Preparation method of low-crystal-point bulk ABS (Acrylonitrile Butadiene Styrene) resin
By adding filtration and screen replacement devices in the ABS resin production line and optimizing process conditions, the problems of impurities and crystal points in ABS resin are solved, product quality and production efficiency are significantly improved, and ABS resin preparation with low crystal points is achieved.
Patent Information
- Application Number
- CN202411142988.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-03
Smart Images

Figure BDA0005001444800000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer compounds, and specifically discloses a method for preparing low-crystal point bulk ABS resin. Background Art
[0002] ABS resin is a thermoplastic polymer material with excellent comprehensive properties. It is currently the most widely used engineering material with the largest output. It is suitable for household electrical appliances such as TV housings, refrigerator linings, vacuum cleaners, etc., as well as plastic products for instruments, telephones, and automobile industries.
[0003] When ABS resin is used for injection molding, crystal points will be generated on the molded sheet. The main reasons are the crystal points of the injection molding raw material ABS resin itself, the injection molding formula and the injection molding extrusion equipment process. At present, the method of reducing the crystal points of the sheet after injection molding and extrusion molding is mostly to add a filter in the extruder, but this method cannot reduce the content of crystal points of the ABS resin raw material itself. Under the condition that the injection molding formula and injection molding equipment process remain unchanged, reducing the crystal points of the raw material ABS resin itself can greatly reduce the crystal points on the sheet after injection molding and improve the economic value of the product.
[0004] In the bulk ABS resin production process, impurities (undissolved particles, excessive polymers, etc.) are generated during the polymerization, transportation and storage of polymers. The raw and auxiliary materials for ABS production carry impurities, and the equipment will drop carbide impurities during long-term operation. If these impurities are carried in ABS resin products, during downstream injection molding production, "crystal points" are formed in the material because the impurities are not easy to melt and disperse. Crystal points with a diameter greater than 700 microns will form "defects" visible to the naked eye on the surface of the ABS resin injection molding material.
[0005] Therefore, how to reduce impurities in ABS resin online to significantly improve the grade of ABS resin products has become a technical challenge. Summary of the invention
[0006] The technical solution adopted by the present invention is as follows:
[0007] In a first aspect, the present invention provides a method for preparing a low-crystal point bulk ABS resin, which specifically comprises the following steps:
[0008] 10-11 parts by weight of low-cis polybutadiene rubber, 12-14 parts by weight of ethylbenzene, 55-65 parts by weight of styrene, and 18-22 parts by weight of acrylonitrile are mixed and dissolved in a glue liquid tank at a temperature not lower than 40° C. to obtain a uniform raw glue liquid without glue lumps; the dissolved glue liquid is filtered through a 100-mesh filter, preheated to a temperature not lower than 80° C., and transported to four plug flow reactors by a conveying device with various additives for bulk polymerization; the total amount of additives added is 0.3-0.8% of the mass of the raw glue liquid as initiator, 1-2.5% of the chain transfer agent, and 1-2.5% of the antioxidant;
[0009] The temperature of the first three reactors is controlled at 100-125°C and increases step by step; the three temperature zones of the fourth reactor are controlled at 140-170°C and increase step by step; the stirring speeds of the four reactors are 5-15 rpm and increase step by step;
[0010] The ABS polymer after the reaction enters the first stage devolatilizer, and the temperature is controlled at 190-200 degrees Celsius; then enters the second stage devolatilizer, and the temperature is controlled at 240-250 degrees Celsius;
[0011] After devolatilization, the material passes through a booster pump, a filter and a screen-changing device and then enters an extruder; the diameter and flow rate of the inlet pipeline of the filter and screen-changing device are set so that the material pressure is in the range of 15-20MPa; the filter screen of the filter and screen-changing device is 100-120 meshes, and impurities, carbides and excessive polymers with larger particle sizes in the polymer are filtered out; the diameter of the outlet pipeline of the filter and screen-changing device is larger than the diameter of the inlet pipeline; the material enters the extruder from the outlet pipeline, and the extruded material is cooled in a water bath and then pelletized to form the final product.
[0012] Preferably, the inner diameter of the inlet pipeline of the filtering and screen changing device is 10 inches, and the outer diameter is 14 inches; the inner diameter of the outlet pipeline of the filtering and screen changing device is 12 inches, and the outer diameter is 16 inches.
[0013] Preferably, the filtering and screen changing device is divided into two branch pipelines before and after, passing through two filter screens at the same time.
[0014] Furthermore, when the equipment is running to the point where the pressure of the filtration and screen changing device is higher than 20MPa, the filtration device on one side is isolated, and the filter screen is replaced by the screen changing equipment, while the filtration device on the other side remains in operation.
[0015] Preferably, the initiator is 1,1-bis(tert-butylperoxy)cyclohexane.
[0016] Preferably, the chain transfer agent is n-dodecyl mercaptan.
[0017] Preferably, the antioxidant is antioxidant 168 or 1010.
[0018] Preferably, the low-cis polybutadiene rubber is one of 55AE and 255T or a mixture of the two.
[0019] Preferably, the obtained ABS resin is formed into a film by a screw extruder, the screw extruder has five temperature zones, one section 245°C / two sections 255°C / three sections 255°C / four sections 255°C / five sections 255°C, the screw extrusion speed is 120r / min, the throughput rate is 3.5m / min, and the traction roller pulls the molten material to form a film.
[0020] In a second aspect, the present invention provides a low crystal point bulk ABS resin, which is prepared by the method described in the first aspect.
[0021] Beneficial effects achieved by the present invention:
[0022] The present invention changes the raw material ratio and process conditions of conventional ABS products, adds filtering and screen changing equipment between the discharge booster pump and the pelletizer of the ABS polymerization device production line, and adjusts the filter screen and pressure to ensure the continuous operation of the device while reducing visible crystal points in the downstream injection molding products, thereby significantly improving the grade and quality of ABS products. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.
[0024] In the following examples and comparative examples, the following substances are used: the initiator is 1,1-bis(tert-butylperoxy)cyclohexane; the chain transfer agent is n-dodecyl mercaptan; the antioxidant is antioxidant 168; and the low-cis polybutadiene rubber is 55AE.
[0025] Comparative Example
[0026] 12% (mass fraction, the same below) of low cis polybutadiene rubber, 11% of ethylbenzene, 60% of styrene, and 17% of acrylonitrile are mixed and dissolved in a glue tank at 30°C to a uniform raw glue solution without glue blocks. The dissolved glue solution is passed through a 100-mesh filter, preheated to 70°C, and transported to four plug flow reactors by a conveying device with various additives for bulk polymerization. The total amount of additives added is 0.3% initiator, 1.1% chain transfer agent, and 1.5% antioxidant. The temperature of the first three reactors is controlled at 100-125°C and increases step by step. The three temperatures of the fourth reactor are controlled at 150°C, 160°C, and 170°C. The stirring speeds of the four reactors are 8, 10, 12, and 12rpm, respectively. The ABS polymer after the reaction enters the first stage devolatilizer, the temperature is controlled at 180°C, and then enters the second stage devolatilizer, the temperature is controlled at 230 degrees Celsius. After devolatilization, the booster pump is used to maintain the pipeline pressure at 4MPa. The material passes through the extruder, and is cooled in a water bath and pelletized to obtain the final ABS resin product. The ABS resin is made into a film through a screw extruder. The screw extruder has five temperature zones, one section at 245°C / two sections at 255°C / three sections at 255°C / four sections at 255°C / five sections at 255°C. The screw extrusion speed is 120r / min, and the passing rate is 3.5m / min. The traction roller pulls the molten material to form an extruded film with a test thickness of 50μm±10μm. After a uniform film is extruded, the film test is started. The test width is 6cm. The crystal point counter is passed longitudinally at a constant pulling rate. The test results are displayed after reaching the test area. The test results are statistically analyzed according to the size grades of crystal point diameters less than 100μm, 100μm-300μm, 300μm-500μm, 500μm-700μm, and greater than 700μm.
[0027] Example 1
[0028] 10% (mass fraction, the same below) of low cis polybutadiene rubber, 12% of ethylbenzene, 58% of styrene, and 20% of acrylonitrile are mixed and dissolved in a glue tank at 40°C to a uniform raw glue solution without glue blocks. The dissolved glue solution is passed through a 100-mesh filter, preheated to 80°C, and transported to four plug flow reactors by a conveying device with various additives for bulk polymerization. The total amount of additives added is 0.3% initiator, 1.1% chain transfer agent, and 1.5% antioxidant. The temperature of the first three reactors is controlled at 100-125°C and increases step by step. The three temperatures of the fourth reactor are controlled at 155°C, 165°C, and 170°C. The stirring speeds of the four reactors are 8, 10, 12, and 12rpm, respectively. The ABS polymer after the reaction enters the first stage devolatilizer, the temperature is controlled at 190°C, and then enters the second stage devolatilizer, the temperature is controlled at 240 degrees Celsius. After devolatilization, the pressure was adjusted to 15 MPa by a booster pump, and then the material entered the filtration and screen changing device and then passed through the filtration device equipped with a 50-mesh filter screen in two ways. After the filtered materials were combined, they entered the extruder from the outlet of the filtration device, cooled in a water bath, and pelletized to obtain the final ABS resin product. The obtained product was tested for crystal point in the same way as the comparative example.
[0029] Example 2
[0030] 10% (mass fraction, the same below) of low-cis-butadiene rubber, 12% of ethylbenzene, 58% of styrene, and 20% of acrylonitrile are mixed and dissolved in a glue tank at 40°C to a uniform raw glue solution without glue blocks. The dissolved glue solution is passed through a 100-mesh filter, preheated to 80°C, and transported to four plug flow reactors by a conveying device with various additives for bulk polymerization. The total amount of additives added is 0.3% initiator, 1.1% chain transfer agent, and 1.5% antioxidant. The temperature of the first three reactors is controlled at 100-125°C and increases step by step. The three temperatures of the fourth reactor are controlled at 155°C, 165°C, and 170°C. The stirring speeds of the four reactors are 8, 10, 12, and 12rpm, respectively. The ABS polymer after the reaction enters the first stage devolatilizer, the temperature is controlled at 190°C, and then enters the second stage devolatilizer, the temperature is controlled at 240 degrees Celsius. After devolatilization, the pressure is adjusted to 15MPa by a booster pump, and then the material enters the filtering and screen changing device and passes through the filtering device equipped with a 100-mesh filter screen in two ways at the same time. After the filtered materials are combined, they enter the extruder from the outlet of the filtering device, and are cooled in a water bath and pelletized to obtain the final ABS resin product. The obtained product is tested for crystal point in the same way as the comparative example.
[0031] Example 3
[0032] 10% (mass fraction, the same below) of low cis polybutadiene rubber, 12% of ethylbenzene, 58% of styrene, and 20% of acrylonitrile are mixed and dissolved in a glue tank at 40°C to a uniform raw glue solution without glue blocks. The dissolved glue solution is passed through a 100-mesh filter, preheated to 80°C, and transported to four plug flow reactors by a conveying device with various additives for bulk polymerization. The total amount of additives added is 0.3% initiator, 1.1% chain transfer agent, and 1.5% antioxidant. The temperature of the first three reactors is controlled at 100-125°C and increases step by step. The three temperatures of the fourth reactor are controlled at 155°C, 165°C, and 170°C. The stirring speeds of the four reactors are 8, 10, 12, and 12rpm, respectively. The ABS polymer after the reaction enters the first stage devolatilizer, the temperature is controlled at 190°C, and then enters the second stage devolatilizer, the temperature is controlled at 240 degrees Celsius. After devolatilization, the pressure is adjusted to 15MPa by a booster pump, and then the material enters the filter and screen changing device and is divided into two paths and simultaneously passes through a filter device equipped with a 150-mesh filter screen. After the filtered materials are combined, they enter the extruder from the outlet of the filter device, and are cooled in a water bath and pelletized to obtain the final ABS resin product. The obtained product is tested for crystal point in the same way as the comparative example.
[0033] Test Results
[0034] The comparative example and the embodiment were tested for impact strength (KJ / m), melt index (g / 10min), and crystal point number, and the comparison results are as follows:
[0035] Table 1 Test results of examples and comparative examples
[0036]
[0037] By changing the raw material ratio and process conditions of conventional ABS products, and adding a filter and screen changing device between the discharge booster pump and the pelletizer of the ABS polymerization unit production line, the number of crystal points in the product can be effectively reduced. Among them, the 100-mesh and 150-mesh filters have a better effect on reducing crystal points, and can effectively remove large-diameter crystal points above 700μm. However, because the pipeline pressure exceeds 20MPa when using a 150-mesh filter, and the filter pressure rises too quickly, the frequency of screen changing increases, the liquid level of the device devolatilizer is unstable, and the risk of carbide falling increases. In summary, the 100-mesh filter and screen changing device can achieve a good effect of reducing crystal points.
[0038] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing low crystal point bulk ABS resin, characterized in that: The specific steps include: 10-11 parts by weight of low-cis polybutadiene rubber, 12-14 parts by weight of ethylbenzene, 55-65 parts by weight of styrene, and 18-22 parts by weight of acrylonitrile are mixed and dissolved in a glue liquid tank to obtain a uniform raw glue liquid without glue lumps; the dissolved glue liquid is passed through a filter with a mesh size of not less than 100, and then transported to four plug flow reactors by a conveying device with various additives for bulk polymerization; the total amount of additives added is 0.3-0.8% of the mass of the raw glue liquid as initiator, 1-2.5% of the chain transfer agent, and 1-2.5% of the antioxidant; The temperature of the first three reactors is controlled at 100-125°C and increases step by step; the three temperature zones of the fourth reactor are controlled at 140-170°C and increase step by step; the stirring speeds of the four reactors are 5-15 rpm and increase step by step; The ABS polymer after the reaction enters the first stage devolatilizer, and the temperature is controlled at 190-200 degrees Celsius; then enters the second stage devolatilizer, and the temperature is controlled at 240-250 degrees Celsius; After devolatilization, the material passes through a booster pump, a filter and a screen changing device and then enters an extruder; the diameter and flow rate of the inlet pipeline of the filter and screen changing device are set so that the material pressure is in the range of 15-20MPa; the filter screen of the filter and screen changing device is 100-120 meshes; the diameter of the outlet pipeline of the filter and screen changing device is larger than the diameter of the inlet pipeline; the material enters the extruder from the outlet pipeline, and the extruded material is cooled in a water bath and then pelletized to form the final product.
2. The method for preparing low crystal point bulk ABS resin according to claim 1, characterized in that: The inner diameter of the inlet pipeline of the filtering and screen changing device is 10 inches, and the outer diameter is 14 inches; the inner diameter of the outlet pipeline of the filtering and screen changing device is 12 inches, and the outer diameter is 16 inches.
3. The method for preparing low crystal point bulk ABS resin according to claim 1, characterized in that: The filtering and screen changing device is divided into two branch pipelines before and after, and passes through two filter screens at the same time.
4. The method for preparing low-crystal point bulk ABS resin according to claim 3, characterized in that: When the equipment is running to the point where the pressure of the filtration and screen changing device is higher than 20MPa, the filtration device on one side is isolated, and the filter screen is replaced by the screen changing equipment, while the filtration device on the other side keeps running.
5. The method for preparing low crystal point bulk ABS resin according to claim 1, characterized in that: The initiator is 1,1-bis(tert-butylperoxy)cyclohexane.
6. The method for preparing low crystal point bulk ABS resin according to claim 1, characterized in that: The chain transfer agent is n-dodecyl mercaptan.
7. The method for preparing low crystal point bulk ABS resin according to claim 1, characterized in that: The antioxidant is antioxidant 168 or 1010.
8. The method for preparing low crystal point bulk ABS resin according to claim 1, characterized in that: The low-cis polybutadiene rubber is one of 55AE and 255T or a mixture of the two.
9. The method for preparing low-crystal point bulk ABS resin according to claim 1, characterized in that: The obtained ABS resin is formed into a film through a screw extruder. The screw extruder has five temperature zones, namely, stage one 245°C / stage two 255°C / stage three 255°C / stage four 255°C / stage five 255°C. The screw extrusion speed is 120r / min, and the throughput rate is 3.5m / min. The traction roller pulls the molten material to form a film.
10. A low crystal point bulk ABS resin prepared by the method according to any one of claims 1 to 9.