / min. The deposition pressure is 6 kPa, 7 kPa, and 10 kPa. The deposition interface thickness is 500 nm and 600 nm.

[0045] Regarding step D):

[0046] The preform obtained in step C) is impregnated with polycarbosilane, and then cross-linked and pyrolyzed at high temperature.

[0047] In certain embodiments of the present invention, the impregnation method may be: immersing the preform in polycarbosilane liquid. The impregnation pressure is less than 10 Pa, such as 0-10 Pa, specifically 8-10 Pa; the time is 10-14 h, such as 12 h. The impregnation is performed in a vacuum oven.

[0048] After the impregnation is completed, the preform is taken out and cross-linked. The cross-linking is carried out under the protection of an inert gas, which may be argon; the temperature is 120-200°C, such as 200°C, 120°C; the rate of heating to the cross-linking temperature is 2-10°C / min, such as 2°C / min, 10°C / min; the cross-linking time is 20-60 min, such as 30 min, 60 min. The pyrolysis is carried out under the protection of an inert gas, which may be argon; the temperature is 1000-1400°C, such as 1100°C, 1400°C; the rate of heating to the pyrolysis temperature is 2-10°C / min, such as 5°C / min; the pyrolysis time is 60-120 min, such as 60 min.

[0049] Regarding step E):

[0050] Repeat step D) until the weight gain rate of the composite material is less than 3%, that is, the densification treatment of the preform is completed to obtain a thermally conductive SiC ceramic-based composite material.

[0051] The heat-conducting SiC ceramic-based composite material prepared by the invention is a directional heat-conducting SiC ceramic-based composite material.

[0052] The present invention also provides a thermally conductive SiC ceramic-based composite material prepared by the preparation method described above.

[0053] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.

[0054] The present invention uses a graphene film after high-temperature graphitization as a thermal conductivity enhancing phase, utilizes the ultra-high horizontal thermal conductivity of the graphene film, maintains its horizontal orientation by arranging layer by layer, forms an efficient heat conduction path in the horizontal direction, and realizes the ultra-high in-plane thermal conductivity of the composite material.

[0055] The present invention uses polyacrylonitrile-based carbon fiber as a toughening phase, so that the obtained thermally conductive SiC ceramic-based composite material has better mechanical properties, lower thermal conductivity and outstanding price advantages. Through layer-by-layer arrangement, the composite material forms a double network structure of graphene thermal conductivity and carbon fiber mechanics, which ensures the mechanical properties of the composite material while achieving thermal insulation performance between composite material layers, and has outstanding cost advantages.

[0056] The heat-conductive SiC ceramic-based composite material prepared by the present invention can quickly conduct heat from a local high-temperature area, reduce the temperature gradient, and prevent high temperature from being conducted along the thickness direction to damage other non-hot end components.

[0057] In order to further illustrate the present invention, a thermal conductive SiC ceramic-based composite material and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments, but it should not be construed as limiting the scope of protection of the present invention.

[0058] The graphene film after high temperature graphitization treatment is prepared according to the following method:

[0059] Under the protection of argon atmosphere, the graphene film was heated to 3000°C at a rate of 5°C / min and heat treated at 3000°C for 120 min to obtain a high-temperature graphitized graphene film with a thickness of 20 μm.

[0060] Example 1

[0061] 1. 11 sheets of T300-3K fiber cloth and 10 sheets of the graphene films treated with high temperature graphitization are alternately stacked together, and sewed together using fiber threads (T300-3K fibers) with a sew density of 0.4 sew threads / cm to obtain a preform.

[0062] 2. The preform is placed in a tubular furnace and debonded at 900° C. for 120 min under argon gas protection to separate the fibers and obtain a debonded preform.

[0063] 3. Place the debonded preform into a chemical vapor deposition furnace and introduce C 3 H 6 The gas was used to deposit a pyrolytic carbon interface at 900 °C. The deposition time was 12 h. The gas flow rate was 200 mL / min and the deposition pressure was 6 kPa. A preform containing a pyrolytic carbon interface with an interface thickness of 500 nm was obtained.

[0064] 4. Place the preform in a vacuum container, pour polycarbosilane until the preform is immersed, then evacuate to 8-10 Pa, maintain the vacuum for 12 hours, then take out the preform, and in an argon protection environment, heat it to 200°C at a rate of 2°C / min for cross-linking for 30 minutes, and then heat it to 1100°C at a rate of 5°C / min for pyrolysis for 60 minutes.

[0065] 5. Repeat the steps of impregnation, cross-linking, and high-temperature cracking in step 4 until the weight gain rate of the composite material is less than 3%, that is, the densification treatment of the preform is completed to obtain a directional heat-conducting SiC ceramic-based composite material.

[0066] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 1.

[0067] Table 1 Performance test results of the composite material of Example 1

[0068]

[0069] Example 2

[0070] 1. 11 sheets of T300-3K fiber cloth and 10 sheets of the graphene films treated with high temperature graphitization are alternately stacked together, and sewed together using fiber threads (T300-3K fibers) with a sew density of 0.6 sew threads / cm to obtain a preform.

[0071] 2. The preform is placed in a tubular furnace and debonded at 900° C. for 90 min under argon gas protection to separate the fibers and obtain a debonded preform.

[0072] 3. Place the debonded preform into a chemical vapor deposition furnace and introduce C 3 H 6 The gas was used to deposit a pyrolytic carbon interface at 900 °C. The deposition time was 16 h. The gas flow rate was 200 mL / min and the deposition pressure was 7 kPa. A preform containing a pyrolytic carbon interface with an interface thickness of 600 nm was obtained.

[0073] 4. Place the preform in a vacuum container, pour polycarbosilane until the preform is immersed, then evacuate to 8-10 Pa, maintain the vacuum for 12 hours, then take out the preform, and in an argon protection environment, heat it to 200°C at a rate of 2°C / min for cross-linking for 30 minutes, and then heat it to 1100°C at a rate of 5°C / min for pyrolysis for 60 minutes.

[0074] 5. Repeat the steps of impregnation, cross-linking, and high-temperature cracking in step 4 until the weight gain rate of the composite material is less than 3%, that is, the densification treatment of the preform is completed to obtain a directional heat-conducting SiC ceramic-based composite material.

[0075] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 2.

[0076] Table 2 Performance test results of the composite material of Example 2

[0077]

[0078] Example 3

[0079] The difference from Example 2 is:

[0080] In step 1, the T300-3K fiber cloth is replaced with the T700-7k fiber cloth. The remaining parameters and steps are the same as those in Example 2 to obtain a thermally conductive SiC ceramic-based composite material.

[0081] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 3.

[0082] Table 3 Performance test results of the composite material of Example 3

[0083]

[0084] Example 4

[0085] The difference from Example 2 is:

[0086] Step 2 is:

[0087] The preform was placed in a tubular furnace and subjected to a debonding treatment at 1200° C. for 40 min under the protection of argon gas, thereby separating the fibers and obtaining a debonded preform.

[0088] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 4.

[0089] Table 4 Performance test results of the composite material of Example 4

[0090]

[0091] Example 5

[0092] The difference from Example 2 is:

[0093] Step 3 is:

[0094] The debonded preform is placed in a chemical vapor deposition furnace and CH 3 SiCl gas was used to deposit a pyrolytic carbon interface at 1200°C. The deposition time was 10 h. The gas flow rate was 900 mL / min and the deposition pressure was 10 kPa. A preform containing a pyrolytic carbon interface with an interface thickness of 500 nm was obtained.

[0095] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 5.

[0096] Table 5 Performance test results of the composite material of Example 5

[0097]

[0098] Example 6

[0099] The difference from Example 2 is:

[0100] Step 4 is:

[0101] The preform is placed in a vacuum container, polycarbosilane is poured until the preform is immersed, and then the vacuum is evacuated to 8-10 Pa. The vacuum is maintained for 12 hours, and then the preform is taken out. In an argon protection environment, the temperature is increased to 120°C at a rate of 10°C / min for cross-linking for 60 minutes, and then the temperature is increased to 1400°C at a rate of 5°C / min for pyrolysis for 60 minutes.

[0102] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 6.

[0103] Table 6 Performance test results of the composite material of Example 6

[0104]

[0105] Comparative Example 1

[0106] The difference from Example 1 is:

[0107] Step 1 is:

[0108] The T300-3K fiber cloth is replaced with an asphalt-based carbon fiber cloth of the same specification; the fiber thread used for stitching is replaced with an asphalt-based carbon fiber, and no graphene film is added; the remaining parameters and steps are the same as those in Example 1, and a thermally conductive SiC ceramic-based composite material is obtained.

[0109] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 7.

[0110] Table 7 Performance test results of the composite material of Comparative Example 1

[0111]

[0112] Comparative Example 2

[0113] The difference from Example 1 is:

[0114] Step 1 is:

[0115] The T300-3K fiber cloth was replaced with an asphalt-based carbon fiber cloth of the same specification; and the fiber thread used for stitching was replaced with an asphalt-based carbon fiber; the remaining parameters and steps were the same as those in Example 1, and a thermally conductive SiC ceramic-based composite material was obtained.

[0116] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 8.

[0117] Table 8 Performance test results of the composite material of Comparative Example 1

[0118]

[0119] Comparative Example 3

[0120] The difference from Example 1 is that (the graphene film is not subjected to high-temperature graphitization treatment):

[0121] Step 1 is:

[0122] Eleven sheets of T300-3K fiber cloth and ten sheets of graphene films were alternately stacked together and sewn together using fiber threads (T300-3K fibers) with a sewing density of 0.4 stitching threads / cm to obtain a preform.

[0123] The remaining parameters and steps are the same as those in Example 1 to obtain a thermally conductive SiC ceramic-based composite material.

[0124] The properties of the composite materials obtained were tested. The in-plane and interlayer thermal conductivities were tested using NETZSCH LFA 467. The density was the volume density, which was measured according to the Archimedean principle and based on the national standard GB / T 25995-2010. The results are shown in Table 9.

[0125] Table 9 Performance test results of the composite material of Comparative Example 3

[0126]

[0127] It can be seen from the above embodiments and comparative examples that the heat-conducting SiC ceramic-based composite material prepared by the present invention has ultra-high thermal conductivity anisotropy, that is, it has ultra-high thermal conductivity in the plane direction, but is almost heat-insulated in the thickness direction. In the direction where heat conduction is required, the material can quickly conduct heat and reduce the temperature gradient, and in the direction where heat conduction is not required, it can block heat conduction and prevent high temperature from damaging other non-hot end components.

[0128] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a thermally conductive SiC ceramic-based composite material, comprising the following steps: A) alternately stacking a two-dimensional fiber cloth and a graphene film after high-temperature graphitization treatment, and sewing them with fiber threads to obtain a preform; the material of the two-dimensional fiber cloth includes polyacrylonitrile-based carbon fiber; B) subjecting the preform to a high temperature debonding treatment; C) subjecting the preform treated in step B) to chemical vapor infiltration treatment to obtain a preform with an interface phase; D) impregnating the preform obtained in step C) with polycarbosilane, then cross-linking and pyrolyzing at high temperature; E) Repeat step D) until the weight gain of the composite material is less than 3%, thereby obtaining a thermally conductive SiC ceramic-based composite material.

2. The preparation method according to claim 1, characterized in that: In step A), the material of the fiber line includes polyacrylonitrile-based carbon fiber.

3. The preparation method according to claim 1, characterized in that: In step A), the temperature of the high temperature graphitization treatment is above 2800°C; The thickness of the graphene film after high-temperature graphitization treatment is 10-100 μm.

4. The preparation method according to claim 1, characterized in that: In step A), the suturing density of the suturing process is 0.3-1 suture thread / cm.

5. The preparation method according to claim 1, characterized in that: In step B), the temperature of the high temperature debonding treatment is 900-1200°C; The high-temperature debonding treatment is carried out under the protection of an inert gas.

6. The preparation method according to claim 1, characterized in that: In step C), the temperature of the chemical vapor infiltration treatment is 600-1300°C, the time is 10-16 h, the gas source is C3H6 gas or CH3SiCl gas, the gas flow rate is 200-1000 mL / min, the deposition pressure is 4-12 kPa, and the deposition interface thickness is 100-1500 nm.

7. The preparation method according to claim 1, characterized in that: In step D), the immersion pressure is less than 10 Pa and the immersion time is 10 to 14 h.

8. The preparation method according to claim 1, characterized in that: In step D), the cross-linking is carried out under the protection of an inert gas; the temperature is 120-200° C.; the rate of heating to the cross-linking temperature is 2-10° C. / min; and the cross-linking time is 20-60 min.

9. The preparation method according to claim 1, characterized in that: In step D), the pyrolysis is carried out under the protection of an inert gas; the temperature is 1000-1400°C; the rate of heating to the pyrolysis temperature is 2-10°C / min; and the pyrolysis time is 60-120min.

10. A thermally conductive SiC ceramic-based composite material prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Graphene paper reinforced carbon / carbon composite material and preparation method thereof

    CN109734468A

  • Ultra-high-temperature ceramic-based composite material with high thermal conductivity, strong bonding force and ablation resistance and preparation method thereof

    CN111454073A

  • Preparation method of C / C-SiC composite material with high thermal conductivity

    CN112110741A

  • Dispersing type heat conduction ceramic-based composite material and preparation method thereof

    CN117303926A

  • Oxidation-ablation-resistant heat-conducting ceramic-based composite material and preparation method thereof

    CN117923923A