Transparent scratch-resistant self-repairing coating material and preparation method thereof

By using asymmetric structure alicyclophase amine curing in the coating, the room temperature viscoelastic response of transparent scratch-resistant self-repair coating is achieved, and the existing coating is solved in the resistance of the The stability issues in terms of scratches and scratch resistance, with efficient self-recovery and good transparency, are suitable for high-demand products such as smart electronic devices, precision instruments and automobiles.

CN119060604AActive Publication Date: 2024-12-03HENAN ACADEMY OF SCI CHEM RES INST CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411065422.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-12-03
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing transparent coating has stability and durability problems in terms of scratch resistance and scratch resistance, and self-repair technology is difficult to meet the high requirements for transparency and aesthetics of products such as smart electronic devices, precision instruments and automobiles. The repairs are limited or require external energy to trigger.

Method used

The synthesis of transparent scratch-resistant self-repair coating is achieved by curing and regulating the siloxane segment modified epoxy resin monomer with asymmetric structure, so as to achieve viscoelastic response under room temperature, thereby achieving coating scratch defects Self-recovery.

Benefits of technology

It realizes efficient self-restoring ability of transparent scratch-resistant self-repair coating, maintains good transparency characteristics and gloss, enhances the coating's weather resistance and waterproof and dust-proof performance, avoids the addition of fillers or additives, and has rapid Controllable repair performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060604A_ABST
    Figure CN119060604A_ABST
Patent Text Reader

Abstract

The invention discloses a transparent scratch-resistant self-repairing coating material and a preparation method thereof, and belongs to the technical field of functional coatings, the preparation method comprises the following steps: stirring and mixing an epoxy resin monomer containing a siloxane chain segment and an alicyclic amine curing agent to obtain a coating casting solution; carrying out vacuum degassing treatment on the coating membrane casting solution; and coating a protected substrate with the casting film solution subjected to vacuum degassing while the casting film solution is hot, curing, taking out, and cooling, so as to obtain the transparent scratch-resistant self-repairing coating. The epoxy resin monomer is modified by using a siloxane chain segment, the flexibility and elasticity of the epoxy resin are optimized, the room-temperature viscoelastic response of the coating is regulated and controlled by using an alicyclic amine curing agent containing an asymmetric structure, and the coating is endowed with excellent scratch-resistant self-repairing performance by improving the internal recovery capability of a polymer network.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional coatings, and in particular relates to a transparent scratch-resistant self-repairing coating material and a preparation method thereof. Background Art

[0002] With the rapid development of smart electronic devices, precision instruments and the automotive industry, the demand for transparent and scratch-resistant surface protection materials is growing. Coating is the most widely used form of surface protection material. It not only gives products aesthetics, but also helps products resist various external intrusion factors as the first line of defense. Smart electronic devices, precision instruments, automobiles and other products are faced with a large number of sharp scratches and wear during use. Damage not only affects the appearance of the product, but also causes the product to be directly exposed to human sweat, wind, sand, rain, snow and other physical and chemical intrusion factors from the user and the external environment. Therefore, there is a huge market demand for coating products that are transparent, scratch-resistant, scratch-resistant and have certain damage self-repair functions. Its application has important practical significance for extending the service life of products, reducing the cost of use, and improving the appearance quality of products.

[0003] At present, there are two main strategies for improving the scratch resistance and mar resistance of coatings. One is to add lubricants or nanofillers to the polymer, and use the lubricants to form a slip layer on the surface of the coating to reduce the friction coefficient of the coating surface. When subjected to external forces, the slip layer can absorb part of the energy and reduce direct damage to the coating. However, this type of coating is prone to lubricant precipitation during long-term use, which affects the stability and durability of the coating. The other is to add nanofillers, mainly by improving the hardness and toughness of the coating, thereby dispersing and absorbing the internal and external stresses acting on the coating surface. However, the dispersion of nanofillers in the coating is difficult to control, and aggregation or uneven dispersion may have an adverse effect on the overall performance of the coating. For the self-repair strategy of coating damage, according to different self-repair mechanisms, it mainly includes two categories: "external aid" self-repair and "intrinsic" self-repair. "External aid" self-repair is to add microcontainers (microcapsules, microvessels) loaded with repair agents inside the material. When the material is damaged, the microcontainers will rupture and release the repair agent at the damaged site. The repair agent will solidify in situ under certain conditions and repair the material damage. However, this repair method determines that the appearance of the defect repaired part will be very different from the original coating, and will leave obvious repair "scars", which cannot meet the application scenarios with extremely high requirements for transparency and aesthetics, such as smart electronic devices, precision instruments, and automotive surfaces. In addition, due to the limitation of microcontainer capacity, the number of effective repairs of this method is extremely limited. "Intrinsic" self-repair is based on the dynamic reversible chemical design of the material itself to achieve self-repair. However, at present, the breaking and recombination of most reversible bonds need to be triggered by external energy such as light and heat, which will affect the properties of the coating itself to a certain extent, and the feature of requiring human intervention also causes application limitations in terms of timeliness and convenience of repair. Therefore, the development of transparent coatings with good scratch resistance and self-repairing properties has always been a hot research and development hotspot that has attracted attention. Summary of the invention

[0004] The present invention provides a transparent scratch-resistant self-repairing coating material and a preparation method thereof. The present invention uses a siloxane segment-modified epoxy resin monomer containing an asymmetric structure to cure and regulate the epoxy resin monomer to synthesize a transparent scratch-resistant self-repairing coating, giving the coating a viscoelastic response at room temperature, thereby achieving a self-recovery response of the scratch defect of the coating.

[0005] In order to achieve the above technical objectives, the technical solution of the present invention is: A method for preparing a transparent scratch-resistant self-repairing coating material comprises the following steps: (1) mixing an epoxy resin monomer containing a siloxane chain segment and an alicyclic amine curing agent to obtain a coating casting solution; (2) vacuum degassing the coating casting liquid; (3) The vacuum degassed casting solution is applied to the protected substrate while hot, solidified, and then removed and cooled to obtain a transparent scratch-resistant self-repairing coating.

[0006] Wherein, in step (1), the molar ratio of the epoxy resin monomer to the alicyclic amine curing agent is 1:0.5-1:1; the stirring conditions are a temperature of 25° C. and a stirring time of 1-2 h.

[0007] The epoxy resin monomer is 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, and the alicyclic amine curing agent is an alicyclic amine curing agent containing an asymmetric structure.

[0008] Wherein, the alicyclic amine curing agent containing an asymmetric structure is isophorone diamine or methylcyclohexane diamine.

[0009] Wherein, in step (2), the vacuum degassing conditions are: temperature 60-70°C, and degassing time 15-30 min.

[0010] Wherein, in step (3), the coating method is spraying, brushing, pouring or dipping; the curing temperature is 60-100°C, and the curing time is 4-12h.

[0011] The present invention also provides a transparent scratch-resistant self-repairing coating material, which is made by adopting the above-mentioned preparation method.

[0012] The technical solution adopted by the present invention is to improve the intrinsic scratch resistance and self-healing properties of the coating by regulating the molecular motion, that is, the bond deformation ability of the molecular structure of the coating. Specifically, by regulating the chemical composition of the coating, a balance between elastic and plastic deformation is achieved, thereby obtaining an ideal viscoelastic behavior. This adjustment allows the coating to absorb and release energy through the movement of molecular chains when subjected to mechanical loads, thereby achieving self-recovery. The regulation of the movement of the molecular chains of the coating is a cost-effective and innovative approach. It not only promotes the plastic deformation ability of the coating and enhances its self-recovery after scratches, but also retains good transparent characteristics because it does not involve the addition of any third components such as fillers or additives. However, achieving viscoelastic-driven surface recovery requires finding a balance between multiple performance parameters, including the dynamic healing ability associated with room temperature, which is affected by the glass transition temperature (T g ). At the same time, the chemical properties of the coating, especially the molecular structure of the polymer and the degree of crosslinking of the polymer network, also play a decisive role in the comprehensive performance of the coating. Therefore, the key to constructing a scratch self-repairing transparent coating material driven only by the intrinsic mechanism is to maintain the polymer T g Below room temperature, the migration ability of polymer chains is improved. After the coating is scratched, low T gThe peculiar viscoelasticity of polymer chains triggers segment migration while inducing bond stretching, enhancing the contact probability of broken bonds and further recovering to their original shape.

[0013] Epoxy resin has excellent mechanical properties, bonding properties and chemical stability, and is currently the most widely used coating resin. However, the interior of traditional epoxy resin materials is a densely cross-linked three-dimensional network, and its cured product is brittle, has low impact strength, and is easily scratched on the surface. g Low, good weather resistance and temperature resistance, flexible and hydrophobic chain segments, introducing them into epoxy resin can significantly improve the flexibility, elasticity, weather resistance, waterproof, dustproof and flame retardant properties of the coating. Although the introduction of flexible segments can reduce the coating T g and improve coating rigidity, but T g Too low will affect the viscoelastic response of the coating at room temperature. In this regard, introducing a curing agent with a specific structure into the design of the epoxy resin system containing silicon oxygen segments can optimize the viscoelasticity of the coating to a certain extent. Alicyclic amine curing agents have a saturated six-membered ring structure and have similar structural characteristics to polyether amines: multiple spatial conformations and good flexibility. At the same time, they also have similar characteristics to aromatic amine structures: rigidity and strength of the ring structure. More importantly, the steric hindrance effect introduced by alicyclic amines with asymmetric structures can significantly improve the plasticizing effect of the coating, thereby enhancing its overall performance. Through structural design, it is expected to combine strength, toughness, scratch resistance and self-healing properties. In addition, most alicyclic amine curing agents are low-viscosity liquids, and the color and gloss of the cured products are better than those of aliphatic amines and polyamides.

[0014] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects: The present invention utilizes siloxane chain segments to modify epoxy resin monomers, optimizes the flexibility and elasticity of epoxy resin, uses alicyclic amine curing agents containing asymmetric structures to regulate the room temperature viscoelastic response of the coating, and imparts excellent scratch resistance and self-repairing properties to the coating by improving the intrinsic recovery ability of the polymer network.

[0015] The present invention provides a transparent scratch-resistant self-repairing coating material and a preparation method thereof. The raw materials required in the invention are all commercially available products. The preparation process does not require any chemical modification steps and can be coated in a variety of ways, which is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the infrared spectrum of the siloxane-modified epoxy coating; Figure 2 It is the DSC analysis diagram of siloxane modified epoxy coating; Figure 3 The scratches on the surface of the siloxane-modified epoxy coating during 100 cycles of scraping with a steel brush; Figure 4 This is the surface scratch condition of the siloxane-modified epoxy coating after 5 cycles of scraping with a steel brush in the comparative example; Figure 5 This is the thermogravimetric analysis diagram of the siloxane-modified epoxy coating; Figure 6 is the light transmittance of the siloxane-modified epoxy coating. DETAILED DESCRIPTION

[0017] The technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0018] This embodiment provides a method for preparing a transparent scratch-resistant self-repairing coating material, comprising the following steps: (1) 1 kg of 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and 0.19 kg of methylcyclohexanediamine (the molar ratio of the two is 1:0.5) are placed in a reactor, stirred and mixed, the reactor temperature is set to 25°C, the stirring time is 1.5 hours, and a coating casting liquid is obtained; (2) The coating casting liquid is subjected to vacuum degassing treatment, and the vacuum degassing conditions are: temperature 65°C, degassing time 25 minutes; (3) The vacuum degassed casting solution is applied to the protected substrate while hot by spraying, brushing, pouring or dipping, and then cured in an oven at 80°C for 8 h, and then taken out and cooled naturally to obtain a transparent scratch-resistant self-repairing coating. Example 2

[0019] This embodiment provides a method for preparing a transparent scratch-resistant self-repairing coating material, comprising the following steps: (1) 1 kg of 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and 0.46 kg of isophorone diamine (the molar ratio of the two is 1:1) are placed in a reactor, stirred and mixed, the reactor temperature is set to 25°C, the stirring time is 1 hour, and a coating casting liquid is obtained; (2) The coating casting liquid is subjected to vacuum degassing treatment, and the vacuum degassing conditions are: temperature 60°C, degassing time 30 minutes; (3) The vacuum degassed casting liquid is applied to the protected substrate while hot by spraying, brushing, pouring or dipping, and then cured in an oven at 60°C for 12 hours, and then taken out and naturally cooled to obtain a transparent scratch-resistant self-repairing coating.

[0020] Comparative Example 1 The difference between Comparative Example 1 and Example 2 is that isophorone diamine is replaced by polyetheramine, comprising the following steps: (1) 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and polyetheramine were stirred and mixed at a molar ratio of 1:1 at a temperature of 25° C. for 2 h to obtain a coating casting solution; (2) The coating casting liquid is subjected to vacuum degassing treatment, and the vacuum degassing conditions are: temperature 70°C, degassing time 15 minutes; (3) The vacuum degassed casting liquid is applied to the protected substrate while hot by spraying, brushing, pouring or dipping, and cured at a curing temperature of 100°C for 4 hours, and then taken out and cooled to obtain a coating.

[0021] The present invention designs a siloxane-modified epoxy resin as a coating film-forming substance, and an asymmetric alicyclic amine as a coating curing agent, and controls the glass transition temperature of the coating, thereby controlling the movement of the polymer molecular chain, thereby achieving viscoelastic driven surface scratch self-repair. Infrared spectrum comparison of siloxane-modified epoxy coating and its monomer ( Figure 1 ) shows, 909 cm -1 The characteristic vibration band of epoxy group at 1000 nm disappeared from the coating sample, which proved that the epoxy resin was cured. The steric hindrance effect provided by the asymmetric structure of alicyclic amine enhanced the plasticizing effect. Figure 2 As shown in Figure 2, the glass transition temperature of the coating is 9.4 °C. The lower glass transition temperature promotes the viscous response and effective elastic behavior of the coating and enhances the autonomous recovery response at room temperature. Figure 3 As shown in the figure, a copper brush was used to scratch the prepared transparent coating 100 times, where (a) is an optical microscope image and (b) is a high-definition lens record. Through optical microscope observation, it was found that the scratches on the coating surface disappeared almost instantly, and no scratch marks were left on the coating surface, showing excellent scratch resistance and self-repairing performance. The comparative example had serious scratches after 5 reciprocating scratches ( Figure 4 Due to the stability of the silicon-oxygen bond, the coating can withstand high temperatures without decomposing easily. The thermal decomposition temperature of the siloxane-modified epoxy coating sample was determined by thermogravimetric analysis. When the sample weight loss rate was 5%, its decomposition temperature (T 5% ) reaches 354 ℃ ( Figure 5 In addition, the coating system does not involve the addition of any third components such as fillers or additives, so that the coating retains good transparency and glossiness. Figure 6As shown, the visible light transmittance of the coating is greater than 90%, and the glossiness (angle 60°) is measured to be 113.7. The excellent optical properties enable the coating protection to maintain the original color and better glossiness of the material without affecting the appearance design of the material. The scratch damage repair behavior of the coating surface in the present invention does not require any conditions to trigger, so it has the significant advantages of fast and controllable response and diverse application scenarios.

[0022] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a transparent scratch-resistant self-repairing coating material, characterized in that The steps include: (1) mixing an epoxy resin monomer containing a siloxane chain segment and an alicyclic amine curing agent to obtain a coating casting solution; (2) vacuum degassing the coating casting liquid; (3) The vacuum degassed casting solution is applied to the protected substrate while hot, solidified, and then removed and cooled to obtain a transparent scratch-resistant self-repairing coating.

2. The method for preparing a transparent scratch-resistant self-repairing coating material according to claim 1, characterized in that: In step (1), the molar ratio of the epoxy resin monomer to the alicyclic amine curing agent is 1:0.5-1:1; the stirring conditions are a temperature of 25° C. and a stirring time of 1-2 h.

3. The method for preparing a transparent scratch-resistant self-repairing coating material according to claim 2, characterized in that: The epoxy resin monomer is 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, and the alicyclic amine curing agent is an alicyclic amine curing agent containing an asymmetric structure.

4. The method for preparing a transparent scratch-resistant self-repairing coating material according to claim 3, characterized in that: The alicyclic amine curing agent containing an asymmetric structure is isophorone diamine or methylcyclohexane diamine.

5. The method for preparing a transparent scratch-resistant self-repairing coating material according to claim 1, characterized in that: In step (2), the vacuum degassing conditions are: temperature 60-70°C, and degassing time 15-30 min.

6. The method for preparing a transparent scratch-resistant self-repairing coating material according to claim 1, characterized in that: In step (3), the coating method is spraying, brushing, pouring or dipping; the curing temperature is 60-100°C, and the curing time is 4-12h.

7. A transparent scratch-resistant self-repairing coating material, characterized in that The invention is prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Scratch-resistant coating

    CN1423682A

  • Coating composition containing silylated derivatives of organic amines and epoxides