Inlaid pouring material for small and special electric machine and pouring process

By using inlaid casting materials and specific processes composed of epoxy resins and other in micro-electric manufacturing, the problem of insufficient thermal deformation temperature in the prior art is solved, efficient curing and aging is achieved, time is shortened and secondary is avoided Demolding step.

CN119081070APending Publication Date: 2024-12-06QINGDAO QINGWEI ELECTRIC APPLIANCE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411233983.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the manufacturing process of micro-type motors, the thermal deformation temperature of the existing epoxy casting process is low, and secondary heating and mold release is required, which affects the performance of the cured substance and extends the curing and aging time.

Method used

Using inlaid casting materials composed of epoxy resin, liquid aromatic amine curing agent, active diluent and polyol glycidyl ether, the casting process without secondary release is achieved through preheating and mold release agent, and the thermal deformation is improved Temperatures are up to 150 degrees Celsius and curing and aging times are shortened by vacuum and heat treatment.

Benefits of technology

Efficient curing and aging without affecting the performance of cured substances in the inlay casting of micro-motors is achieved, which shortens 1/3 of the curing and aging time and avoids the secondary mold release step.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081070A_ABST
    Figure CN119081070A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of pouring methods, in particular to an inlay pouring material for a small and special electric machine and a pouring process, and the inlay pouring material for the small and special electric machine comprises the following components in parts by weight: 100 parts of epoxy resin, 5-20 parts of a liquid aromatic amine curing agent, 20-30 parts of a reactive diluent and 5-10 parts of polyol glycidyl ether. During pouring, all the matching faces of the tool and all the matching faces of the poured part are coated with a release agent, and the tool, the poured part and epoxy resin are preheated; uniformly stirring epoxy resin, a liquid aromatic amine curing agent, a reactive diluent and polyol glycidyl ether which are preheated in advance to prepare a casting material; after the preheating time is up, the cast part and the tool are coated with the release agent again; after the cast part and the tool are assembled together, the procedures of casting, drying, demolding, curing, aging and cooling are carried out, secondary demolding is not needed, the performance of a cast cured product is not affected, and the curing and aging time is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of casting methods, and in particular to an inlay casting material and a casting process for a micro motor. Background Art

[0002] Micro motors, also known as micro special motors, are micro motors with a diameter of less than 160 mm or rated power or with special performance or special purpose. Micro motors are often used in control systems to detect, calculate, amplify, execute or convert electromechanical signals or energy, or to transmit mechanical loads, or as AC or DC power supplies for equipment. Micro motors are essential basic products in various fields such as industrial automation, agricultural modernization, weapon equipment modernization, office automation, and home modernization. They have a wide range of applications and will be further expanded with economic development and technological progress.

[0003] In the manufacturing process of micro motors, the problem of inlaying and fixing micro parts is often faced. Due to the limited volume and space, the inlaying and fixing of parts often faces great challenges. At present, micro parts are inlaid by welding and bonding. This kind of inlay only plays the role of riveting to fix the relative position, and does not play the role of structural support. Structural support still needs to be achieved by epoxy casting.

[0004] However, the existing epoxy casting process for micro motors usually has a heat deformation temperature of only 110°C, requiring secondary heating for demolding, which affects the performance of the cast solid and results in long curing and aging times. Summary of the invention

[0005] The purpose of the present invention is to provide an inlay casting material and casting process for micro motors. When inlay casting is performed on micro motor parts, no secondary demoulding is required, thereby not affecting the performance of the cast solidified material and shortening the curing and aging time.

[0006] To achieve the above objectives, in a first aspect, the present invention provides an inlay casting material for micro motors, which consists of the following components, by weight: 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of active diluent and 5-10 parts of polyol glycidyl ether.

[0007] Wherein, the epoxy resin adopts epoxy resin with brand number 634.

[0008] Wherein, the liquid aromatic amine curing agent adopts a liquid aromatic amine curing agent with a brand of LB701.

[0009] Wherein, the active diluent is an epoxy resin active diluent.

[0010] Wherein, the polyol glycidyl ether adopts the polyol glycidyl ether with the brand number of 664.

[0011] In a second aspect, the present invention further provides an inlay casting process for a micro motor, comprising:

[0012] Use ethanol to clean the tooling and apply release agent to each mating surface of the tooling;

[0013] Use water-free compressed air to blow the cast parts clean, and apply release agent to each mating surface of the cast parts;

[0014] Prepare 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of reactive diluent and 5-10 parts of polyol glycidyl ether respectively according to weight proportion;

[0015] Preheat the tooling, cast parts and epoxy resin;

[0016] 5 minutes before the end of preheating, the preheated epoxy resin, liquid aromatic amine curing agent, reactive diluent and polyol glycidyl ether are stirred evenly to prepare a casting material;

[0017] After the preheating time is up, take out the casting and tooling and apply the release agent again;

[0018] After assembling the cast part and the tooling together, pour the epoxy glue into the tooling along one side of the tooling. Vacuum immediately after pouring, reaching -0.1MPa within 1 minute, and maintaining -0.1MPa for 6 minutes, for 5 consecutive times, for a total of 30 minutes;

[0019] Dry the cast parts and tooling at 125-135°C;

[0020] The dried cast parts and tooling are demoulded one by one. After demoulding, they are cured at a temperature of 155-165°C for 2 hours, and then aged at 165-175°C for 3 hours. The heating is stopped and the parts are naturally cooled to room temperature.

[0021] The invention discloses an inlay casting material and casting process for micro motors. During casting, ethanol is used to clean the tooling, and a mold release agent is applied to each mating surface of the tooling; water-free compressed air is used to blow the casted part clean, and a mold release agent is applied to each mating surface of the casted part; 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of active diluent and 5-10 parts of polyol glycidyl ether are weighed respectively according to weight proportion; the tooling, the casted part and the epoxy resin are preheated; 5 minutes before the end of preheating, the preheated epoxy resin, liquid aromatic amine curing agent, active diluent and polyol glycidyl ether are preheated. Stir the oil ether evenly to obtain the casting material; after the preheating time is up, take out the cast parts and tooling, and apply the release agent again; after the cast parts and tooling are assembled together, pour the epoxy glue into the tooling along one side, and immediately evacuate after pouring, reaching -0.1MPa within 1 minute, and maintaining -0.1MPa for 6 minutes, 5 times in a row, a total of 30 minutes; dry the cast parts and tooling at a temperature of 125-135°C; demold the dried cast parts and tooling one by one, and cure at a temperature of 155-165°C for 2 hours after demolding, and then stop heating after aging at 165-175°C for 3 hours, and naturally cool to room temperature. When the present invention is used for inlay casting of micro-motor parts, the thermal deformation temperature of the present invention can reach 150 degrees Celsius, and no secondary demolding is required. The mold can be demolded after gelling, which does not affect the performance of the cast solid, and the curing and aging time is shortened by 1 / 3. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0023] Figure 1 The present invention is a flow chart of an inlay casting process for micro motors. DETAILED DESCRIPTION

[0024] In a first aspect, the present invention provides an inlay casting material for micro motors, which is composed of the following components in parts by weight: 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of active diluent and 5-10 parts of polyol glycidyl ether.

[0025] Preferably, in the above formula ratio, the present invention provides an optimal combination, including the following components in parts by weight: 100 parts of epoxy resin, 12 parts of liquid aromatic amine curing agent; 25 parts of active diluent; and 7 parts of polyol glycidyl ether.

[0026] According to this specific implementation, the epoxy resin uses epoxy resin with a brand number of 634.

[0027] Wherein, the liquid aromatic amine curing agent adopts a liquid aromatic amine curing agent with a brand of LB701.

[0028] Secondly, the active diluent is an epoxy resin active diluent. Preferably, the active diluent is an environmentally friendly A-grade colorless and odorless epoxy resin glue active diluent, specifically a 5748 active diluent.

[0029] Meanwhile, the polyol glycidyl ether adopts polyol glycidyl ether with a brand number of 664.

[0030] The inlay casting material for micro motors of the present invention comprises the following steps: during casting, the tooling is cleaned with ethanol, and a mold release agent is applied to each mating surface of the tooling; a cast piece is blown clean with anhydrous compressed air, and a mold release agent is applied to each mating surface of the cast piece; 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of active diluent, and 5-10 parts of polyol glycidyl ether are weighed respectively according to weight proportion; the tooling, the cast piece, and the epoxy resin are preheated; 5 minutes before the end of the preheating, the preheated epoxy resin, liquid aromatic amine curing agent, active diluent, and polyol glycidyl ether are stirred. Mix well to obtain casting material; after the preheating time is up, take out the cast parts and tooling, and apply the release agent again; after the cast parts and tooling are assembled together, pour the epoxy glue into the tooling along one side, and immediately evacuate after pouring, reaching -0.1MPa within 1 minute, and maintain -0.1MPa for 6 minutes, 5 times in a row, a total of 30 minutes; the cast parts and tooling are dried at a temperature of 125-135°C; demold the dried cast parts and tooling one by one, and cure at a temperature of 155-165°C for 2 hours after demolding, and then stop heating after aging at 165-175°C for 3 hours, and naturally cool to room temperature. When embedding and casting micro-motor parts, the thermal deformation temperature of the present invention can reach 150 degrees Celsius, and no secondary demolding is required. Demolding can be done after gelling, which does not affect the performance of the cast solid, and the curing and aging time is shortened by 1 / 3.

[0031] See also Figure 1 In a second aspect, the present invention provides an inlay casting process for a micro motor, comprising:

[0032] S1 uses ethanol to clean the tooling and applies a release agent to each mating surface of the tooling;

[0033] The tooling is equipment designed according to the requirements of the outer dimensions of the cast parts.

[0034] S2 uses water-free compressed air to blow the cast parts clean and applies release agent to each mating surface of the cast parts;

[0035] S3 prepares to weigh 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of reactive diluent and 5-10 parts of polyol glycidyl ether respectively according to weight proportion;

[0036] In the above formula ratio, the present invention provides an optimal combination, including the following components in parts by weight: 100 parts of epoxy resin, 12 parts of liquid aromatic amine curing agent, 25 parts of active diluent, and 7 parts of polyol glycidyl ether.

[0037] S4 preheats the tooling, cast parts and epoxy resin;

[0038] S5 5 minutes before the end of preheating, the preheated epoxy resin, liquid aromatic amine curing agent, reactive diluent and polyol glycidyl ether are stirred evenly to obtain a casting material;

[0039] S6 After the preheating time is up, take out the cast parts and tooling and apply the release agent again;

[0040] S7 After the casting and the tooling are assembled together, the epoxy glue is poured into the tooling along one side of the tooling. After pouring, vacuum is immediately drawn to reach -0.1MPa within 1 minute, and -0.1MPa is maintained for 6 minutes, for 5 consecutive times, for a total of 30 minutes;

[0041] After assembling the cast part and the tooling together, place them in a vacuum furnace, pour the epoxy glue into the tooling along one side of the tooling, and immediately evacuate the furnace after pouring to reach -0.1MPa within 1 minute, and maintain -0.1MPa for 6 minutes, for 5 consecutive times, for a total of 30 minutes.

[0042] S8: drying the cast parts and tooling at a temperature of 125-135°C;

[0043] After taking it out from the vacuum furnace, put it into a blast-type constant temperature electric drying oven, heat the oven temperature to 125-135°C in advance, and set the timer for 1 hour.

[0044] S9 demoulds the dried cast parts and tooling one by one, and after demoulding, cures at a temperature of 155-165°C for 2 hours, then ages at 165-175°C for 3 hours, stops heating, and naturally cools to room temperature.

[0045] The dried cast parts and tooling are demoulded one by one and put back into the blast-type constant temperature electric drying oven after demoulding; they are cured at 155-165℃ for 2 hours in the blast-type constant temperature electric drying oven, and then aged at 165-175℃ for 3 hours. The blast-type constant temperature electric drying oven stops heating, does not open the furnace door, and cools naturally to room temperature.

[0046] The present invention discloses an inlay casting process for micro motors. When inlay casting is performed on micro motor parts, the thermal deformation temperature of the present invention can reach 150 degrees Celsius. No secondary demoulding is required. The mold can be demoulded after gelation, and the performance of the cast solidified material is not affected. The curing and aging time is shortened by 1 / 3.

[0047] What is disclosed above is only one or more preferred embodiments of the present application, and cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiments and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.

Claims

1. A kind of inlay casting material for micro motors, It is characterized in that The invention is composed of the following components by weight: 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of active diluent and 5-10 parts of polyol glycidyl ether.

2. A casting material for a micro motor as claimed in claim 1, It is characterized in that The epoxy resin is 634 epoxy resin.

3. The inlay casting material for micro motors according to claim 1, It is characterized in that The liquid aromatic amine curing agent is a liquid aromatic amine curing agent with a brand number of LB701.

4. The inlay casting material for micro motors according to claim 1, It is characterized in that The active diluent is an epoxy resin active diluent.

5. The inlay casting material for micro motors according to claim 1, It is characterized in that The polyol glycidyl ether adopts the polyol glycidyl ether with the brand number of 664.

6. An inlay casting process for a micro motor, using an inlay casting material for a micro motor as claimed in any one of claims 1 to 5, It is characterized in that include: Use ethanol to clean the tooling and apply release agent to each mating surface of the tooling; Use water-free compressed air to blow the cast parts clean, and apply mold release agent to each mating surface of the cast parts; Prepare 100 parts of epoxy resin, 5-20 parts of liquid aromatic amine curing agent, 20-30 parts of reactive diluent and 5-10 parts of polyol glycidyl ether respectively according to weight proportion; Preheat the tooling, cast parts and epoxy resin; 5 minutes before the end of preheating, the preheated epoxy resin, liquid aromatic amine curing agent, reactive diluent and polyol glycidyl ether are stirred evenly to prepare a casting material; After the preheating time is up, take out the casting and tooling and apply the release agent again; After assembling the cast part and the tooling together, pour the epoxy glue into the tooling along one side of the tooling. Vacuum immediately after pouring, reaching -0.1MPa within 1 minute, and maintaining -0.1MPa for 6 minutes, for 5 consecutive times, for a total of 30 minutes; Dry the cast parts and tooling at 125-135°C; The dried cast parts and tooling are demoulded one by one. After demoulding, they are cured at a temperature of 155-165°C for 2 hours, and then aged at 165-175°C for 3 hours. The heating is stopped and the parts are naturally cooled to room temperature.