Hot isostatic pressure diffusion bonding synchronous aging treatment method for high-temperature alloy and copper alloy
By synchronously performing aging treatment in thermal isostatic diffusion connections, the problems of long process cycles and stress changes in high-temperature alloys and copper alloys are solved, and efficient connections of different metals are achieved, improving the mechanical properties and corrosion resistance of the product.
Patent Information
- Application Number
- CN202411190169.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-28
AI Technical Summary
In the prior art, the connection process cycle between high-temperature alloys and copper alloys is long and the process controllability is poor, which can easily lead to stress concentration and dimensional distortion, affecting the mechanical properties and corrosion resistance of the product.
The synchronous aging treatment method of thermal isostatic pressure diffusion connection is adopted. The solid solution treatment of high-temperature alloy is first carried out, and then bonded to the copper alloy surface. After vacuum sealing and welding, the thermal isostatic pressure diffusion connection is carried out in the thermal isostatic furnace and the same furnace is carried out. In the aging treatment, the heating and pressure increase rate is controlled at 5 to 10°C/min, the pressure is maintained at 100 to 150 MPa, the insulation time is 1 to 4 hours, and the pressure is removed and picked up after cooling.
Shorten the production cycle, improve processing accuracy and production efficiency, avoid metal dedissolution and precipitation, obtain high-performance connecting joints, and reduce costs.
Smart Images

Figure CN119077102A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of dissimilar metal solid phase welding, and in particular to a synchronous aging treatment method for hot isostatic pressing diffusion bonding of a high-temperature alloy and a copper alloy. Background Art
[0002] With the development of aerospace technology, a single high-temperature alloy material cannot meet the development of modern aerospace technology. It is often necessary to prepare a bimetallic structure by welding dissimilar materials to achieve high performance requirements.
[0003] For example, copper and copper alloys have excellent thermal and electrical conductivity. Connecting copper with high-temperature alloys can not only meet the high performance requirements of aerospace components, but also enhance heat dissipation and reduce costs through copper. After solid solution and aging treatment, high-temperature alloys have good strength, corrosion resistance and high-temperature mechanical properties. Therefore, high-temperature alloys are widely used in the aerospace field.
[0004] For precipitation-strengthened high-temperature alloys, solution aging treatment is a common heat treatment method to improve the performance of high-temperature alloys. After solution treatment, the high-temperature alloy obtains a supersaturated solid solution. In the subsequent aging treatment, the second phase precipitates from the supersaturated solid solution and disperses in the matrix to form a precipitation phase. The precipitation phase can effectively prevent the movement of grain boundaries and dislocations and optimize the mechanical properties of high-temperature alloys. However, aging treatment changes the internal stress state of parts and components, making them prone to defects such as dimensional distortion.
[0005] The existing hot isostatic pressing process is to place the product in a closed container, use inert gases such as nitrogen and argon as pressure transmission media, apply equal pressure to the product in all directions under the combined action of high temperature and high pressure, and press and sinter the product. Because the processed workpiece is uniformly pressed in all directions, under the combined action of high temperature and high pressure, the product has the advantages of high density, good uniformity, and excellent performance. The hot isostatic pressing diffusion bonding process can significantly improve the defects such as looseness and shrinkage of the workpiece while completing the connection of the workpiece, and improve the various performances of the product. The effective welding of high-temperature alloys and copper alloys is achieved through hot isostatic pressing diffusion bonding, which avoids the defects such as pores and looseness in traditional welding, and improves the mechanical properties and service life of the product. At present, the conventional process for connecting high-temperature alloys and copper alloys is high-temperature alloy solid solution aging treatment, vacuum diffusion furnace diffusion bonding, and hot isostatic pressing treatment. This process has many production processes, a long cycle, poor process controllability, and is prone to stress concentration, resulting in reduced mechanical properties and corrosion resistance of the material. Experience shows that the longer the stagnation time from the workpiece leaving the factory to the aging treatment, the worse the mechanical properties of the later product.
[0006] The Chinese invention patent application with publication number CN116689929A discloses a hot isostatic pressing diffusion bonding method for copper and stainless steel, wherein the surfaces of the copper and stainless steel to be bonded are treated to make the connection surfaces smooth and free of impurities, the copper and stainless steel are placed in a sleeve for assembly and connection, and then sent into a vacuum degassing furnace to be heated to 300-350°C and kept warm for 3-5 hours. During this process, the sleeve is evacuated to form a seal, and then hot isostatic pressing diffusion bonding is performed, and solution aging treatment is performed after cooling with the furnace. The advantage of this method is that the water vapor and oxygen in the sleeve can be fully removed during the vacuum stage, reducing the production of hydrides and oxides in the subsequent hot isostatic pressing stage, and effectively improving the tensile strength and welding surface bonding rate of the product. However, solid solution aging treatment needs to be performed separately after hot isostatic pressing, the production cycle is long, and metal precipitation is prone to occur during the aging transfer time, which affects the quality of the final product.
[0007] The Chinese invention patent application with publication number CN108544074A discloses a method for diffusion bonding of a high-temperature alloy and an oxygen-free copper ring. A copper sheath is manufactured according to the high-temperature alloy ring. The thickness of the sheath is greater than the thickness of the copper layer of the connector, leaving a certain processing allowance. The surface of the high-temperature alloy ring and the copper sheath are polished and ultrasonically cleaned with acetone. The sheath is sealed and welded with a vacuum electron beam, and placed in a hot isostatic pressing device for hot isostatic pressing diffusion bonding. The excess oxygen-free copper is removed by later mechanical processing. This method effectively avoids the problems of peeling, falling off, delamination and separation of the connection layer from the substrate, reduces the porosity of the connection layer, and achieves good metallurgical bonding. However, this method directly performs hot isostatic pressing diffusion bonding after preparing the high-temperature alloy ring, and does not perform solid solution aging treatment. Problems such as precipitation phase, grain refinement, and stress concentration are prone to occur in the high-temperature alloy, affecting the final product performance. Summary of the invention
[0008] In view of the above problems, the present invention proposes a simultaneous aging treatment method for hot isostatic pressing diffusion bonding of high-temperature alloys and copper alloys, which can improve the strength of the high-temperature alloy while suppressing the dimensional distortion caused by stress changes during the aging process through the diffusion pressure of hot isostatic pressing diffusion bonding, thereby improving processing accuracy, shortening the process cycle of the finished product, and greatly improving production efficiency.
[0009] The technical solution of the present invention is: comprising the following steps: Step 1: Prepare a high-temperature alloy with a predetermined structure and perform a solid solution treatment; Step 2: Prepare a copper alloy with a predetermined structure, polish the surface of the high-temperature alloy and the copper alloy to make it smooth and clean; Step 3: Keep the copper alloy obtained in step 2 in contact with the surface to be connected in the high-temperature alloy structure, and perform vacuum sealing welding; Step 4: Send the vacuum-sealed structural parts into a hot isostatic pressing furnace for hot isostatic diffusion bonding and aging treatment in the same furnace, including: heating and pressurizing in sequence, heat preservation and pressure maintenance in the high temperature stage, pressure maintenance and temperature reduction along with the furnace, and pressure relief and part removal after the parts are cooled to room temperature; The heating rate of the heating and pressure increasing process is 5-10°C / min, and the temperature is increased to 750-850°C; When the pressure in the heating and pressure increasing process rises to 100-150 MPa, the pressure increase is stopped and the heat preservation and pressure maintaining process begins; The high temperature section is kept warm and pressurized for 1 to 4 hours. The temperature is lowered along with the furnace pressure. After the temperature drops to room temperature, the pressure is released and the parts are taken out to obtain the finished product.
[0010] Furthermore, the specific steps of the solution treatment in step 1 are: after heating the high temperature treatment furnace to the solution temperature, quickly put the high temperature alloy into the heat treatment furnace, keep it warm for 5 to 60 minutes, then take out the high temperature alloy and water cool it to room temperature.
[0011] Furthermore, step 2 is specifically as follows: using 120#, 400#, and 800# sandpaper to grind the interfaces of the high-temperature alloy and the copper alloy to be connected step by step, then immersing them in dilute hydrochloric acid, ultrasonically cleaning them in alcohol, drying them with cold air, and sealing and storing the cleaned parts.
[0012] Furthermore, step 3 specifically includes: completely fitting the connecting surface of the copper alloy strip to the surface of the high-temperature alloy part to be connected, and vacuum sealing and welding.
[0013] Furthermore, in step 4, the heating rate of the temperature and pressure increasing process is 5-10°C / min, and the temperature is increased to 750-850°C.
[0014] Furthermore, in step 4, argon gas is filled as a pressure medium to increase the temperature and pressure. When the pressure in the temperature and pressure increasing process reaches 100-150 MPa, the pressure increase is stopped and the temperature and pressure maintaining process begins.
[0015] Furthermore, in step 4, the pressure in the furnace needs to be maintained as the temperature decreases, and the pressure is released and the parts are taken out after the temperature drops to room temperature.
[0016] Furthermore, in step 4, multiple connecting parts can be simultaneously fed into the hot isostatic pressing furnace for hot isostatic pressing treatment.
[0017] Compared with the prior art, the present invention has the following beneficial effects: 1. The hot isostatic pressing diffusion bonding and simultaneous aging treatment process method of the high-temperature alloy and the copper alloy provided by the present invention directly performs hot isostatic pressing diffusion bonding on the high-temperature alloy and the copper alloy and performs aging treatment in the same furnace in the hot isostatic pressing equipment, and simplifies the processes of solid solution, vacuum diffusion bonding, hot isostatic pressing densification, and artificial aging in the traditional process into a new process of solid solution and hot isostatic pressing diffusion bonding, eliminating the process of aging the connecting parts separately, shortening the production cycle, and saving production costs.
[0018] 2. The invention provides a method for simultaneous aging treatment of hot isostatic pressing diffusion bonding of high-temperature alloys and copper alloys. The connecting parts are simultaneously aged during hot isostatic pressing diffusion bonding. There is no aging transfer time, which avoids metal dissolution and precipitation in the high-temperature alloy, obtains high-performance connection joints, and lays a foundation for improving the quality of dissimilar metal connections.
[0019] 3. The hot isostatic pressing diffusion bonding simultaneous aging treatment process method for high-temperature alloys and copper alloys provided by the present invention suppresses dimensional distortion caused by stress changes during aging through the diffusion pressure of hot isostatic pressing diffusion bonding, thereby improving processing accuracy.
[0020] Fourth, the present invention is different from the traditional method of performing solution aging treatment separately after hot isostatic pressing, or performing solution aging treatment before hot isostatic pressing. Instead, considering the characteristics that the aging temperature of the high-temperature alloy is close to the hot isostatic pressing diffusion bonding temperature, the high-temperature alloy is solution treated separately before hot isostatic pressing, and the connecting parts are aged in the same furnace during hot isostatic pressing. The hot isostatic pressing diffusion bonding and aging treatment are carried out simultaneously, which can greatly save time and reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The present invention is a schematic diagram of deep drawing when the high-temperature alloy and copper alloy hot isostatic pressing diffusion bonding simultaneous aging treatment process method is used to manufacture a high-temperature alloy ribbed thin-walled structural part, comprising a high-temperature alloy ribbed wall panel 1, a copper alloy thin plate 2, and a deep drawing upper die 3.
[0022] Figure 2 The hot isostatic pressing assembly schematic diagram is provided for manufacturing a high-temperature alloy ribbed thin-walled structural component by adopting the hot isostatic pressing diffusion bonding and simultaneous aging treatment process method of a high-temperature alloy and a copper alloy provided by the present invention, comprising a high-temperature alloy ribbed wall panel 1 and a copper alloy thin plate 2 which are bonded after deep drawing, a lower sheath 4 and an upper sheath 5.
[0023] Figure 3 The schematic diagram of the finished product of a high-temperature alloy ribbed thin-walled structural part is shown in FIG. 1 , which is manufactured by adopting the hot isostatic pressing, diffusion bonding and simultaneous aging treatment process method of the high-temperature alloy and the copper alloy provided by the present invention.
[0024] Figure 4 The schematic diagram of the assembly of a porous bimetallic rotor plunger manufactured by adopting the hot isostatic pressing diffusion bonding and synchronous aging treatment process method of a high-temperature alloy and a copper alloy provided by the present invention includes a porous bimetallic rotor plunger 6 and a tin bronze cylinder 7.
[0025] Figure 5 The schematic diagram of the finished porous bimetallic rotor plunger is shown in FIG. 1 , which is a schematic diagram of the finished product of the porous bimetallic rotor plunger manufactured by adopting the hot isostatic pressing, diffusion bonding and simultaneous aging treatment process method of the high-temperature alloy and the copper alloy provided by the present invention. DETAILED DESCRIPTION
[0026] In order to clearly illustrate the technical features of this patent, three embodiments of the method of this patent are described in detail below through specific implementation methods and combined with their accompanying drawings. Embodiment 1:
[0027] like Figure 1-Figure 3 As shown, in this embodiment, GH4099 high temperature alloy and T2 copper are used, and the processing target is a ribbed wall plate structure. The method for manufacturing a ribbed thin-walled structure by hot isostatic pressing, diffusion bonding and synchronous aging treatment of a high temperature alloy and a copper alloy includes the following steps: Step 1: Prepare a GH4099 high temperature alloy ribbed wall panel 1 of a predetermined structure and perform a solid solution treatment; The high temperature treatment furnace is heated to a solution temperature of 1140-1170°C. After reaching the target temperature, the ribbed thin-walled part 1 made of GH4099 high temperature alloy is quickly placed in the heat treatment furnace. After keeping the temperature for 5-60 minutes, the GH4099 high temperature alloy ribbed wall panel 1 is taken out and water-cooled to room temperature.
[0028] Step 2: Prepare a T2 copper sheet 2 of a predetermined structure, and polish and clean the surfaces of the GH4099 high-temperature alloy ribbed wall plate 1 and the T2 copper sheet 2; Step 3: placing the copper alloy obtained in step 2 in a package and sealing it with welding to keep it in contact with the surface to be connected in the high-temperature alloy structure; First, the drawing die 3 is designed according to the structure of the GH4099 high-temperature alloy ribbed thin-walled part 1. Considering that one side of the GH4099 high-temperature alloy ribbed thin-walled part 1 has a plurality of array-distributed receiving grooves, the drawing die 3 needs to be adapted to the receiving grooves. Therefore, the die 3 has a plurality of block structures, and corresponds to the receiving grooves one by one. During drawing, the T2 copper sheet 2 is drawn and pressed into the receiving groove to fit the surface of the high-temperature alloy. Then, if Figure 1 As shown, the T2 copper sheet 2 is used as the original blank, the GH4099 high-temperature alloy ribbed wall plate 1 is used as the lower mold, the T2 copper sheet 2 is placed in the center on the upper surface of the GH4099 high-temperature alloy ribbed wall plate 1, and the T2 copper sheet 2 is deep-drawn by a deep-drawing process to fit the inner surface of the accommodating groove of the GH4099 high-temperature alloy ribbed wall plate 1, and the excess copper is removed by machining to obtain Figure 3 The structural parts shown; Finally, the size of the sheath is designed according to the obtained structural part. The sheath includes an upper sheath 4 and a lower sheath 5. After closing, the two sheaths wrap the structure of the ribbed thin-walled part 1 and the entire outer wall of the T2 copper connector 2. The thickness of the sheath should be based on the thickness of the formed connector plus a certain processing allowance. Boron nitride is sprayed on the lower side of the upper sheath 4 and the inner side of the lower sheath 5, and the obtained structural part is placed in the sheath, and vacuum-sealed; Step 4: Send the vacuum-sealed structural parts, the upper and lower packages together into a hot isostatic pressing furnace for hot isostatic diffusion bonding. The assembly method is as follows: Figure 2 As shown; The sheath obtained in step 4 is placed in a hot isostatic pressing furnace, filled with argon as a pressure medium, heated to 750-850°C at 5-10°C, and pressurized to 120-140MPa, kept warm for 1-2h, and then cooled with the furnace while maintaining the pressure. After it drops to room temperature, the pressure is released and the parts are taken out, thereby achieving diffusion bonding between the ribbed thin-walled parts and T2 copper and aging treatment of the high-temperature alloy.
[0029] When discharging, cut the bag obtained in step 4 to obtain the final product. Figure 3 . Embodiment 2:
[0030] like Figure 1-Figure 3 As shown, in this embodiment, the GH4099 high temperature alloy and red copper are processed into ribbed wall plate structural parts. The method for manufacturing ribbed thin-walled structural parts by hot isostatic pressing diffusion bonding and synchronous aging treatment of high temperature alloy and copper alloy includes the following steps: Step 1: Prepare a GH4099 high temperature alloy ribbed wall panel 1 of a predetermined structure and perform a solid solution treatment; The high temperature treatment furnace is heated to a solution temperature of 1140-1170°C. After reaching the target temperature, the ribbed thin-walled part 1 made of GH4099 high temperature alloy is quickly placed in the heat treatment furnace. After keeping the temperature for 5-60 minutes, the GH4099 high temperature alloy ribbed wall panel 1 is taken out and water-cooled to room temperature.
[0031] Step 2: Prepare a copper sheet 2 of a predetermined structure, polish the surface of the GH4099 high-temperature alloy ribbed wall plate 1 and the copper sheet 2 to make them smooth and clean; Step 3: Use diffusion bonding to keep the copper alloy obtained in step 2 in contact with the surface to be connected in the high-temperature alloy structure; First, the drawing die 3 is designed according to the structure of the GH4099 high-temperature alloy ribbed thin-walled part 1. Considering that one side of the GH4099 high-temperature alloy ribbed thin-walled part 1 has a plurality of array-distributed receiving grooves, the drawing die 3 needs to be adapted to the receiving grooves. Therefore, the die 3 has a plurality of block structures, which correspond to the receiving grooves one by one. During drawing, the copper sheet 2 is drawn and pressed into the receiving groove to fit the surface of the high-temperature alloy. Then, if Figure 1 As shown, the copper sheet 2 is used as the original blank, the GH4099 high temperature alloy ribbed wall plate 1 is used as the lower mold, the copper sheet 2 is placed in the center on the upper surface of the GH4099 high temperature alloy ribbed wall plate 1, and the copper is deep-drawn by the deep drawing process to fit the inner surface of the accommodating groove of the GH4099 high temperature alloy ribbed wall plate 1 to obtain Figure 3 The structural parts shown; Finally, the obtained structure is placed in a vacuum sintering furnace, with the graphite mold as the upper and lower pressure heads, and the vacuum is pumped to 10 -3 Pa, heat up to 850-900℃ at 5-10℃ and then pressurize to 3-5MPa, keep warm and keep pressure for 1-2h, then cool down to room temperature with the furnace and take out the parts, at the same time, realize the diffusion connection between the upper surface of the rib of the ribbed thin-walled part 1 and the copper and the aging treatment of the high-temperature alloy.
[0032] Step 4: Put the GH4099 high-temperature alloy and copper connector obtained in step 3 into a hot isostatic pressing furnace, fill it with argon as the pressure medium, heat it to 750-850°C at 5-10°C, increase the pressure to 100-150MPa, keep it warm for 1-2h, then cool it down with the furnace while keeping the pressure, and release the pressure to remove the parts after it drops to room temperature.
[0033] When discharging, the excess copper on the surface of the finished product obtained in step 5 is removed by machining to obtain the final finished product as shown in FIG. Figure 3 . Embodiment 3:
[0034] like Figure 4-Figure 5 As shown, in this embodiment, high-temperature alloy steel and tin bronze are used, and the processing target is a rotor plunger. The method for manufacturing a high-temperature alloy steel porous bimetallic rotor plunger and a tin bronze connector by a hot isostatic pressing diffusion bonding and synchronous aging treatment process of a high-temperature alloy and a copper alloy includes the following steps: Step 1: Prepare a high-temperature alloy steel porous bimetallic rotor plunger 6 of a predetermined structure and perform a solid solution treatment; The high temperature treatment furnace is heated to a solution temperature of 980-1020°C. After reaching the target temperature, the porous bimetallic rotor plunger 6 made of high temperature alloy steel is quickly placed in the heat treatment furnace. After keeping the temperature for 5-60 minutes, the porous bimetallic rotor plunger 6 is taken out and water-cooled to room temperature.
[0035] Step 2: Prepare a tin bronze cylinder 7 of a predetermined structure, and polish and clean the surfaces of the porous bimetallic rotor plunger 6 and the tin bronze cylinder 7 to be connected; Step 3: Use diffusion bonding to keep the surface to be connected of the tin bronze cylinder 7 obtained in step 2 in close contact with the surface to be connected of the porous bimetallic rotor plunger 6; The tin bronze cylinders 7 are placed one by one into the holes of the porous bimetallic rotor plunger 6, and the obtained structural parts are placed in a vacuum sintering furnace, with the graphite mold as the upper and lower pressure heads, and the vacuum is evacuated to 10 -3 Pa, heat up to 850-900℃ at 5-10℃ and then pressurize to 3-5MPa, keep warm and keep pressure for 1-2h, then cool down to room temperature with the furnace and take out the parts, at the same time, realize the diffusion connection between the brim of the tin bronze cylinder 7 and the upper surface of the porous bimetallic rotor plunger 6, and complete the aging treatment of the high-temperature alloy.
[0036] Step 4: Place the porous bimetallic rotor plunger 6 and the tin bronze cylinder 7 obtained in step 3 into a hot isostatic pressing furnace, fill with argon as the pressure medium, increase the temperature to 750-850°C at 5-10°C, increase the pressure to 100-150MPa, keep warm for 1-4h, then cool down with the furnace while maintaining the pressure, and release the pressure and take out the parts after it drops to room temperature.
[0037] When discharging, the finished product obtained in step 4 is taken out, and the tin bronze on the brim of the upper surface is removed by machining to obtain the final finished product as shown in FIG. Figure 5 .
[0038] There are many specific implementation ways of the present invention. The above is only the preferred implementation mode of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements can be made without departing from the principle of the present invention. These improvements should also be regarded as the protection scope of the present invention.
Claims
1. A method for simultaneous aging treatment of hot isostatic pressing diffusion bonding of high temperature alloy and copper alloy, characterized in that: The steps include: Step 1: Prepare a high-temperature alloy with a predetermined structure and perform a solid solution treatment; Step 2: Prepare a copper alloy with a predetermined structure, polish the surface of the high-temperature alloy and the copper alloy to make it smooth and clean; Step 3: Keep the copper alloy obtained in step 2 in contact with the surface to be connected in the high-temperature alloy structure, and perform vacuum sealing welding; Step 4: Send the sealed and welded structural parts into a hot isostatic pressing furnace for hot isostatic diffusion bonding and aging treatment in the same furnace, including: heating and pressurizing in sequence, heat preservation and pressure maintenance in the high temperature section, pressure maintenance and temperature reduction along with the furnace, and pressure relief and part removal after the temperature drops to room temperature; The heating rate of the heating and pressure increasing process is 5-10°C / min, and the temperature is increased to 750-850°C; When the pressure in the heating and pressure increasing process rises to 100-150 MPa, the pressure increase is stopped and the heat preservation and pressure maintaining process begins; The heat preservation and pressure preservation time in the high temperature section is 1 to 4 hours. After the furnace is cooled to room temperature, the pressure is released and the parts are taken out to obtain the finished product.
2. A method for simultaneous aging treatment of hot isostatic pressing diffusion bonding of high temperature alloy and copper alloy according to claim 1, characterized in that: The specific steps of the solution treatment in step 1 are: heating the high temperature treatment furnace to the solution temperature, and after reaching the solution temperature, quickly putting the high temperature alloy into the heat treatment furnace, keeping it warm for 5 to 60 minutes, and then taking out the high temperature alloy and cooling it to room temperature with water.
3. The method for simultaneous aging treatment of hot isostatic pressing diffusion bonding of high temperature alloy and copper alloy according to claim 1, characterized in that: Step 2 is as follows: use 120#, 400#, and 800# sandpaper to polish the interfaces of the high-temperature alloy and the copper alloy to be connected step by step, then soak them in dilute hydrochloric acid, ultrasonically clean them in alcohol, blow dry them with cold air, and seal the cleaned parts for storage.
4. The method for hot isostatic pressing diffusion bonding simultaneous aging treatment of high temperature alloy and copper alloy according to claim 1, characterized in that: Step 3 is specifically as follows: completely fitting the connecting surface of the copper alloy strip to the surface of the high-temperature alloy piece to be connected, and vacuum sealing and welding.
5. A method for simultaneous aging treatment of hot isostatic pressing diffusion bonding of high temperature alloy and copper alloy according to claim 4, characterized in that: The heating rate of the temperature and pressure increasing process in step 4 is 5-10°C / min, and the temperature is increased to 750-850°C.
6. The method for simultaneous aging treatment of hot isostatic pressing diffusion bonding of high temperature alloy and copper alloy according to claim 1, characterized in that: In step 4, argon gas is filled as the pressure medium to increase the temperature and pressure. When the pressure in the temperature and pressure increase process reaches 100-150 MPa, the pressure increase is stopped and the temperature and pressure maintenance process begins.
7. The method for hot isostatic pressing diffusion bonding simultaneous aging treatment of high temperature alloy and copper alloy according to claim 1, characterized in that: In step 4, the pressure is maintained as the furnace cools down, and the pressure is released and the parts are taken out after the temperature drops to room temperature.
Citation Information
Patent Citations
Vacuum diffusion bonding method for TC18 titanium alloys
CN103317225A
Manufacturing method of target assembly
CN105624622A
Hot isostatic pressure diffusion bonding method of copper chromium zirconium-stainless steel composite plate
CN108067724A
Hot isostatic pressing treatment process method for casting forming ZL101A aluminum alloy
CN111500952A
Heat treatment method for selective laser melting forming GH4099 high-temperature alloy
CN115502416A