Anti-interference electromagnetic shielding absorbing special rubber material and preparation process thereof

A specialized rubber composition with conductive fillers and a specific preparation process addresses the limitations of traditional rubbers, enhancing electromagnetic shielding and wave absorption through a conductive grid structure and dielectric/magnetic polarization, achieving effective and cost-efficient performance.

CN119081245AInactive Publication Date: 2024-12-06GUANGDONG RUNYIN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411443416.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional special rubbers face challenges in achieving high conductivity with carbon-based materials and metal powders due to their high density and cost, which limits their effectiveness in electromagnetic shielding and wave absorption.

Method used

A special rubber composition comprising conductive fillers, resistive and dielectric absorbers, magnetic medium absorbers, iron oxide, and hydroxyl iron, along with a specific preparation process that includes crushing, oil mixing, secondary mixing, desulfurization, and refining, to create a conductive and cost-effective material.

Benefits of technology

The solution results in a rubber material with improved electromagnetic shielding and wave absorption capabilities, utilizing a conductive filler grid structure and dielectric and magnetic loss tangents for effective wave absorption, meeting user needs while being environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081245A_ABST
    Figure CN119081245A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-interference electromagnetic shielding absorbing special rubber material and a preparation process of the anti-interference electromagnetic shielding absorbing special rubber material. The special rubber is prepared from, by weight, 10-15 parts of conductive filler, 5-8 parts of resistance type absorbent, 5-8 parts of dielectric type absorbent, 5-8 parts of magnetic medium type absorbent, 6-10 parts of iron oxide, 6-10 parts of hydroxyl iron, 6-10 parts of hydroxyl body and 50-55 parts of raw rubber, the selected composite metal material is a conductive material, and the special rubber is good in conductivity, low in density and low in cost; along with the input of a reinforcing agent, a plasticizer and an anti-aging agent, the rubber component is isolated by a large number of composite metal materials, the grid structure of the conductive filler is developed, the anti-interference electromagnetic shielding performance of the special rubber is improved, the use requirements of people are met, and the resistance-type absorbent has higher dielectric loss tangent and can be used as a conductive material for the special rubber. Electromagnetic waves are absorbed by means of electron polarization or interface polarization attenuation of a medium, and the magnetic medium type absorbent has high magnetic loss angle tangent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of special rubbers, in particular to an anti-interference electromagnetic shielding and wave-absorbing special rubber material and a preparation process thereof. Background Art

[0002] Special rubber refers to rubber with special uses and small usage, which accounts for about 1% of the total rubber usage. Most of them are saturated rubbers, with carbon chains and heterochains as the main chains. Except for silicone rubber, all of them are polar. These rubbers are diverse in structure and have their own characteristics in performance. Special rubbers include nearly 10 types such as fluororubber, silicone rubber, and polyurethane rubber.

[0003] With the rapid development and widespread application of electronics, computers and telecommunications technology, the electromagnetic environment in space has become increasingly complex. Various electronic instruments, communication equipment and computers themselves will generate electromagnetic waves, affecting the normal operation of other equipment. At the same time, they themselves will be interfered by external electromagnetic waves, which has a huge potential hazard to important systems such as precision instruments, aerospace engineering, navigation equipment, scientific measurement, and medical care equipment. Ordinary silicone rubber itself is a high-insulating material with low magnetic permeability, and it has no shielding or absorption effect on electromagnetic waves. However, since silicone rubber has excellent high and low temperature resistance, weather aging resistance, low processing viscosity and high filling capacity that other rubbers cannot match, people have realized the application of silicone rubber in the field of electromagnetic shielding by adding a large amount of conductive fillers or magnetic fillers. This kind of silicone rubber is a special rubber.

[0004] However, traditional special rubber has the following disadvantages:

[0005] Carbon materials and metal powders are added to traditional special rubbers to make them conductive and anti-electromagnetic. Carbon materials have average conductivity, and it is difficult to prepare highly conductive rubbers with a volume resistivity below lohm-cm. Metal powders have the disadvantages of high density and high cost, and cannot meet people's usage needs. Summary of the invention

[0006] The purpose of the present invention is to provide an anti-interference electromagnetic shielding and wave absorbing special rubber material and its preparation process, so as to solve the problem proposed in the above background technology that carbon-based materials and metal powder are added to the traditional special rubber for conductive and anti-electromagnetic properties. The carbon-based materials have general conductivity and it is difficult to prepare highly conductive rubber with a volume resistivity below lohm-cm. The metal powder has the disadvantages of high density and high cost and cannot meet people's usage needs.

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solution: an anti-interference electromagnetic shielding wave-absorbing special rubber material, comprising the following components: by weight, 10-15 parts of conductive filler, 5-8 parts of resistive absorbent, 5-8 parts of dielectric absorbent, 5-8 parts of magnetic medium absorbent, 6-10 parts of iron oxide, 6-10 parts of hydroxyl iron, 6-10 parts of hydroxyl body and 50-55 parts of rubber raw rubber.

[0008] As a preferred technical solution of the present invention, calculated by weight, the conductive filler is 15 parts, the resistive absorber is 5 parts, the dielectric absorber is 5 parts, the magnetic absorber is 6 parts, the iron oxide is 6 parts, the hydroxy iron is 6 parts, the hydroxyl body is 6 parts and the rubber is 51 parts.

[0009] As a preferred technical solution of the present invention, calculated by weight, the conductive filler is 10 parts, the resistive absorber is 6 parts, the dielectric absorber is 6 parts, the magnetic absorber is 6 parts, the iron oxide is 6 parts, the hydroxy iron is 6 parts, the hydroxyl body is 6 parts and the rubber is 54 parts.

[0010] As a preferred technical solution of the present invention, calculated by weight, the conductive filler is 10 parts, the resistive absorber is 5 parts, the dielectric absorber is 5 parts, the magnetic absorber is 5 parts, the iron oxide is 6 parts, the hydroxy iron is 6 parts, the hydroxyl body is 8 parts and the rubber is 55 parts.

[0011] As a preferred technical solution of the present invention, calculated by weight, the conductive filler is 12 parts, the resistive absorber is 6 parts, the dielectric absorber is 6 parts, the magnetic absorber is 6 parts, the iron oxide is 6 parts, the hydroxy iron is 6 parts, the hydroxyl body is 6 parts and the rubber is 52 parts.

[0012] As a preferred technical solution of the present invention, the conductive filler includes silver-plated glass beads, silver-plated aluminum powder, silver-plated nickel powder, silver-plated copper powder, nickel-plated graphite and nickel-plated carbon fiber.

[0013] As a preferred technical solution of the present invention, the resistive absorber includes conductive carbon black, graphite, carbon fiber and silicon carbide, and the dielectric absorber includes barium titanate, silicon nitride and iron nitride.

[0014] As a preferred technical solution of the present invention, the iron oxide is SrCo2Fe 16 O 27 .

[0015] The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material of the present invention comprises the following steps:

[0016] Step 1: Crushing: Use a common double-roll crusher or a common rubber mixer to crush 50-55 parts of the block rubber raw rubber;

[0017] Step 2, oil mixing: put the coarsely crushed rubber particles into a high-speed desulfurizer, first stir and crush them at high speed for 2-3 minutes, then add softener activator and 5-8 parts of resistive absorbent, 5-8 parts of dielectric absorbent and 5-8 parts of magnetic absorbent according to the formula, and stir evenly for 5 minutes;

[0018] Step 3, secondary mixing: add 10-15 parts of conductive filler, 6-10 parts of iron oxide, 6-10 parts of hydroxy iron and 6-10 parts of hydroxyl body to the oil-mixed mixture, and stir evenly for 5 minutes;

[0019] Step 4, desulfurization: the mixed mixture is subjected to desulfurization processing;

[0020] Step 5, refining: the desulfurized rubber is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes. It can be sheeted after refining once.

[0021] As a preferred technical solution of the present invention, the desulfurization in the step 4 is specifically as follows: first, the desulfurization conditions of the dynamic desulfurization tank are: pressure 2.8-3.0Mpa, pressure holding time 60 minutes, and the correct desulfurization time needs to be found; second, a special pressure kneading desulfurizer for butyl regenerated rubber: loading 80kg, temperature 210°C, time 12 minutes, and it is particularly important to open the cover and turn the rubber every 3 minutes to achieve the purpose of uniform desulfurization, and environmental protection facilities must be installed; third, desulfurization in the open mill: no pressurization and heating are required, and desulfurization and production of butyl regenerated rubber can be achieved at room temperature, without the generation of wastewater and waste gas, and no pollution. It is a green and environmentally friendly process for producing butyl regenerated rubber.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The composite metal material used for this special rubber is a conductive material with good conductivity, low density and low cost. With the input of reinforcing agent, plasticizer and antioxidant, the rubber component is isolated by a large amount of composite metal material, and the conductive filler grid structure is developed, which improves the anti-interference electromagnetic shielding performance of the special rubber and meets people's use needs;

[0024] 2. Resistive absorbers have a higher dielectric loss tangent and rely on the electronic polarization or interface polarization attenuation of the medium to absorb electromagnetic waves. Dielectric absorbers absorb electromagnetic waves through dielectric polarization relaxation loss. Magnetic dielectric absorbers have a higher magnetic loss tangent, which makes the prepared special materials have good wave absorption characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a flow chart of the present invention;

[0026] Figure 2 This is a SEM image of the silver-coated glass microbeads of the present invention;

[0027] Figure 3 This is a SEM image of the silver-plated aluminum powder of the present invention;

[0028] Figure 4 It is the SEM picture of nickel-plated graphite of the present invention;

[0029] Figure 5 This is a SEM image of the nickel-plated carbon fiber of the present invention;

[0030] Figure 6 The SEM, EDS and XRD diagrams of the iron oxide of the present invention are shown below;

[0031] Figure 7 This is a graph showing the relationship between the bandwidth and peak area of ​​the iron oxide of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] See also Figure 1-7 The present invention provides an anti-interference electromagnetic shielding wave-absorbing special rubber material, which includes the following components: by weight, 10-15 parts of conductive filler, 5-8 parts of resistive absorbent, 5-8 parts of dielectric absorbent, 5-8 parts of magnetic medium absorbent, 6-10 parts of iron oxide, 6-10 parts of hydroxyl iron, 6-10 parts of hydroxyl body and 50-55 parts of rubber raw rubber.

[0035] The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material of the present invention comprises the following steps:

[0036] Step 1: Crushing: Use a common double-roll crusher or a common rubber mixer to crush 50-55 parts of the block rubber raw rubber;

[0037] Step 2, oil mixing: put the coarsely crushed rubber particles into a high-speed desulfurizer, first stir and crush them at high speed for 2-3 minutes, then add softener activator and 5-8 parts of resistive absorbent, 5-8 parts of dielectric absorbent and 5-8 parts of magnetic absorbent according to the formula, and stir evenly for 5 minutes;

[0038] Step 3, secondary mixing: add 10-15 parts of conductive filler, 6-10 parts of iron oxide, 6-10 parts of hydroxy iron and 6-10 parts of hydroxyl body to the oil-mixed mixture, and stir evenly for 5 minutes;

[0039] Step 4, desulfurization: the mixed mixture is subjected to desulfurization processing;

[0040] Step 5, refining: the desulfurized rubber is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes. It can be sheeted after refining once.

[0041] The desulfurization in step 4 is specifically as follows: first, the desulfurization conditions of the dynamic desulfurization tank: pressure 2.8-3.0Mpa, pressure holding time 60 minutes, and the correct desulfurization time needs to be found; second, the special pressure kneading desulfurizer for butyl regenerated rubber: loading 80kg, temperature 210℃, time 12 minutes, and it is particularly important to open the cover and turn the rubber over every 3 minutes to achieve the purpose of uniform desulfurization, and environmental protection facilities must be installed; third, desulfurization in the open mill: no pressurization and heating are required, and desulfurization and production of butyl regenerated rubber can be achieved at room temperature, without the generation of wastewater and waste gas, and no pollution. It is a green and environmentally friendly process for producing butyl regenerated rubber.

[0042] Embodiment 2:

[0043] See also Figure 1-7 The present invention provides an anti-interference electromagnetic shielding wave absorbing special rubber material, which includes the following components: by weight, 15 parts of conductive filler, 5 parts of resistive absorbent, 5 parts of dielectric absorbent, 6 parts of magnetic medium absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 6 parts of hydroxyl body and 51 parts of rubber raw rubber.

[0044] The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material of the present invention comprises the following steps:

[0045] Step 1: Crushing: Use a common double-roller coarse crusher or a common rubber mixer to coarsely crush 51 parts of the block rubber raw rubber product;

[0046] Step 2, oil mixing: put the coarsely crushed rubber particles into a high-speed desulfurizer, firstly stir and crush them at high speed for 2-3 minutes, then add softener activator and 5 parts of resistive absorbent, 5 parts of dielectric absorbent and 6 parts of magnetic absorbent according to the formula, and stir evenly for 5 minutes;

[0047] Step 3, secondary mixing: add 15 parts of conductive filler, 6 parts of iron oxide, 6 parts of hydroxy iron and 6 parts of hydroxyl body to the oil-mixed mixture, and stir evenly for 5 minutes;

[0048] Step 4, desulfurization: the mixed mixture is subjected to desulfurization processing;

[0049] Step 5, refining: the desulfurized rubber is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes. It can be sheeted after refining once.

[0050] The desulfurization in step 4 is specifically as follows: first, the desulfurization conditions of the dynamic desulfurization tank: pressure 2.8-3.0Mpa, pressure holding time 60 minutes, and the correct desulfurization time needs to be found; second, the special pressure kneading desulfurizer for butyl regenerated rubber: loading 80kg, temperature 210℃, time 12 minutes, and it is particularly important to open the cover and turn the rubber over every 3 minutes to achieve the purpose of uniform desulfurization, and environmental protection facilities must be installed; third, desulfurization in the open mill: no pressurization and heating are required, and desulfurization and production of butyl regenerated rubber can be achieved at room temperature, without the generation of wastewater and waste gas, and no pollution. It is a green and environmentally friendly process for producing butyl regenerated rubber.

[0051] Example 3

[0052] See also Figure 1-7 The present invention provides an anti-interference electromagnetic shielding wave absorbing special rubber material, which includes the following components: by weight, 10 parts of conductive filler, 6 parts of resistive absorbent, 6 parts of dielectric absorbent, 6 parts of magnetic medium absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 6 parts of hydroxyl body and 54 parts of rubber raw rubber.

[0053] The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material of the present invention comprises the following steps:

[0054] Step 1: Crushing: Use a common double-roller coarse crusher or a common rubber mixer to coarsely crush 54 parts of the block rubber raw rubber product;

[0055] Step 2, oil mixing: put the coarsely crushed rubber particles into a high-speed desulfurizer, first stir and crush them at high speed for 2-3 minutes, then add softener activator and 6 parts of resistive absorbent, 6 parts of dielectric absorbent and 6 parts of magnetic absorbent according to the formula, and stir evenly for 5 minutes;

[0056] Step 3, secondary mixing: add 10 parts of conductive filler, 6 parts of iron oxide, 6 parts of hydroxy iron and 6 parts of hydroxyl body to the oil-mixed mixture, and stir evenly for 5 minutes;

[0057] Step 4, desulfurization: the mixed mixture is subjected to desulfurization processing;

[0058] Step 5, refining: the desulfurized rubber is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes. It can be sheeted after refining once.

[0059] The desulfurization in step 4 is specifically as follows: first, the desulfurization conditions of the dynamic desulfurization tank: pressure 2.8-3.0Mpa, pressure holding time 60 minutes, and the correct desulfurization time needs to be found; second, the special pressure kneading desulfurizer for butyl regenerated rubber: loading 80kg, temperature 210℃, time 12 minutes, and it is particularly important to open the cover and turn the rubber over every 3 minutes to achieve the purpose of uniform desulfurization, and environmental protection facilities must be installed; third, desulfurization in the open mill: no pressurization and heating are required, and desulfurization and production of butyl regenerated rubber can be achieved at room temperature, without the generation of wastewater and waste gas, and no pollution. It is a green and environmentally friendly process for producing butyl regenerated rubber.

[0060] Example 4

[0061] See also Figure 1-7 The present invention provides an anti-interference electromagnetic shielding wave absorbing special rubber material, which includes the following components: by weight, 10 parts of conductive filler, 5 parts of resistive absorbent, 5 parts of dielectric absorbent, 5 parts of magnetic medium absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 8 parts of hydroxyl body and 55 parts of rubber raw rubber.

[0062] The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material of the present invention comprises the following steps:

[0063] Step 1: Crushing: Use a common double-roller crusher or a common rubber mixer to crush 55 parts of the block rubber raw rubber products;

[0064] Step 2, oil mixing: put the coarsely crushed rubber particles into a high-speed desulfurizer, first stir and crush them at high speed for 2-3 minutes, then add softener activator and 5 parts of resistive absorbent, 5 parts of dielectric absorbent and 5 parts of magnetic absorbent according to the formula, and stir evenly for 5 minutes;

[0065] Step 3, secondary mixing: add 10 parts of conductive filler, 6 parts of iron oxide, 6 parts of hydroxy iron and 8 parts of hydroxyl body to the oil-mixed mixture, and stir evenly for 5 minutes;

[0066] Step 4, desulfurization: the mixed mixture is subjected to desulfurization processing;

[0067] Step 5, refining: the desulfurized rubber is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes. It can be sheeted after refining once.

[0068] The desulfurization in step 4 is specifically as follows: first, the desulfurization conditions of the dynamic desulfurization tank: pressure 2.8-3.0Mpa, pressure holding time 60 minutes, and the correct desulfurization time needs to be found; second, the special pressure kneading desulfurizer for butyl regenerated rubber: loading 80kg, temperature 210℃, time 12 minutes, and it is particularly important to open the cover and turn the rubber over every 3 minutes to achieve the purpose of uniform desulfurization, and environmental protection facilities must be installed; third, desulfurization in the open mill: no pressurization and heating are required, and desulfurization and production of butyl regenerated rubber can be achieved at room temperature, without the generation of wastewater and waste gas, and no pollution. It is a green and environmentally friendly process for producing butyl regenerated rubber.

[0069] Example 5

[0070] See also Figure 1-7 The present invention provides an anti-interference electromagnetic shielding wave absorbing special rubber material, which includes the following components: by weight, 12 parts of conductive filler, 6 parts of resistive absorbent, 6 parts of dielectric absorbent, 6 parts of magnetic medium absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 6 parts of hydroxyl body and 52 parts of rubber raw rubber.

[0071] The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material of the present invention comprises the following steps:

[0072] Step 1: Crushing: Use a common double-roller crusher or a common rubber mixer to crush the two parts of the block rubber raw rubber products;

[0073] Step 2, oil mixing: put the coarsely crushed rubber particles into a high-speed desulfurizer, first stir and crush them at high speed for 2-3 minutes, then add softener activator and 6 parts of resistive absorbent, 6 parts of dielectric absorbent and 6 parts of magnetic absorbent according to the formula, and stir evenly for 5 minutes;

[0074] Step 3, secondary mixing: add 12 parts of conductive filler, 6 parts of iron oxide, 6 parts of hydroxy iron and 6 parts of hydroxyl body to the oil-mixed mixture, and stir evenly for 5 minutes;

[0075] Step 4, desulfurization: the mixed mixture is subjected to desulfurization processing;

[0076] Step 5, refining: the desulfurized rubber is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes. It can be sheeted after refining once.

[0077] The desulfurization in step 4 is specifically as follows: first, the desulfurization conditions of the dynamic desulfurization tank: pressure 2.8-3.0Mpa, pressure holding time 60 minutes, and the correct desulfurization time needs to be found; second, the special pressure kneading desulfurizer for butyl regenerated rubber: loading 80kg, temperature 210℃, time 12 minutes, and it is particularly important to open the cover and turn the rubber over every 3 minutes to achieve the purpose of uniform desulfurization, and environmental protection facilities must be installed; third, desulfurization in the open mill: no pressurization and heating are required, and desulfurization and production of butyl regenerated rubber can be achieved at room temperature, without the generation of wastewater and waste gas, and no pollution. It is a green and environmentally friendly process for producing butyl regenerated rubber.

[0078] Conductive fillers include silver-coated glass beads, silver-coated aluminum powder, silver-coated nickel powder, silver-coated copper powder, nickel-coated graphite and nickel-coated carbon fiber.

[0079] The resistive absorbers include conductive carbon black, graphite, carbon fiber and silicon carbide, and the dielectric absorbers include barium titanate, silicon nitride, iron nitride.

[0080] Iron oxide is SrCo2Fe 16 O 27 .

[0081] In the present invention, a common double-roll coarse crusher or a common rubber mixer can be used to coarsely crush 50-55 parts of blocky raw rubber products; the coarsely crushed rubber particles are loaded into a high-speed desulfurizer, firstly subjected to high-speed stirring and crushing for 2-3 minutes, and then softener activator and 5-8 parts of resistive absorbent, 5-8 parts of dielectric absorbent and 5-8 parts of magnetic absorbent are added according to the formula, and stirred evenly for 5 minutes; 10-15 parts of conductive filler, 6-10 parts of iron oxide, 6-10 parts of hydroxy iron and 6-10 parts of hydroxyl body are added to the mixture after oil mixing, and stirred evenly for 5 minutes; the mixed mixture is subjected to desulfurization processing; the desulfurized rubber material is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes, and the sheet can be removed after refining once. During the processing, the preparation ingredient list of the raw rubber is as follows:

[0082]

[0083]

[0084] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. Anti-interference electromagnetic shielding wave absorbing special rubber material, characterized in that: The invention comprises the following components: by weight, 10-15 parts of conductive filler, 5-8 parts of resistive absorbent, 5-8 parts of dielectric absorbent, 5-8 parts of magnetic absorbent, 6-10 parts of iron oxide, 6-10 parts of hydroxy iron, 6-10 parts of hydroxyl body and 50-55 parts of raw rubber.

2. The anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: In terms of weight, there are 15 parts of conductive filler, 5 parts of resistive absorbent, 5 parts of dielectric absorbent, 6 parts of magnetic absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 6 parts of hydroxyl body and 51 parts of rubber.

3. The anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: In terms of weight, there are 10 parts of conductive filler, 6 parts of resistive absorbent, 6 parts of dielectric absorbent, 6 parts of magnetic absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 6 parts of hydroxyl body and 54 parts of rubber.

4. The anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: In terms of weight, there are 10 parts of conductive filler, 5 parts of resistive absorbent, 5 parts of dielectric absorbent, 5 parts of magnetic absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 8 parts of hydroxyl body and 55 parts of rubber.

5. The anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: In terms of weight, there are 12 parts of conductive filler, 6 parts of resistive absorbent, 6 parts of dielectric absorbent, 6 parts of magnetic absorbent, 6 parts of iron oxide, 6 parts of hydroxy iron, 6 parts of hydroxyl body and 52 parts of rubber.

6. The anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: The conductive filler includes silver-plated glass microbeads, silver-plated aluminum powder, silver-plated nickel powder, silver-plated copper powder, nickel-plated graphite and nickel-plated carbon fiber.

7. The anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: The resistive absorbent includes conductive carbon black, graphite, carbon fiber and silicon carbide, and the dielectric absorbent includes barium titanate, silicon nitride and iron nitride.

8. The anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: The iron oxide is SrCo2Fe 16 O 27 .

9. The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Crushing: Use a common double-roll crusher or a common rubber mixer to crush 50-55 parts of the block rubber raw rubber; Step 2, oil mixing: put the coarsely crushed rubber particles into a high-speed desulfurizer, first stir and crush them at high speed for 2-3 minutes, then add softener activator and 5-8 parts of resistive absorbent, 5-8 parts of dielectric absorbent and 5-8 parts of magnetic absorbent according to the formula, and stir evenly for 5 minutes; Step 3, secondary mixing: add 10-15 parts of conductive filler, 6-10 parts of iron oxide, 6-10 parts of hydroxy iron and 6-10 parts of hydroxyl body to the oil-mixed mixture, and stir evenly for 5 minutes; Step 4, desulfurization: the mixed mixture is subjected to desulfurization processing; Step 5, refining: the desulfurized rubber is mainly thinly passed on the mixer, and each time it is refined for 15-20 minutes. It can be sheeted after refining once.

10. The preparation process of the anti-interference electromagnetic shielding wave absorbing special rubber material according to claim 1, characterized in that: The desulfurization in step 4 is specifically as follows: first, the desulfurization conditions of the dynamic desulfurization tank are: pressure 2.8-3.0Mpa, pressure holding time 60 minutes, and the correct desulfurization time needs to be found; second, the butyl regenerated rubber special pressure kneading desulfurizer: loading 80kg, temperature 210℃, time 12 minutes, it is particularly important to open the cover and turn the rubber every 3 minutes to achieve the purpose of uniform desulfurization, and environmental protection facilities must be installed; Third, desulfurization on the mixing mill: no need for pressurization and heating, desulfurization can be achieved at room temperature to produce butyl reclaimed rubber, no waste water or waste gas is generated, no pollution, it is a green and environmentally friendly process for producing butyl reclaimed rubber.