Method for preparing copper tailing silicon fertilizer by utilizing high-energy ball milling and low-temperature calcining technology

Through high-energy ball mill collaborative low-temperature calcination technology, the problem of difficult use of fine-grain tailings in copper tailings is solved, and the preparation of high-efficiency silicon fertilizer is realized, which reduces the calcination temperature and energy consumption, increases the effective silicon content of silicon fertilizer, and simplifies the The process meets agricultural standards and reduces environmental protection pressure.

CN119080565APending Publication Date: 2024-12-06JIANGXI COPPER TECHNOLOGY RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411203562.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing technology, the efficient utilization of copper tailings is scarce, resulting in low overall resource utilization and limited product added value. Especially in the traditional building materials production process, fine-grain tailings are difficult to directly utilize, and in the existing silicon fertilizer production process. The high calcination temperature or complex process increases costs.

Method used

Using high-energy ball mill collaborative low-temperature calcination technology, copper tailings are mixed with calcium-containing activators and alkaline fluxes, and staged high-energy ball mills and low-temperature calcination to reduce the calcination temperature, increase the activation degree of silica, and prepare high-efficiency silicon fertilizers .

Benefits of technology

It realizes efficient activation of fine-grain copper tailings, reduces calcination temperature, increases the effective silicon content of silicon fertilizers, simplifies the process, reduces energy consumption, meets agricultural standards, and reduces the environmental protection brought by tailings accumulation. pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080565A_ABST
    Figure CN119080565A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of comprehensive utilization of resources, and particularly relates to a method for preparing a silicon fertilizer by treating copper tailings through a high-energy ball milling and low-temperature calcination technology. Mixing the silicon powder with a calcium-containing activating agent and an alkaline fluxing agent, performing high-energy ball milling pretreatment to obtain a mixed material, and calcining and grinding the mixed material to obtain the silicon fertilizer. The low-temperature preparation of the copper tailing silicon fertilizer is realized by utilizing a high-energy ball milling and low-temperature calcining technology, the calcining temperature for preparing the silicon fertilizer from the flotation tailings is obviously reduced, no alkaline wastewater is generated in the production process, and the production process is simple. In addition, by means of efficient resource utilization of the fine-fraction copper tailings, the problem of recycling of the superfine-particle-size tailings is solved, and the environmental pressure caused by discharging of the superfine-particle-size tailings is greatly reduced. The content of effective silicon in the prepared silicon fertilizer is higher than 20%, and the silicon fertilizer can be used as a fertilizer to provide nutrients and improve the soil structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of comprehensive resource utilization, and specifically relates to a method for preparing copper tailings silicon fertilizer by utilizing high-energy ball milling and low-temperature calcination technology. Background Art

[0002] Due to the large volume of the building materials field, the utilization of copper tailings as building materials has become the main way to dispose of tailings on a large scale. However, the mineral composition of copper mines in my country is complex, and dehydration-classification treatment is a necessary measure for the large-scale utilization of copper tailings as building materials. However, the resulting fine-grained tailings with small particle size and large specific surface area are often difficult to be directly used in the traditional building materials production process, and there are very few efficient ways to utilize them, resulting in low overall resource utilization and limited product added value.

[0003] Silicon, as the fourth largest plant nutrient element after nitrogen, phosphorus and potassium, is an important component of plant growth. As a new type of fertilizer, silicon fertilizer can not only provide nutrients for crops and enhance their photosynthesis, which has a significant effect on increasing crop yields, but also can regulate and improve soil structure, passivate heavy metals in the soil, and play a positive role in improving crop quality. Domestically produced silicon fertilizers are mainly divided into two categories: synthetic silicon fertilizers and industrial waste recycled silicon fertilizers. Synthetic silicon fertilizers are mainly high-efficiency silicon fertilizers with sodium silicate and sodium metasilicate as the main components. They are expensive and difficult to promote. Industrial waste recycled silicon fertilizers generally use high-temperature calcination or hydrothermal treatment of silicon-containing solid waste to activate silicon.

[0004] In terms of the chemical composition of raw materials, the chemical composition of copper tailings is mainly SiO2, and contains a variety of essential elements for plants such as K, Ca, Mg, etc., and the use of copper tailings to produce silicon fertilizer has significant advantages. There are related technologies for using tailings to produce silicon fertilizer in the prior art, such as patent application number 201711061548.7 "A method for recovering molybdenum and sulfur from molybdenum tailings and using them as raw materials to prepare molybdenum silicon fertilizer", and patent application number 202210173277.9 "A process for making high-quality and efficient silicon fertilizer using copper tailings", but the calcination activation temperature of the tailings in the above technologies is generally higher than 1100℃; although the patent application number 201711061548.7 "A method for preparing slow-release silicon fertilizer" realizes the low-temperature preparation of silicon fertilizer from phosphorus tailings, its complex process and high-proportion chemical raw materials increase the production cost of silicon fertilizer. Summary of the invention

[0005] The invention discloses a method for preparing copper tailings silicon fertilizer by utilizing high-energy ball milling in coordination with low-temperature calcination technology, so as to solve any of the above and other potential problems in the prior art.

[0006] To achieve the above object, the technical solution of the present invention is: a method for preparing silicon fertilizer by using high-energy ball milling and low-temperature calcination technology, the method specifically comprising the following steps:

[0007] S1) firstly mix the fine-grained copper tailings after classification with a calcium-containing activator and an alkaline flux in a certain ratio to obtain a mixed material;

[0008] S2) The mixed material obtained in S1) is subjected to high-energy ball milling pretreatment, and then subjected to low-temperature calcination and powder grinding treatment to obtain silicon fertilizer.

[0009] Furthermore, the fine-grained copper tailings are fine mud byproducts obtained after the copper tailings are subjected to cyclone classification treatment.

[0010] Furthermore, the mass ratio of the fine-grained copper tailings, the calcium-containing activator and the alkaline flux in S1) is 1:(0.5-1.5):(0.1-0.5).

[0011] Further, the calcium-containing activator is one or more of calcium oxide, calcium hydroxide, calcium carbonate, and calcium peroxide;

[0012] The alkaline flux is one or more of sodium hydroxide, sodium carbonate and potassium carbonate.

[0013] Further, the specific process of the high-energy ball milling pretreatment process in S2) is:

[0014] The mixed material obtained in S1) is placed in a ball mill, the ball-to-material ratio is controlled to be 2:1-4:1, the ratio of large, medium and small zirconia grinding balls is 3:4:3, and high-energy ball milling is performed in stages to obtain a specific surface area of ​​1200-1500m 2 / kg of material.

[0015] Furthermore, the staged high-energy ball milling is specifically as follows: in the first stage, ball milling is performed at a rotation speed of 200 to 400 rpm for 1 to 20 minutes; in the second stage, ball milling is performed at a rotation speed of 400 to 750 rpm for 10 to 60 minutes.

[0016] Furthermore, the specific process of low-temperature calcination is: calcining at a temperature of 700-900° C. for 10-60 minutes.

[0017] Furthermore, the particle size of the ground silicon fertilizer in S2) is 180 mesh.

[0018] Furthermore, the ball mill is a planetary mill, a vibrating ball mill or a stirring ball mill.

[0019] A silicon fertilizer is prepared by the above method.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention utilizes high-energy ball milling pretreatment to effectively reduce the calcination process temperature of tailings for preparing silicon fertilizer, and obtains silicon fertilizer with an effective silicon content of 20-30%, which can not only provide nutrients for crops, but also improve soil acidification, fix heavy metals in the soil, and reduce their impact on crops.

[0022] (2) The present invention utilizes the characteristic that sericite in fine-grained copper tailings is susceptible to mechanical chemical action, and pre-treats the fine-grained copper tailings with a calcium-containing activator and an alkaline flux through high-energy ball milling to promote the refinement of the fine-grained copper tailings grains, and the specific surface area thereof can reach 1200 to 1500 m 2 / kg, maximizing the activation of silica in the tailings.

[0023] (3) The present invention provides a high-value utilization method for ultra-fine tailings, that is, fully utilizing the elements Si, Ca, K, Mg and the like in copper tailings, and achieving the purpose of efficiently absorbing ultra-fine tailings, thereby alleviating the environmental pressure caused by tailings accumulation. In addition, the production process is simple, and no alkaline wastewater is generated, thus solving the problem of high cost and high energy consumption in the process of producing silicon fertilizer from tailings. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a schematic diagram of the process flow of the method for preparing copper tailings silicon fertilizer by using high-energy ball milling and low-temperature calcination technology.

[0025] Figure 2 This is the SEM image of the silicon fertilizer prepared in Example 2. DETAILED DESCRIPTION

[0026] The present invention is further described below, but the following detailed description is not to be construed as limiting the present invention.

[0027] like Figure 1 As shown, the present invention provides a method for preparing silicon fertilizer by using high-energy ball milling and low-temperature calcination technology, and the method specifically comprises the following steps:

[0028] S1) firstly mix the fine-grained copper tailings after classification with a calcium-containing activator and an alkaline flux in a certain ratio to obtain a mixed material;

[0029] S2) The mixed material obtained in S1) is subjected to high-energy ball milling pretreatment, and then subjected to low-temperature calcination and powder grinding treatment to obtain silicon fertilizer.

[0030] The fine-grained copper tailings are fine mud byproducts obtained after the copper tailings are subjected to cyclone classification treatment.

[0031] The mass ratio of the fine-grained copper tailings, the calcium-containing activator and the alkaline flux in S1) is 1: (0.5-1.5): (0.1-0.5).

[0032] The calcium-containing activator is one or more of calcium oxide, calcium hydroxide, calcium carbonate and calcium peroxide;

[0033] The alkaline flux is one or more of sodium hydroxide, sodium carbonate and potassium carbonate.

[0034] The specific process of the high-energy ball milling pretreatment process in S2) is:

[0035] The mixed material obtained in S1) is placed in a ball mill, the ball-to-material ratio is controlled to be 2:1-4:1, the ratio of large, medium and small zirconia grinding balls is 3:4:3, and high-energy ball milling is performed in stages to obtain a specific surface area of ​​1200-1500m 2 / kg of material.

[0036] The staged high-energy ball milling is specifically as follows: in the first stage, the ball milling is performed at a rotation speed of 200 to 400 rpm for 1 to 20 minutes; in the second stage, the ball milling is performed at a rotation speed of 400 to 750 rpm for 10 to 60 minutes.

[0037] The specific process of low temperature calcination is: calcining at a temperature of 700-900° C. for 10-60 minutes.

[0038] The particle size of the silicon fertilizer after grinding in S2) is 180 mesh.

[0039] The ball mill is a planetary mill, a vibrating ball mill or a stirring ball mill.

[0040] A silicon fertilizer is prepared by the above method.

[0041] The fine-grained copper tailings described in the following examples and comparative examples are all obtained by cyclone classification from tailings produced by a copper mine in Jiangxi, China.

[0042] Embodiment 1:

[0043] Fine-grained copper tailings, calcium-containing activator and alkaline flux were mixed in a ratio of 1:0.45:0.25 and placed in a ball mill. The ball-to-material ratio was controlled to be 2:1-4:1, and the ratio of large, medium and small zirconia grinding balls was 3:4:3. First, the ball mill speed was adjusted to 250 rpm and ground for 10 minutes, then the ball mill speed was adjusted to 600 rpm and ground for 20 minutes until the specific surface area of ​​the mixed material was 1152 m 2 / kg is used for discharging, and finally the ground mixed material is calcined at 700℃ for 30 minutes; the calcined sample is ground and passed through a 180-mesh sieve to obtain the silicon fertilizer product.

[0044] After testing, the effective silicon content in the prepared silicon fertilizer is 21.79%.

[0045] Embodiment 2:

[0046] The fine-grained copper tailings, calcium-containing activator and alkaline flux were mixed in a ratio of 1:0.45:0.25 and placed in a ball mill. The ball-to-material ratio was controlled to be 2:1-4:1, and the ratio of large, medium and small zirconia grinding balls was 3:4:3. The ball mill speed was adjusted to 200 rpm, and the grinding was performed for 10 minutes. Then the ball mill speed was adjusted to 750 rpm and the grinding was performed for 20 minutes until the specific surface area of ​​the mixed material was 1362 m 2 / kg is discharged, and finally the ground mixed material is calcined at 700°C for 1 hour; the calcined sample is ground and passed through a 180-mesh sieve to obtain a silicon fertilizer product. The SEM image of the silicon fertilizer is shown in Figure 2 shown.

[0047] After testing, the effective silicon content in the prepared silicon fertilizer is 26.81%.

[0048] From the above results, it can be seen that the low-temperature activation of mineral processing fine mud is achieved by using high-energy ball milling and coordinated calcination technology, and the silicon fertilizer obtained meets the technical indicators of effective silicon content in the agricultural standard "NY / T797-2004 Silicon Fertilizer".

[0049] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.

[0050] The above is a detailed introduction to a method for preparing copper tailings silicon fertilizer using high-energy ball milling and low-temperature calcination technology provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and its core idea of ​​the present application; at the same time, for those of ordinary skill in the art, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

[0051] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.

[0052] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.

[0053] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0054] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.

Claims

1. A method for preparing silicon fertilizer using high-energy ball milling and low-temperature calcination technology, characterized in that: The method specifically comprises the following steps: S1) firstly mix the fine-grained copper tailings after classification with a calcium-containing activator and an alkaline flux in a certain ratio to obtain a mixed material; S2) The mixed material obtained in S1) is subjected to high-energy ball milling pretreatment, and then subjected to low-temperature calcination and powder grinding treatment to obtain silicon fertilizer.

2. The method according to claim 1, characterized in that The fine-grained copper tailings are fine mud byproducts obtained after the copper tailings are subjected to cyclone classification treatment.

3. The method according to claim 1, characterized in that The mass ratio of the fine-grained copper tailings, the calcium-containing activator and the alkaline flux in S1) is 1: (0.5-1.5): (0.1-0.5).

4. The method according to claim 1, characterized in that The calcium-containing activator is one or more of calcium oxide, calcium hydroxide, calcium carbonate and calcium peroxide; The alkaline flux is one or more of sodium hydroxide, sodium carbonate and potassium carbonate.

5. The method according to claim 1, characterized in that The specific process of the high-energy ball milling pretreatment process in S2) is: The mixed material obtained in S1) is placed in a ball mill, the ball-to-material ratio is controlled to be 2:1-4:1, the ratio of large, medium and small zirconia grinding balls is 3:4:3, and high-energy ball milling is performed in stages to obtain a specific surface area of ​​1200-1500m 2 / kg of material.

6. The method according to claim 5, characterized in that The staged high-energy ball milling is specifically as follows: in the first stage, the ball milling is performed at a rotation speed of 200 to 400 rpm for 1 to 20 minutes; in the second stage, the ball milling is performed at a rotation speed of 400 to 750 rpm for 10 to 60 minutes.

7. The method according to claim 1, characterized in that The specific process of low-temperature calcination is: calcining at a temperature of 700-900° C. for 10-60 minutes.

8. The method according to claim 1, characterized in that: The particle size of the silicon fertilizer after grinding in S2) is 180 mesh.

9. The method according to claim 5, characterized in that The ball mill is a planetary mill, a vibrating ball mill or a stirring ball mill.

10. A silicon fertilizer, characterized in that: The silicon fertilizer is prepared by the method according to any one of claims 1 to 9.