Method for removing thallium in high-salinity brine generated in process of extracting lithium from lepidolite ore
By controlling the pH value and using specific thallium remover and flocculant, the adaptability and efficiency of thallium removal in high-salt brine during lithium mica extraction is solved, and the effect of efficient thallium removal is achieved. It is suitable for lithium mica process flow wastewater treatment.
Patent Information
- Application Number
- CN202411337647.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology of removing thallium in high-salt brine produced during lithium mica ore extraction is not suitable for the traditional method. The processing time is long, the cost is high or the equipment investment is large, and it is not suitable for the specific wastewater characteristics in the lithium mica process flow.
By controlling the pH value during the reaction, the heavy metal impurity thallium is separated by using the thallium remover YHHB-DeT1-CT, the coagulant YHHB-DeT1-ZN and the flocculant polyacrylamide.
The content of thallium in high-salt brine was efficiently removed, reducing it from 877.29 to 714.83μg/L to 11.55 to 20.32μg/L, and the thallium removal efficiency reached 97.2 to 98.68%. It is suitable for wastewater treatment in the lithium mica mine extraction process.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for removing thallium from high-salinity brine produced in a lithium extraction process of lepidolite ore. Background Art
[0002] Thallium is a highly toxic heavy metal element that is toxic to the liver, kidneys and nerves. It can be enriched in aquatic organisms through enrichment in the ecological chain and eventually accumulate in the human body. In the process of preparing lithium carbonate using lithium mica, the trace element thallium contained in the lithium mica will enter the mother liquor and wastewater during the roasting and leaching process steps. The thallium in lithium mica exists in the form of monovalent thallium. During roasting, a part of it is carried out with the flue gas and eventually enters the desulfurization wastewater through the desulfurization process; during leaching, thallium enters the mother liquor and enters the subsequent drainage.
[0003] The methods for removing thallium from wastewater generally include oxidation, sulfidation, adsorption, and electrocoagulation. Oxidation and sulfidation are suitable for wastewater with a high initial thallium concentration. The treatment time is moderate and requires subsequent flocculation and treatment of hazardous waste. The adsorption method takes a long time to treat and requires frequent regeneration of the adsorption material. Electrocoagulation has a high degree of automation, but the equipment investment cost is relatively high.
[0004] Traditional methods of removing thallium from wastewater are mainly aimed at the steel industry, lead and zinc industry, etc., and are not fully suitable for the wastewater generated in the lithium extraction process of lepidolite. The wastewater generated in the lithium extraction process of lepidolite mainly comes from the desulfurization wastewater of roasting flue gas, the total discharged wastewater after leaching and precipitation of lithium, and initial rainwater. The pH and heavy metal ion concentration range of the wastewater generated in the lithium extraction process of lepidolite are different from those of the traditional steel industry, lead and zinc industry, etc. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for removing thallium from high-salinity brine produced in the process of extracting lithium from lepidolite ore in view of the above-mentioned deficiencies in the prior art. The method can achieve the purpose of removing thallium, a heavy metal impurity, from the high-salinity brine by controlling the pH value in the reaction process, using a thallium removal agent YHHB-DeT1-CT, a coagulant aid YHHB-DeT1-ZN and a flocculant polyacrylamide.
[0006] In order to solve the above technical problems, the present invention provides a method for removing thallium from high-salinity brine produced in the process of extracting lithium from lepidolite ore, comprising the following steps:
[0007] S1, take the brine produced in the process of roasting and leaching lithium extraction of lithium mica ore and put it into a reaction tank 1, add sodium hydroxide solution and thallium removal agent while stirring, adjust the pH value, and after sufficient stirring, obtain a mixed solution 1;
[0008] S2, sequentially adding the mixed solution 1 prepared in S1 and the coagulant aid into the reaction tank 2, fully reacting and adjusting the pH value in the reaction tank 2 to obtain reacted brine;
[0009] S3, adding polyacrylamide to water to obtain a flocculant solution, starting a deep cone thickener, and then adding the reacted brine and flocculant solution prepared in S2 to the deep cone thickener to separate the slag liquid to obtain a supernatant 1 and an underflow 1;
[0010] S4, the supernatant 1 prepared in S3 is transferred into an inclined tube sedimentation tank, and after sedimentation, a supernatant 2 and an underflow 2 are obtained, wherein the supernatant 2 obtained is the lithium sulfate solution after thallium is removed, and the underflow 2 obtained is returned to S3 for further separation.
[0011] According to the method for removing thallium from high-salinity brine produced in the process of extracting lithium from lepidolite ore provided by the present invention, the volume ratio of the brine, the sodium hydroxide solution and the thallium removal agent in S1 is 1L:1-3mL:2-3mL, the mass fraction of the sodium hydroxide solution is 30-35%, and the thallium removal agent is YHHB-DeT1-CT.
[0012] According to the method for removing thallium from high-salinity brine produced in the process of extracting lithium from lepidolite ore provided by the present invention, the stirring speed in S1 is 80-70 rpm / min, the pH value is adjusted to 9-11, and the sufficient stirring time is 15-20 min.
[0013] According to the method for removing thallium from high-salt brine produced in the process of extracting lithium from lepidolite ore provided by the present invention, the coagulant in S2 is YHHB-DeT1-ZN, the volume ratio of the mixed solution 1 and the coagulant is 1000:1-2, the time for sufficient reaction is 25-30 minutes, and the pH value is 8-10.
[0014] According to the method for removing thallium from high-salt brine produced in the process of extracting lithium from lepidolite ore provided by the present invention, the volume ratio of polyacrylamide and water in S3 is 1000:1-3, the rotation speed of the deep cone thickener is 40-45 rpm / min, and the volume ratio of the brine after the reaction to the flocculant solution is 1000:0.3-1.
[0015] According to the method for removing thallium from high-salt brine produced in the process of extracting lithium from lepidolite ore provided by the present invention, the underflow 1 in S3 is moved into a membrane filter press for filtration to obtain filter residue and filtrate, the filter residue enters a ton bag through a slag discharge hopper and is transported to a hazardous waste warehouse for centralized treatment, and the filtrate is merged into the liquid after thallium removal.
[0016] According to the method for removing thallium from high-salinity brine produced in the process of extracting lithium from lepidolite ore provided by the present invention, the sedimentation time in S4 is 30 to 60 minutes.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] The invention provides a method for removing thallium from high-salinity brine generated in a lithium extraction process of lepidolite ore. The method achieves the purpose of removing thallium, a heavy metal impurity in the high-salinity brine, by controlling the pH value in the reaction process and adding a thallium removal agent YHHB-DeT1-CT, a coagulant aid YHHB-DeT1-ZN and a flocculant polyacrylamide. The method can reduce the thallium content in the high-salinity brine from 877.29 to 714.83 μg / L to 11.55 to 20.32 μg / L, and the thallium removal efficiency reaches 97.2 to 98.68%. DETAILED DESCRIPTION
[0019] Example 1
[0020] The origin of the lithium mica ore in this embodiment is Yifeng County, Yichun City, Jiangxi Province.
[0021] This embodiment provides a method for removing thallium from high-salinity brine produced during lithium extraction from lepidolite ore, comprising the following steps:
[0022] S1, take 1L of brine produced during the roasting, leaching and lithium extraction of lithium mica ore into a reaction tank 1, stir at a speed of 80rpm / min, then add 3mL of a 30% sodium hydroxide solution and 3mL of a thallium removal agent YHHB-DeT1-CT, adjust the pH value to 11, and stir for 20min to obtain a mixed solution 1;
[0023] S2, adding the mixed solution 1 prepared in S1 and the coagulant aid YHHB-DeT1-ZN into the reaction tank 2 in a volume ratio of 1000:2, reacting for 30 minutes, adjusting the pH value in the reaction tank 2 to 10, and obtaining the reacted brine;
[0024] S3, adding flocculant polyacrylamide into water at a volume ratio of 1000:3 to obtain a flocculant solution, starting a deep cone thickener, adjusting its speed to 45 rpm / min, and then adding the reacted brine and flocculant solution prepared in S2 into the deep cone thickener at a volume ratio of 1000:1 to separate the residue liquid to obtain supernatant 1 and underflow 1, transferring the underflow 1 into a membrane filter press for filtration to obtain filter residue and filtrate, and the filter residue enters a ton bag through a slag unloading hopper and is transported to a hazardous waste warehouse for centralized treatment;
[0025] S4, the supernatant 1 prepared in S3 is transferred into an inclined tube sedimentation tank, and after sedimentation for 60 minutes, a supernatant 2 and an underflow 2 are obtained, wherein the supernatant 2 obtained is the lithium sulfate solution after thallium is removed, and the underflow 2 obtained is returned to S3 for further sedimentation and separation.
[0026] The thallium content in the raw brine selected in S1 of this embodiment was detected, and the thallium content in the brine was 877.29 μg / L. The thallium content in the supernatant 2 prepared in S4 was detected, and the thallium content in the supernatant 2 was 11.55 μg / L. The thallium removal efficiency was 98.68%.
[0027] Under alkaline conditions, the thallium remover utilizes its own powerful thiol groups and thallium to generate a hydrophobic colloid, which carries a negative charge. With the help of a coagulant, the colloid is effectively precipitated and separated from the water following the precipitation. The method provided in this embodiment combines the dual effects of thiol recapture and colloidal physical charge coagulation to achieve the removal of thallium.
[0028] Example 2
[0029] This embodiment provides a method for removing thallium from high-salinity brine produced during lithium extraction from lepidolite ore, comprising the following steps:
[0030] S1, take 1L of brine produced during the roasting, leaching and lithium extraction of lithium mica ore into a reaction tank 1, stir at a speed of 75rpm / min, then add 2mL of a 32% sodium hydroxide solution and 3mL of a thallium removal agent YHHB-DeT1-CT, adjust the pH value to 10, and stir for 20min to obtain a mixed solution 1;
[0031] S2, adding the mixed solution 1 prepared in S1 and the coagulant YHHB-DeT1-ZN into the reaction tank 2 in a volume ratio of 1000:1.5, reacting for 28 minutes, adjusting the pH value in the reaction tank 2 to 9 to obtain the reacted brine;
[0032] S3, adding polyacrylamide as a flocculant to water at a volume ratio of 1000:2 to obtain a flocculant solution, starting a deep cone thickener, adjusting its speed to 40 rpm / min, and then adding the brine and flocculant solution after the reaction prepared in S2 to the deep cone thickener at a volume ratio of 1000:0.8 to separate the residue liquid, obtaining a supernatant 1 and an underflow 1, transferring the underflow 1 to a membrane filter press for filtration to obtain a filter residue and a filtrate, and the filter residue is discharged into a ton bag through a slag discharge hopper and transported to a hazardous waste warehouse for centralized treatment;
[0033] S4, the supernatant 1 prepared in S3 is transferred into an inclined tube sedimentation tank, and after sedimentation for 50 minutes, a supernatant 2 and an underflow 2 are obtained, wherein the supernatant 2 obtained is the lithium sulfate solution after thallium is removed, and the underflow 2 obtained is returned to S3 for further sedimentation and separation.
[0034] The thallium content in the raw brine selected in S1 of this embodiment was detected, and the thallium content in the brine was 714.83 μg / L. The thallium content in the supernatant 2 prepared in S4 was detected, and the thallium content in the supernatant 2 was 20.32 μg / L. The thallium removal efficiency was 97.3%.
[0035] Example 3
[0036] This embodiment provides a method for removing thallium from high-salinity brine produced during lithium extraction from lepidolite ore, comprising the following steps:
[0037] S1, take 1L of brine produced during the roasting, leaching and lithium extraction of lithium mica ore into a reaction tank 1, stir at a speed of 70rpm / min, then add 1mL of a 31% sodium hydroxide solution and 2mL of a thallium removal agent YHHB-DeT1-CT, adjust the pH value to 9, and stir for 15min to obtain a mixed solution 1;
[0038] S2, adding the mixed solution 1 prepared in S1 and the coagulant YHHB-DeT1-ZN into the reaction tank 2 in a volume ratio of 1000:1, reacting for 25 minutes, and adjusting the pH value in the reaction tank 2 to 8 to obtain the reacted brine;
[0039] S3, adding flocculant polyacrylamide into water at a volume ratio of 1000:1 to obtain a flocculant solution, starting the deep cone thickener, adjusting its speed to 42rpm / min, and then adding the brine and flocculant solution prepared in S2 to the deep cone thickener at a volume ratio of 1000:0.3 to separate the residue liquid, obtaining supernatant 1 and underflow 1, transferring the underflow 1 into a membrane filter press for filtration to obtain filter residue and filtrate, and the filter residue enters a ton bag through a slag unloading hopper and is transported to a hazardous waste warehouse for centralized treatment;
[0040] S4, the supernatant 1 prepared in S3 is transferred into an inclined tube sedimentation tank, and after sedimentation for 30 minutes, a supernatant 2 and an underflow 2 are obtained, wherein the supernatant 2 obtained is the lithium carbonate solution after thallium is removed, and the underflow 2 obtained is returned to S3 for further sedimentation and separation.
[0041] The thallium content in the raw brine selected in S1 of this embodiment was detected, and the thallium content in the brine was 784.5 μg / L. The thallium content in the supernatant 2 prepared in S4 was detected, and the thallium content in the supernatant 2 was 12.31 μg / L. The thallium removal efficiency was 98.43%.
[0042] Example 4
[0043] This embodiment provides a method for removing thallium from high-salinity brine produced during lithium extraction from lepidolite ore, comprising the following steps:
[0044] S1, take 1L of brine produced during the roasting, leaching and lithium extraction of lithium mica ore into a reaction tank 1, stir at a speed of 80rpm / min, then add 2mL of a 35% sodium hydroxide solution and 2.5mL of a thallium removal agent YHHB-DeT1-CT, adjust the pH value to 10, and stir for 20min to obtain a mixed solution 1;
[0045] S2, adding the mixed solution 1 prepared in S1 and the coagulant YHHB-DeT1-ZN into the reaction tank 2 in a volume ratio of 1000:2, reacting for 28 minutes, and adjusting the pH value in the reaction tank 2 to 9 to obtain the reacted brine;
[0046] S3, adding flocculant polyacrylamide into water at a volume ratio of 1000:2 to obtain a flocculant solution, starting the deep cone thickener, adjusting its speed to 40rpm / min, and then adding the brine and flocculant solution prepared in S2 to the deep cone thickener at a volume ratio of 1000:0.9 to separate the residue liquid to obtain supernatant 1 and underflow 1, transferring the underflow 1 into a membrane filter press for filtration to obtain filter residue and filtrate, and the filter residue enters a ton bag through a slag unloading hopper and is transported to a hazardous waste warehouse for centralized treatment;
[0047] S4, the supernatant 1 prepared in S3 is transferred into an inclined tube sedimentation tank, and after sedimentation for 40 minutes, a supernatant 2 and an underflow 2 are obtained, wherein the supernatant 2 obtained is the lithium sulfate solution after thallium is removed, and the underflow 2 obtained is returned to S3 for further sedimentation and separation.
[0048] The thallium content in the raw brine selected in S1 of this embodiment was detected, and the thallium content in the brine was 835.12 μg / L. The thallium content in the supernatant 2 prepared in S4 was detected, and the thallium content in the supernatant 2 was 16.43 μg / L. The thallium removal efficiency was 98.03%.
[0049] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for removing thallium from high-salinity brine produced during lithium extraction from lepidolite ore, characterized in that: The following steps are involved: S1, take the brine produced in the process of roasting and leaching lithium extraction of lithium mica ore and put it into a reaction tank 1, add sodium hydroxide solution and thallium removal agent while stirring, adjust the pH value, and after sufficient stirring, obtain a mixed solution 1; S2, sequentially adding the mixed solution 1 prepared in S1 and the coagulant aid into the reaction tank 2, fully reacting and adjusting the pH value in the reaction tank 2 to obtain reacted brine; S3, adding polyacrylamide to water to obtain a flocculant solution, starting a deep cone thickener, and then adding the reacted brine and flocculant solution prepared in S2 to the deep cone thickener to separate the slag liquid to obtain a supernatant 1 and an underflow 1; S4, the supernatant 1 prepared in S3 is transferred into an inclined tube sedimentation tank, and after sedimentation, a supernatant 2 and an underflow 2 are obtained, wherein the supernatant 2 obtained is the lithium sulfate solution after thallium is removed, and the underflow 2 obtained is returned to S3 for further separation.
2. The method for removing thallium from the high-salinity brine produced in the lithium extraction process of lepidolite ore according to claim 1, characterized in that: The volume ratio of the brine, the sodium hydroxide solution and the thallium removal agent in S1 is 1L: 1-3mL: 2-3mL, the mass fraction of the sodium hydroxide solution is 30-35%, and the thallium removal agent is YHHB-DeT1-CT.
3. The method for removing thallium from the high-salinity brine produced in the lithium extraction process of lepidolite ore according to claim 1, characterized in that: The stirring speed in S1 is 80-70 rpm / min, the pH value is adjusted to 9-11, and the sufficient stirring time is 15-20 min.
4. The method for removing thallium from the high-salinity brine produced in the lithium extraction process of lepidolite ore according to claim 1, characterized in that: The coagulant in S2 is YHHB-DeT1-ZN, the volume ratio of the mixed solution 1 to the coagulant is 1000:1-2, the time for sufficient reaction is 25-30 minutes, and the pH value is 8-10.
5. The method for removing thallium from the high-salinity brine produced in the lithium extraction process of lepidolite ore according to claim 1, characterized in that: The volume ratio of polyacrylamide and water in S3 is 1000:1-3, the rotation speed of the deep cone thickener is 40-45 rpm / min, and the volume ratio of the brine after the reaction and the flocculant solution is 1000:0.3-1.
6. The method for removing thallium from the high-salinity brine produced in the lithium extraction process of lepidolite ore according to claim 1, characterized in that: The underflow 1 in S3 is transferred to a membrane filter press for filtration to obtain filter residue and filtrate. The filter residue enters a ton bag through a slag discharge hopper and is transported to a hazardous waste warehouse for centralized treatment. The filtrate is merged into the thallium-removed liquid.
7. The method for removing thallium from the high-salinity brine produced in the lithium extraction process of lepidolite ore according to claim 1, characterized in that: The sedimentation time described in S4 is 30 to 60 minutes.
Citation Information
Patent Citations
Thallium-containing heavy metal wastewater advanced treatment method
CN103693819A
Thallium removing method for thallium-containing sintering flue gas desulfurization waste water
CN106517587A
Thallium removal process for lead-zinc smelting wastewater
CN115947436A
Thallium removal composition and treatment method of thallium-containing wastewater
CN117209036A
Method for removing thallium ions in mica lithium extraction wastewater
CN117945580A