Material adding device, material adding method, welding method and defect repairing method

By designing an additive device with multiple feed pipes and feed control devices, the problem of difficulty in achieving continuous additives of mixed materials in the prior art is solved, precise control of the proportion of additive raw materials is achieved, and the scope of application of additives is expanded. And improves welding and defect repair quality.

CN119077110APending Publication Date: 2024-12-06CHINA-UKRAINE INST OF WELDING GUANGDONG ACAD OF SCI
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411235956.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing friction stir additive technology is difficult to meet the continuous additive needs of mixed materials, especially for the additive needs of continuously changing material ratios, and it is impossible to effectively use materials such as debris, particles or powder for additives.

Method used

An additive device is designed, including multiple feed pipes and feed control devices. Through the mixing and control of different additive raw materials, the additive raw material ratio can be adjusted accurately in the agitating chamber, and the input can be made into the agitating chamber. Different portions of additive raw materials and the rotation and movement of the agitating tool can be used to achieve additive, welding and defect repair.

Benefits of technology

The continuous additive of mixed materials is realized, the scope of application of additives is expanded, and the diverse additive needs can be met, the welding quality and defect repair effect is improved, and the thinning problem of friction stir welds is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077110A_ABST
    Figure CN119077110A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solid phase additive manufacturing, and discloses an additive device, an additive method, a welding method and a defect repairing method.The additive device comprises a main shaft and an outer shaft shoulder, a stirring cavity is formed between the outer shaft shoulder and the main shaft, a cutter handle and a stirring tool are arranged in the stirring cavity, and the end, away from the stirring tool, of the cutter handle is connected with the main shaft; a discharge opening is formed in one side, close to the stirring tool, of the stirring cavity; the outer shaft shoulder is connected with a plurality of feeding pipelines, each feeding pipeline is provided with a feeding control device, the feeding pipelines communicate with the stirring cavity so as to input additive raw materials into the stirring cavity, and the feeding control devices are used for controlling the proportion of the additive raw materials input into the stirring cavity; different material adding raw materials can be input into the stirring cavity through different feeding pipelines, the feeding control device can control the quantity of the different material adding raw materials entering the stirring cavity, and therefore the proportion of the mixed material adding raw materials can be adjusted, the application range of the material adding is wider, and the using requirements of material adding, welding and repairing can be better met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid-phase additive manufacturing, and in particular to an additive device and additive method, a welding method and a defect repairing method. Background Art

[0002] Additive Manufacturing (AM) is the process of pre-building and planning 3D models through computer technology, combining digital controllable heat sources to melt, clad or stack materials layer by layer to quickly form structural or functional parts. It has five major technical characteristics: digital manufacturing, dimensionality reduction manufacturing, accumulation manufacturing, direct manufacturing, and rapid manufacturing. It has received widespread attention around the world and has brought a series of profound changes to the traditional manufacturing industry. It can be widely used in aerospace, national defense, medical, architectural design, automobile manufacturing and other fields.

[0003] Among them, the friction stir additive technology is to generate heat through friction between materials, so that the material is plasticized but not melted, thereby achieving additive. However, the existing friction stir additive technology can often only perform additive processing on a single material. When faced with mixed additives such as granular materials and powder materials, mixed additives of materials with different components, and mixed additives of materials of different materials, it is often difficult to meet the use requirements, especially when the material ratio has a continuously changing additive demand, it is even more difficult to meet. Its scope of use is limited and it is difficult to meet the growing demand for additives. In addition, in the existing technology, general additive methods can often only use wires or rods, but some materials do not have finished wires or rods. The existing additive devices and methods cannot use debris, particles or powders for additives, and the limitations of its material use are also large. Summary of the invention

[0004] The technical problem to be solved by the present invention is: how to realize continuous addition of mixed materials. In order to solve the above technical problem, the present invention provides an additive device, including a coaxially arranged main shaft and an outer shoulder, the outer shoulder is fixedly connected to the main shaft and forms a stirring chamber, a coaxially fixedly connected knife handle and a stirring tool are arranged in the stirring chamber, the end of the knife handle away from the stirring tool is coaxially fixedly connected to the main shaft, and the stirring chamber is provided with a discharge opening on a side close to the stirring tool;

[0005] The outer shoulder is connected to a plurality of feed pipes, each of which is provided with a feed control device. The feed pipe is connected to the stirring chamber to input additive raw materials into the stirring chamber, and the plurality of feed control devices are used to control the ratio of the additive raw materials input into the stirring chamber.

[0006] Preferably, the feed control device comprises a first control valve and a second control valve which are arranged on the feed pipeline, a silo is formed between the first control valve and the second control valve, and a weight sensor is arranged in the silo.

[0007] Preferably, it also includes a cooling device, which includes a cooling bin sleeved on the outer wall of the outer shaft shoulder, the cooling bin is connected to a water inlet pipeline and a water outlet pipeline, a temperature sensor is provided at the water outlet end of the cooling bin, and a flow rate controller is provided at the water inlet end of the cooling bin.

[0008] Preferably, the end surface of the stirring tool away from the handle is flush with the end surface of the outer shoulder away from the main body.

[0009] Preferably, the outer wall of the stirring tool is provided with a thread, the pitch of the thread is 3mm to 10mm, and the difference between the inner diameter and the outer diameter of the thread is 4mm to 10mm; the end of the stirring tool away from the tool handle is provided with a cone, and the cone is used to be inserted into the substrate to be added.

[0010] Preferably, the stirring tool is made of tool steel, nickel-based alloy or tungsten-rhenium alloy.

[0011] Preferably, the additive raw material is a granular material, a powder material, a chip material, or any combination of granular material, powder material and chip material.

[0012] The present invention also provides an additive method, which uses the additive device described above and includes the following steps:

[0013] A1. Start the spindle, which drives the stirring tool to rotate at a set speed in the stirring chamber through the tool handle, and move the position of the additive device so that the cone at the end of the stirring tool moves to the working position, and then the cone is inserted downward into the substrate, while keeping the distance between the lower end surface of the outer shoulder and the substrate within a first preset range;

[0014] A2. According to the preset material ratio, different additive raw materials of different amounts are simultaneously delivered to the stirring chamber through the feed pipe. After the additive raw materials in the stirring chamber are evenly mixed and fully rubbed and plasticized by the substrate, the equipment is started to move the entire additive device along the planned path to achieve preliminary additive;

[0015] A3. When the previous layer of material addition is completed, the material addition device is lifted to the starting working position of the next layer, and then step A2 is repeated to achieve multi-layer material addition;

[0016] A4. When the additive process is completed, the delivery of the additive raw material is stopped, the spindle stops rotating, and the additive device is lifted and reset to the initial position.

[0017] The present invention also provides a welding method, using the aforementioned material adding device, comprising the following steps:

[0018] B1. Start the spindle, which drives the stirring tool to rotate at a set speed in the stirring chamber through the tool handle, and move the position of the additive device so that the cone at the end of the stirring tool moves to the working position, and then the cone is inserted downward between the two plates to be welded, so that the tip of the cone is flush with the bottom of the plates to be welded, and at the same time, the distance between the lower end surface of the outer shoulder and the plates to be welded is kept in the second preset range;

[0019] B2. The solder is transported into the stirring chamber through the feed pipe. After the solder in the stirring chamber and the plate to be welded are fully rubbed and plasticized, the equipment is started to move the entire additive device along the planned path to achieve welding and form a weld with excess height at the welding point;

[0020] B3. When the welding track reaches the final point, keep the spindle rotating and feeding, lift the welding rod to the first preset height at a certain speed, and move the welding rod to the first preset length in the opposite direction. After the welding is finished, lift the welding rod to the first preset height at a certain speed again, and move the welding rod to the first preset length along the original track.

[0021] B4. Repeat step B3 until the bottom of the stirring needle is higher than the weld surface;

[0022] B5. Stop feeding the solder, stop the spindle from rotating, and lift the additive device to reset it to its initial position.

[0023] The present invention also provides a defect repair method, which uses the above-mentioned additive device and includes the following steps:

[0024] C1. Start the spindle, which drives the stirring tool to rotate at a set speed in the stirring chamber through the tool handle, and move the position of the additive device so that the cone at the end of the stirring tool moves to the working position, and then the cone is inserted downward into the defect of the plate to be repaired and stays at the defect for a preset time;

[0025] C2. Start the equipment to move the additive device along the defect track, and at the same time, deliver the repairing raw material of the same material as the plate to be repaired into the stirring chamber through the feed pipe to complete the repair of the defect;

[0026] C3. When the welding track reaches the final point, keep the spindle rotating and feeding, lift it to the second preset height at a certain speed, and move it to the second preset length in the opposite direction. After the end, lift it to the second preset height at a certain speed again, and move it along the original track for the second preset length.

[0027] C4. Repeat step C3 until the bottom of the stirring needle is higher than the weld surface;

[0028] C5. Stop feeding the solder, stop the spindle from rotating, and lift the additive device to reset to its initial position.

[0029] Compared with the prior art, the additive device, additive method, welding method and defect repair method provided in the embodiments of the present invention have the following beneficial effects:

[0030] In the present invention, a plurality of feed pipes are connected to the stirring chamber, and different feed pipes can input different additive raw materials into the stirring chamber. Different additive raw materials are stirred and driven by a stirring tool in the stirring chamber to be fully mixed. Under the triple action of the external shoulder, the stirring tool and the substrate, the mixed additive raw materials are plasticized and extruded from the discharge opening onto the substrate to complete the additive process. The feed control device can control the amount of different additive raw materials entering the stirring chamber, thereby continuously adjusting the material ratio of the mixed additive raw materials, so that the application range of the additive is wider and can meet more additive needs.

[0031] In addition, during welding, solder can be added to the weld, and the obtained weld thickness is greater than or equal to the material being welded, avoiding the reduction of load-bearing capacity caused by the thinning of the stir friction weld. At the same time, at the end of welding, the keyhole at the tail of the stir friction weld can be backfilled with welding by adding solder, without the need for additional repair or extraction. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a front view of the present invention;

[0033] Figure 2 The present invention Figure 1 A cross-sectional view of

[0034] Figure 3 It is a schematic structural diagram of the additive method of the present invention;

[0035] Figure 4 is a schematic diagram of the steps of the additive method of the present invention;

[0036] Figure 5 It is a structural schematic diagram of the welding method of the present invention;

[0037] Figure 6 It is a schematic diagram of the steps of the welding method of the present invention;

[0038] Figure 7 It is a structural schematic diagram of the defect repair method of the present invention;

[0039] Figure 8 It is a schematic diagram of the steps of the defect repair method of the present invention.

[0040] In the figure: 1. main shaft; 2. outer shoulder; 3. stirring chamber; 31. discharge opening; 4. knife handle; 5. stirring tool; 51. cone; 52. thread; 6. feed pipe; 7. feed control device; 71. first control valve; 72. second control valve; 73. silo; 74. weight sensor; 8. cooling device; 81. cooling silo; 82. water inlet pipe; 83. water outlet pipe; 84. temperature sensor; 85. flow rate controller; 9. substrate; 10. plate to be welded; 11. plate to be repaired. DETAILED DESCRIPTION

[0041] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0042] like Figure 1 and Figure 2 As shown, a preferred embodiment of the present invention provides an additive device, comprising a coaxially arranged main shaft 1 and an outer shoulder 2, the outer shoulder 2 is fixedly connected to the main shaft 1 and forms a stirring chamber 3, a coaxially fixedly connected tool handle 4 and a stirring tool 5 are arranged in the stirring chamber 3, the tool handle 4 is coaxially fixedly connected to the main shaft 1 at one end away from the stirring tool 5, and the stirring chamber 3 is provided with a discharge opening 31 on a side close to the stirring tool 5;

[0043] The outer shoulder 2 is connected to a plurality of feed pipes 6 , and the feed pipes 6 are provided with a feed control device 7 . The feed pipes 6 are connected to the stirring chamber 3 to input the additive raw materials into the stirring chamber 3 . The plurality of feed control devices 7 are used to control the ratio of the additive raw materials input into the stirring chamber 3 .

[0044] See also Figure 1 Specifically, a plurality of feed pipes 6 are respectively connected to different raw material storage bins, and the raw material storage bins can input additive raw materials into the stirring chamber 3. Different additive raw materials are stored in different raw material storage bins. The different additive raw materials are fully mixed in the stirring chamber 3, and then frictionally plasticized, and finally discharged to the substrate 9 to be added through the discharge opening 31. In the actual additive process, with different additive requirements, for example, when alloy materials with different proportions are required, or when alloy materials with continuously changing material proportions are required, or when different metals need to be added alternately, or when the additive appearance color needs to change continuously to form a gradient color, the ratio between different additive raw materials also needs to change to meet the requirements of use.

[0045] In the first specific embodiment, when a fixed ratio of alloy material is required for additive manufacturing, a traditional practice is to pre-mix a certain amount of alloy powder with a fixed ratio, and then transport the mixed powder to the stirring chamber 3 through a feed pipeline for additive manufacturing. However, it is difficult to accurately control the amount of alloy powder that needs to be pre-mixed. If the amount is too small, it will not be enough, and if the amount is too large, it will easily cause waste, and the mixed alloy powder will also be difficult to completely separate. In this embodiment, each feed control device 7 can be preset and adjusted according to the material ratio required for the additive alloy powder, so that the additive raw materials entering the stirring chamber 3 at the same time meet the material ratio required for the additive layer, thereby meeting the additive requirements. This method is suitable for additive or welding processing of some alloy materials with special material requirements.

[0046] In the second specific embodiment, due to special needs, when the material ratio of the additive layer needs to be continuously changed to achieve special effects such as color gradient or performance gradient, the traditional additive device is often unable to achieve the above-mentioned complex additive needs because a single feed pipeline inputs a single additive raw material; in this embodiment, multiple feed control devices 7 can be used to control the input speed and input amount of different additive raw materials at the same time to continuously adjust the input state of each additive raw material, and then continuously adjust the material ratio of the additive layer.

[0047] In the third specific embodiment, when different materials of metal need to be used for alternating additives due to special needs, the traditional method of switching additive raw materials is often troublesome. It is necessary to stop the additive and then replace the additive raw materials before continuing the additive. This makes the additive layers not continuous and the work efficiency is also low. In this embodiment, when it is necessary to switch different metal materials for alternating additives, the timing of different metal materials entering the stirring chamber 3 can be controlled by the feed control device 7, so as to achieve the continuity of alternating additives of different metal materials without stopping the additive device, and the work efficiency will be higher.

[0048] In some embodiments, the feed control device 7 includes a first control valve 71 and a second control valve 72 disposed on the feed pipe 6 , a silo 73 is formed between the first control valve 71 and the second control valve 72 , and a weight sensor 74 is disposed in the silo 73 .

[0049] The silo 73 can temporarily store the additive raw materials, and the weight sensor 74 can monitor the weight of the additive raw materials in the silo 73. According to the data fed back by the weight sensors 74 in the multiple feed pipes 6, the first control valve 71 and the second control valve 72 can be intelligently adjusted to thereby realize the control of the additive raw material ratio.

[0050] Specifically, in the first embodiment, according to the amount of additive raw materials per unit time required for actual additive and the ratio between the various additive raw materials, the ratio of the opening of the first control valve 71 and the second control valve 72 in each feed control device 7 can be adjusted, so as to accurately control the amount of each additive raw material input into the stirring chamber 3, accurately control the ratio of the additive raw materials, and when the additive is completed, the first control valve 71 and the second control valve 72 can be closed in time to avoid the problem of insufficient or waste of additive raw materials caused by the early mixing of the additive raw materials, and the unmixed additive raw materials can be better recycled and reused later. In this solution, the weight sensor 74 can monitor the change of the weight of the additive raw materials in the silo 73 in real time. When the fluctuation of the weight change exceeds the preset range, the additive can provide feedback in time and adjust the opening of each first control valve 71 and the second control valve 72 to make the ratio of the additive raw materials more accurate. In addition, in the mode of the above-mentioned embodiment, the real-time adjustment of the input amount of the additive raw material is achieved by real-time adjustment of the opening of the two control valves in the feed control device 7; for the second embodiment in which the additive raw material needs to be continuously changed, the above-mentioned method can also be used to control multiple first control valves 71 and second control valves 72, and the weight sensor 74 performs weight feedback to achieve it.

[0051] Furthermore, in another working mode, since the additive raw material needs to be fully stirred, frictionally and plasticized in the stirring chamber 3 before additive can be carried out, there is a plasticization time period. During this time period, the additive raw material enters the silo 73 through the first control valve 71 for the second time. At this time, the second control valve 72 is in a closed state, and the gravity sensor continuously monitors the weight of the additive raw material in the silo 73. When it is monitored that the weight of the additive raw material in the silo 73 reaches the preset standard weight of a single input, the first control valve 71 is closed. When the weight of all the additive raw materials required reaches the standard weight of a single input, it means that the additive raw material ratio at this time also reaches the preset standard. At this time, all the second control valves 72 can be opened synchronously, so that all the additive raw materials are synchronously input into the stirring chamber 3 for stirring, frictional and plasticization, thereby completing the additive preparation process and preparing for additive work. At this time, the second control valve 72 is closed again, the first control valve 71 is opened, the feed pipe 6 starts to input the additive raw material into the silo 73, and the weight sensor 74 repeats the weight monitoring and control.

[0052] In the third embodiment, the input control of the additive raw material is relatively simple. When adding material, the two control valves in one of the feed control devices 7 are always opened. The weight sensor 74 also monitors the amount of additive raw material that has been output and feeds back information to a processor such as a computer. The processor determines when to switch the additive raw material based on the preset additive length. When it is necessary to switch to other metals for additive, the control valves in the original feed control device 7 are all closed, and the two control valves on the other new feed control device 7 are opened. The opening of the control valve is adjusted according to the actual additive demand.

[0053] In some embodiments, a cooling device 8 is also included, which includes a cooling bin 81 sleeved on the outer wall of the outer shoulder 2, the cooling bin 81 is connected to a water inlet pipeline 82 and a water outlet pipeline 83, a temperature sensor 84 is provided at the water outlet end of the cooling bin 81, and a flow rate controller 85 is provided at the water inlet end of the cooling bin 81.

[0054] Specifically, during the friction stirring process, the temperature of the additive raw material needs to be controlled. If the temperature of the additive raw material is too high, the additive raw material is easy to melt, which is not convenient for the additive work. The cooling chamber 81 sleeved on the outer wall of the outer shoulder 2 can take away the heat of the additive raw material in the stirring chamber 3 by continuously inputting cooling water, and the flow rate and flow of the cooling water are controlled by the flow rate controller 85 to control the temperature of the additive raw material, so that the additive raw material can be plasticized after being fully stirred without melting, which is convenient for the smooth development of the subsequent additive work.

[0055] In some embodiments, the end surface of the stirring tool 5 away from the handle 4 is flush with the end surface of the outer shoulder 2 away from the main body.

[0056] Furthermore, a thread 52 is provided on the outer wall of the stirring tool 5, the pitch of the thread 52 is 3mm to 10mm, and the difference between the inner diameter and the outer diameter of the thread 52 is 4mm to 10mm; a cone 51 is provided at one end of the stirring tool 5 away from the handle 4, and the cone 51 is used to be inserted into the substrate 9 to be added.

[0057] Furthermore, the stirring tool 5 is made of tool steel or nickel-based alloy or tungsten-rhenium alloy.

[0058] Specifically, the end of the outer shoulder 2 away from the main shaft 1 is provided with a discharge opening 31, and the discharge opening 31 is connected to the stirring chamber 3. The plasticized additive raw material in the stirring chamber 3 is discharged to the substrate 9 through the discharge opening 31, and the end face of the stirring tool 5 away from the handle 4 is flush with the end face of the discharge opening 31, so that the plasticized additive raw material can be better and more stably discharged to the substrate 9 without additive defects. As the friction stirring additive device moves, the end face of the outer shoulder 2 can apply pressure to the additive raw material, making the additive layer more flat and stable. The pitch and other size ranges of the thread 52 on the stirring tool 5 are the preferred ranges in one embodiment. In addition, the cone 51 is inserted into the substrate 9, and the additive raw material that has been initially stirred, frictionally and plasticized in the stirring chamber 3 flows downward under the guidance of the cone 51 and contacts the substrate 9. As the stirring tool 5 rotates, the cone 51 will also rotate, which can make the additive raw material and the substrate 9 fully frictionally plasticized, so that the additive raw material can be better combined with the substrate 9, and the connection between the additive layer and the substrate 9 is also tighter and more reliable.

[0059] Furthermore, the additive raw material is a granular material, a powder material, a chip material, or any combination of granular material, powder material, and chip material.

[0060] It should be noted that in the existing technology, some alloy materials do not have the form of wires or rods, and their external form is mostly plates. These plates will produce a large amount of debris, powder or particles during the processing. For this part of the material, the existing additive devices and additive methods are often unable to recycle. In the present invention, when the additive raw materials are mixed, the feed pipe 6 can be fed with metal powder, metal particles, metal debris, etc., or a mixture of two or three materials. Furthermore, the material of the additive can also be a non-metallic material, such as different plastic particles or resin particles. The additive device and method in the present application can fully recycle the debris or particles or powder generated after processing different plates for additive. The use range of its additive is wider, and the recycled materials can be better utilized, making the additive cost lower; and the use of debris raw materials or granular raw materials also enables the feed control device 7 to better control the amount of additive raw materials input into the stirring chamber 3 through the feed pipe 6, so that the control of the additive raw material ratio is more precise, and various additive raw materials are easier to be mixed evenly in the stirring chamber 3; of course, in the actual production process, granular materials, powder materials and debris materials can be used alone, or they can be used in combination of two or three, which makes the application of the device more extensive.

[0061] like Figure 3 and Figure 4 As shown, the present invention also provides an additive method, which uses the additive device described above and includes the following steps:

[0062] A1. Start the spindle 1, which drives the stirring tool 5 to rotate at a set speed in the stirring chamber 3 through the tool handle 4, and move the position of the additive device so that the cone 51 at the end of the stirring tool 5 moves to the working position, and then the cone 51 is inserted downward into the substrate 9, while keeping the distance between the lower end surface of the outer shoulder 2 and the substrate 9 within a first preset range;

[0063] A2. Different amounts of different additive raw materials are simultaneously delivered to the stirring chamber 3 through the feed pipe 6 according to the preset material ratio. After the additive raw materials in the stirring chamber 3 are evenly mixed and fully rubbed and plasticized by the substrate 9, the device is started to move the entire additive device along the planned path to achieve preliminary additive.

[0064] A3. When the previous layer of material addition is completed, the material addition device is lifted to the starting working position of the next layer, and then step A2 is repeated to achieve multi-layer material addition;

[0065] A4. When the additive process is completed, the delivery of the additive raw material is stopped, the spindle 1 stops rotating, and the additive device is lifted and reset to the initial position.

[0066] Among them, when it is necessary to perform additive work, the additive device is first moved to the working position through the displacement device, and the substrate 9 to be added is fixed on the workbench below the working position. At the same time, the spindle 1 also rotates and drives the stirring tool 5 to rotate through the tool handle 4. When the stirring tool 5 reaches the working position and the rotation speed reaches the preset speed, the displacement device will drive the stirring friction device to move downward, so that the cone 51 at the end of the stirring tool 5 is inserted into the substrate 9 until the distance between the outer shoulder 2 and the substrate 9 is 1mm to 3mm; then, according to the preset ratio of each additive raw material, different amounts of different additive raw materials are input into the stirring chamber 3 through the feeding pipe 6, so that the multiple additive raw materials can be fully mixed in the stirring chamber 3, and then driven by the stirring tool 5 to stir Stir and rub, and contact and rub with the substrate 9 for plasticization. After the additive raw material and the substrate 9 are rubbed for a preset time, the equipment can be started, and the displacement device drives the additive device to move along the planned path to realize the additive work of the bottom additive layer; and when the upper additive layer is formed, the displacement device will lift the additive device and move it to the starting working position of the next layer, and then the new additive raw material can be transported into the stirring chamber 3 through the feeding pipe 6 to carry out the second layer of additive work. This cycle can realize multi-layer additive. It should be noted that the ratio of the additive raw materials between each additive layer can be different. The amount of additive raw materials input into the stirring chamber 3 by adjusting each feeding pipe 6 can be different each time the additive is added, that is, the alternating additive of different metal materials can be realized.

[0067] like Figure 5 and Figure 6As shown, the present invention also provides a welding method, using the aforementioned material adding device, comprising the following steps:

[0068] B1. Start the spindle 1, which drives the stirring tool 5 to rotate at a set speed in the stirring chamber 3 through the tool handle 4, and move the position of the material adding device so that the cone 51 at the end of the stirring tool 5 moves to the working position, and then the cone 51 is inserted downward between the two plates to be welded, so that the tip of the cone 51 is flush with the bottom of the plate 10 to be welded, and at the same time, the distance between the lower end surface of the outer shoulder 2 and the plate 10 to be welded is kept within a second preset range;

[0069] B2. The solder is conveyed into the stirring chamber 3 through the feeding pipe 6. After the solder in the stirring chamber 3 and the plate 10 to be welded are fully rubbed and plasticized, the equipment is started to move the entire additive device along the planned path to achieve welding and form a weld with excess height at the welding position;

[0070] B3. When the welding track reaches the final point, keep the spindle rotating and feeding, lift the welding rod to the first preset height at a certain speed, and move the welding rod to the first preset length in the opposite direction. After the welding is finished, lift the welding rod to the first preset height at a certain speed again, and move the welding rod to the first preset length along the original track.

[0071] B4. Repeat step B3 until the bottom of the stirring needle is higher than the weld surface;

[0072] B5. Stop feeding the solder, stop the spindle from rotating, and lift the additive device to reset to its initial position.

[0073] Among them, the first preset height is 0.5mm to 1mm, and the first preset length is 5mm to 10mm. When it is necessary to weld two plates, first fix the plates to be welded on the workbench through the limit device, and determine the starting point and end point of the welding path, and then move the additive device to the initial preset working position through the displacement device, that is, above the starting point of the welding path, and then start the spindle 1 to make the rotation speed of the stirring tool 5 reach the preset speed, and then drive the additive device downward through the displacement device until the cone 51 at the end of the stirring tool 5 is inserted into the welding gap of the plate 10 to be welded, wherein the needle tip of the cone 51 is flush with the bottom of the plate 10 to be welded, and the distance between the outer shoulder 2 and the plate 10 to be welded is controlled within the range of 1mm to 3mm; after the additive device reaches the working position, based on Depending on the material of the plate 10 to be welded, during actual welding, it may be necessary to use an alloy material mixed with multiple additive raw materials or to continuously adjust the material ratio of the solder to achieve special welding requirements. At this time, the amount of additive raw materials input into the stirring chamber 3 by different feed pipes 6 can be adjusted according to demand. After the additive raw materials are fully mixed and stirred in the stirring chamber 3 and fully rubbed and plasticized with the plate 10 to be welded, the equipment is started, and the displacement device drives the additive device to move along a pre-planned welding path, thereby achieving welding and forming a weld with excess height on the surface of the gap to be welded. The excess height has a certain heat preservation and slow cooling effect, which is very effective in refining the grains and reducing welding stress. It is also a collection area for impurities such as pores, which can improve the welding quality. After welding is completed, the tail end of the weld needs to be polished.

[0074] like Figure 7 and Figure 8 As shown, the present invention also provides a defect repair method, using the above-mentioned additive device, comprising the following steps:

[0075] C1. Start the spindle 1, which drives the stirring tool 5 to rotate at a set speed in the stirring chamber 3 through the tool handle 4, and move the position of the material adding device so that the cone 51 at the end of the stirring tool 5 moves to the working position, and then the cone 51 is inserted downward into the defect of the plate to be repaired and stays at the defect for a preset time;

[0076] C2, starting the equipment to move the material adding device along the defect track, and at the same time delivering the repairing raw material of the same material as the plate 11 to be repaired into the stirring chamber 3 through the feeding pipe 6 to complete the repair of the defect;

[0077] C3. When the welding track reaches the final point, keep the spindle rotating and feeding, lift it to the second preset height at a certain speed, and move it to the second preset length in the opposite direction. After the end, lift it to the second preset height at a certain speed again, and move it along the original track for the second preset length.

[0078] C4. Repeat step C3 until the bottom of the stirring needle is higher than the weld surface;

[0079] C5. Stop feeding the solder, stop the spindle from rotating, and lift the additive device to reset to its initial position.

[0080] Among them, the second preset height is 0.5mm to 1mm, and the second preset length is 5mm to 10mm. When the defects on the plate need to be repaired, the additive device is first moved to the top of the plate 11 to be repaired by the displacement device, and the position of the additive device is adjusted, and then the main shaft 1 is started to rotate the stirring tool 5 at a preset speed, and then the additive device is driven to move downward, so that the main body of the end of the stirring tool 5 is inserted into the defect to be repaired, and stays for at least 3 seconds, so that the cone 51 can form a molten pool on the plate to be repaired, and then the equipment is started, the stirring tool 5 moves along the extension direction of the preset defect, and at the same time, the same additive raw material as the plate 11 to be repaired is fed into the stirring chamber 3 through the feed pipe 6 to repair the defect. After the defect repair is completed, the tail end of the weld needs to be polished. It should be understood that the plate 11 to be repaired is often made of alloy material, so different additive raw materials can be prepared according to the actual composition of the plate 11 to be repaired, so that the composition of the mixed additive raw materials is consistent with the composition of the plate 11 to be repaired, so as to improve the repair effect.

[0081] In summary, the present invention can transport different additive raw materials into the stirring chamber 3 through multiple feed pipes 6, and control the amount of different additive raw materials input into the stirring chamber 3 through the feed control devices 7 on different feed pipes 6, thereby adjusting the ratio of the mixed additive raw materials to meet different additive requirements.

[0082] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. An additive device, characterized in that: It comprises a coaxially arranged main shaft and an outer shoulder, the outer shoulder is fixedly connected to the main shaft and forms a stirring chamber, a coaxially fixedly connected knife handle and a stirring tool are arranged in the stirring chamber, one end of the knife handle away from the stirring tool is coaxially fixedly connected to the main shaft, and the stirring chamber is provided with a discharge opening on a side close to the stirring tool; The outer shoulder is connected to a plurality of feed pipes, each of which is provided with a feed control device. The feed pipe is connected to the stirring chamber to input additive raw materials into the stirring chamber, and the plurality of feed control devices are used to control the ratio of the additive raw materials input into the stirring chamber.

2. The additive device according to claim 1, characterized in that: The feed control device comprises a first control valve and a second control valve which are arranged on the feed pipeline, a silo is formed between the first control valve and the second control valve, and a weight sensor is arranged in the silo.

3. The additive device according to claim 1, characterized in that: It also includes a cooling device, which includes a cooling bin sleeved on the outer wall of the outer shaft shoulder, the cooling bin is connected to a water inlet pipeline and a water outlet pipeline, a temperature sensor is provided at the water outlet end of the cooling bin, and a flow rate controller is provided at the water inlet end of the cooling bin.

4. The additive device according to claim 1, characterized in that: The end surface of the stirring tool away from the handle is flush with the end surface of the outer shoulder away from the main body.

5. The additive device according to claim 1, characterized in that: The outer wall of the stirring tool is provided with a thread, the pitch of the thread is 3mm to 10mm, and the difference between the inner diameter and the outer diameter of the thread is 4mm to 10mm; the end of the stirring tool away from the tool handle is provided with a cone, and the cone is used to be inserted into the substrate to be added.

6. The additive device according to claim 1, characterized in that: The stirring tool is made of tool steel or nickel-based alloy or tungsten-rhenium alloy.

7. The additive device according to claim 1, characterized in that: The additive raw material is a granular material, a powder material, a chip material, or any combination of granular material, powder material, and chip material.

8. An additive method, characterized in that: The additive device according to any one of claims 1 to 5 comprises the following steps: A1. Start the spindle, which drives the stirring tool to rotate at a set speed in the stirring chamber through the tool handle, and move the position of the additive device so that the cone at the end of the stirring tool moves to the working position, and then the cone is inserted downward into the substrate, while keeping the distance between the lower end surface of the outer shoulder and the substrate within a first preset range; A2. According to the preset material ratio, different additive raw materials of different amounts are simultaneously delivered to the stirring chamber through the feed pipe. After the additive raw materials in the stirring chamber are evenly mixed and fully rubbed and plasticized by the substrate, the equipment is started to move the entire additive device along the planned path to achieve preliminary additive; A3. When the previous layer of material addition is completed, the material addition device is lifted to the starting working position of the next layer, and then step A2 is repeated to achieve multi-layer material addition; A4. When the additive process is completed, the delivery of the additive raw material is stopped, the spindle stops rotating, and the additive device is lifted and reset to the initial position.

9. A welding method, characterized in that: The additive device according to any one of claims 1 to 5 comprises the following steps: B1. Start the spindle, which drives the stirring tool to rotate at a set speed in the stirring chamber through the tool handle, and move the position of the additive device so that the cone at the end of the stirring tool moves to the working position, and then the cone is inserted downward between the two plates to be welded, so that the tip of the cone is flush with the bottom of the plates to be welded, and at the same time, the distance between the lower end surface of the outer shoulder and the plates to be welded is kept in the second preset range; B2. The solder is transported into the stirring chamber through the feed pipe. After the solder in the stirring chamber and the plate to be welded are fully rubbed and plasticized, the equipment is started to move the entire additive device along the planned path to achieve welding and form a weld with excess height at the welding point; B3. When the welding track reaches the final point, keep the spindle rotating and feeding, lift the welding rod to the first preset height at a certain speed, and move the welding rod to the first preset length in the opposite direction. After the welding is finished, lift the welding rod to the first preset height at a certain speed again, and move the welding rod to the first preset length along the original track. B4. Repeat step B3 until the bottom of the stirring needle is higher than the weld surface; B5. Stop feeding the solder, stop the spindle from rotating, and lift the additive device to reset to its initial position.

10. A defect repair method, characterized in that: The additive device according to any one of claims 1 to 5 comprises the following steps: C1. Start the spindle, which drives the stirring tool to rotate at a set speed in the stirring chamber through the tool handle, and move the position of the additive device so that the cone at the end of the stirring tool moves to the working position, and then the cone is inserted downward into the defect of the plate to be repaired and stays at the defect for a preset time; C2. Start the equipment to move the additive device along the defect track, and at the same time, deliver the repairing raw material of the same material as the plate to be repaired into the stirring chamber through the feed pipe to complete the repair of the defect; C3. When the welding track reaches the final point, keep the spindle rotating and feeding, lift it to the second preset height at a certain speed, and move it to the second preset length in the opposite direction. After the end, lift it to the second preset height at a certain speed again, and move it along the original track for the second preset length. C4. Repeat step C3 until the bottom of the stirring needle is higher than the weld surface; C5. Stop feeding the solder, stop the spindle from rotating, and lift the additive device to reset to its initial position.

Citation Information

Cited By

  • Wire stirring friction additive and subtractive integrated device and method

    CN120170471A

  • Friction stir deposition additive process capable of adaptively regulating and controlling forming stress

    CN120587635A

  • Friction stir repair process for shallow cracks of arc-shaped component

    CN120680109A