Automotive interior material and preparation method thereof

By using calcium and zinc thermal stabilizers, polyol phosphates and amino POSS and PVC resin in automotive interior materials, the problem of easy degradation of PVC materials at high temperatures is solved, and its thermal stability and mechanical properties are significantly improved. Suitable for use environments that are exposed to outdoors for a long time.

CN119081307AActive Publication Date: 2024-12-06HUNAN DALI TECH CONSULTING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411186199.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Traditional automotive interior material PVC is prone to degradation and aging under light and high temperature environments, resulting in a decline in mechanical properties and is difficult to meet the needs of long-term exposure to outdoors.

Method used

Combined with PVC resin with a composite thermal stabilizer including calcium and zinc heat stabilizer, polyol phosphate and amino POSS, and prepared automotive interior materials through the hot pressing process of a double-roller plasticizer and a flat-panel vulcanizer to improve their thermal stability. and mechanical properties.

Benefits of technology

It effectively improves the thermal stability and mechanical properties of automotive interior materials, extends its service life, and reduces the performance decline in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081307A_ABST
    Figure CN119081307A_ABST
Patent Text Reader

Abstract

The invention relates to the field of high polymer materials, in particular to an automotive interior material and a preparation method thereof, and the automotive interior material comprises PVC (polyvinyl chloride) resin and a composite heat stabilizer, the invention discloses an automotive interior material, which comprises PVC resin and a composite heat stabilizer, the composite heat stabilizer comprises a calcium-zinc heat stabilizer, polyol phosphate and amino POSS, the mass ratio of the PVC resin to the composite heat stabilizer is (20-40): 1, and the mass ratio of the calcium-zinc heat stabilizer to the polyol phosphate to the amino POSS is (1-5): (1-5): (1-5). And the thermal aging resistance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, in particular to an automobile interior material and a preparation method thereof. Background Art

[0002] The car interior system is an important part of the car body, and the design workload of the interior system accounts for more than 60% of the car styling design workload, far exceeding the car's appearance, and is one of the most important parts of the car body.

[0003] Traditional automotive interior materials are mostly PVC materials, but PVC materials have poor stability to light and heat. They will degrade and age under light or high temperature, causing mechanical properties to decline. Although the impact of light can be reduced by applying film, in summer, cars are exposed to the outdoors for a long time, and the temperature inside the car can often reach above 70°C, which will undoubtedly accelerate the degradation and aging of PVC materials, causing the performance of automotive interior materials to decline. Summary of the invention

[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes an automobile interior material and a preparation method thereof.

[0005] The technical solutions adopted are as follows:

[0006] An automobile interior material, comprising PVC resin and a composite heat stabilizer;

[0007] The composite heat stabilizer comprises a calcium zinc heat stabilizer, a polyol phosphate ester and an amino POSS.

[0008] Furthermore, the mass ratio of the PVC resin to the composite heat stabilizer is 20-40:1.

[0009] Furthermore, the mass ratio of the calcium zinc heat stabilizer, the polyol phosphate and the amino POSS is 1-5:1-5:1-5.

[0010] Furthermore, the structural formula of the polyol phosphate is as follows:

[0011]

[0012] Wherein, R1 and R2 are each independently a C1-C10 alkyl group or a C6-C30 aromatic group. Further, R1 and R2 are each independently a C6-C10 alkyl group, a phenyl group, or a biphenyl group. Further, the polyol phosphate is any one or more combinations of the following compounds:

[0013]

[0014]

[0015] Furthermore, the amino POSS is octa-p-aminophenyl POSS and / or N-phenylamino POSS.

[0016] Furthermore, it also includes ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin.

[0017] The present invention also provides a method for preparing an automobile interior material:

[0018] PVC resin, composite heat stabilizer, ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin are mixed and plasticized on a double-roll plasticizer, and then hot-pressed on a flat vulcanizer before demoulding and cutting.

[0019] Furthermore, the hot pressing temperature is 170-190° C., the hot pressing pressure is 5-15 MPa, and the hot pressing time is 5-10 min.

[0020] Beneficial effects of the present invention:

[0021] The present invention provides an automobile interior material. PVC molecules have some unstable defect structures. It is precisely because of the existence of these defect structures that the PVC material is easily degraded at high temperatures. The calcium zinc heat stabilizer in the present invention can replace the unstable structures of allyl chloride, tertiary chlorine, secondary chlorine, etc., reduce unstable factors, solve the thermal stability problem from the root, and reduce the autocatalytic effect by absorbing HCl generated in the neutralization system.

[0022] In the present invention, the polyol phosphate is used as an auxiliary heat stabilizer. The hydroxyl group in its structure can coordinate with the metal ions in the calcium zinc heat stabilizer, neutralize or complex some by-products produced by the stabilizer, play a stabilizing role, and can effectively improve the static heat stability time. The phosphite structure can replace the chlorine atom in the allylic position, or combine with the generated conjugated diene structure to destroy its conjugation effect, which can effectively improve the initial whiteness and thermal stability of the product.

[0023] The Si-O and Si-C inorganic cores in the amino POSS structure of the present invention have good heat resistance and flame retardancy, and play a positive role in improving the thermal stability and mechanical properties of PVC. The reason may be that the amino group can form a chelate with zinc ions to inhibit "zinc burning", thereby maintaining long-term thermal stability.

[0024] The automobile interior material prepared by the invention has good thermal stability and mechanical properties and excellent heat aging resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM photograph of the automotive interior material prepared in Example 1, showing that its surface is uniform and dense. DETAILED DESCRIPTION

[0026] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0027] PVC resin: QS-1000F, Sinopec;

[0028] Calcium zinc heat stabilizer: STA-102CA, Qingyang County Ruiying Plastic Chemical Sales Co., Ltd.;

[0029] Polyol phosphate ester: homemade;

[0030] Octa-p-aminophenyl POSS: CAS 518359-82-5, Shanghai Shiyang Chemical Co., Ltd.;

[0031] N-phenylamino POSS: CAS1708993-28-5, Forsman Technology (Beijing) Co., Ltd.;

[0032] ACR: Japan Kanebuchi PA20;

[0033] CPE: Runfeng Synthetic Technology;

[0034] Heavy calcium carbonate: Guangdong Yongfeng Chemical Co., Ltd.;

[0035] Titanium dioxide: Guangdong Yongfeng Chemical Co., Ltd.;

[0036] Polyethylene wax: Dongguan Dingxin Plastic Raw Materials Co., Ltd.;

[0037] Paraffin: Dongguan Dingxin Plastic Raw Materials Co., Ltd.

[0038] Embodiment 1:

[0039] This embodiment provides an automotive interior material, the specific formula is as follows (by weight):

[0040] 100 parts of PVC resin, 2 parts of calcium zinc heat stabilizer, 1 part of polyol phosphate, 1 part of octa-aminophenyl POSS, 5 parts of ACR, 5 parts of CPE, 25 parts of heavy calcium carbonate, 5 parts of titanium dioxide, 0.5 parts of polyethylene wax, and 0.5 parts of paraffin wax;

[0041] Among them, the structural formula of polyol phosphate is as follows:

[0042]

[0043] The preparation method of polyol phosphate is as follows:

[0044]

[0045] In a four-necked flask equipped with strong stirring, condenser and thermometer, add 75g toluene and 101g epoxidized glycerol alcoholysed castor oil polyol, mix well and heat to 40°C, then slowly drop the mixed solution (composed of 75g toluene, 95g didecyl phosphate and 0.5g triphenylphosphine) for 0.5h. After the addition is complete, heat to 75°C and react for 5h. After the reaction is complete, return to room temperature, neutralize the reaction system to pH 7 with 1mol / L sodium hydroxide solution, and then remove small molecules by reduced pressure distillation.

[0046] The preparation method of the above-mentioned automobile interior material is as follows:

[0047] Mix PVC resin, calcium zinc heat stabilizer, polyol phosphate, octa-aminophenyl POSS, ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin, and plasticize on a double-roll plasticizer at 160°C for 5 minutes. Then, hot press on a flat vulcanizer at 180°C and 15MPa for 10 minutes, cool to room temperature, demold, and cut.

[0048] Embodiment 2:

[0049] This embodiment provides an automotive interior material, the specific formula is as follows (by weight):

[0050] 100 parts of PVC resin, 2 parts of calcium zinc heat stabilizer, 1 part of polyol phosphate, 1 part of octa-aminophenyl POSS, 5 parts of ACR, 5 parts of CPE, 25 parts of heavy calcium carbonate, 5 parts of titanium dioxide, 0.5 parts of polyethylene wax, and 0.5 parts of paraffin wax;

[0051] Among them, the structural formula of polyol phosphate is as follows:

[0052]

[0053] The preparation method of polyol phosphate is as follows:

[0054]

[0055] In a four-necked flask equipped with strong stirring, condenser and thermometer, add 75g toluene and 101g epoxidized glycerol alcoholysed castor oil polyol, mix well and heat to 40°C, then slowly drop the mixed solution (composed of 75g toluene, 78.5g monodecylphenyl phosphate and 0.5g triphenylphosphine) for 0.5h. After the addition is complete, heat to 75°C and react for 5h. After the reaction is complete, return to room temperature, neutralize the reaction system to pH 7 with 1mol / L sodium hydroxide solution, and then remove small molecules by reduced pressure distillation.

[0056] The preparation method of the above-mentioned automobile interior material is as follows:

[0057] Mix PVC resin, calcium zinc heat stabilizer, polyol phosphate, octa-aminophenyl-POSS, ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin, and plasticize on a double-roll plasticizer at 160°C for 5 minutes. Then, hot press on a flat vulcanizer at 180°C and 15MPa for 10 minutes, cool to room temperature, demold, and cut.

[0058] Embodiment 3:

[0059] This embodiment provides an automotive interior material, the specific formula is as follows (by weight):

[0060] 100 parts of PVC resin, 2 parts of calcium zinc heat stabilizer, 2 parts of polyol phosphate, 1 part of octa-aminophenyl POSS, 5 parts of ACR, 5 parts of CPE, 25 parts of heavy calcium carbonate, 5 parts of titanium dioxide, 0.5 parts of polyethylene wax, and 0.5 parts of paraffin wax;

[0061] Among them, the structural formula of polyol phosphate is as follows:

[0062]

[0063] The preparation method of polyol phosphate is the same as that in Example 1.

[0064] The preparation method of the above-mentioned automobile interior material is as follows:

[0065] Mix PVC resin, calcium zinc heat stabilizer, polyol phosphate, octa-aminophenyl POSS, ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin, and plasticize on a double-roll plasticizer at 160°C for 5 minutes. Then, hot press on a flat vulcanizer at 180°C and 15MPa for 10 minutes, cool to room temperature, demold, and cut.

[0066] Embodiment 4:

[0067] This embodiment provides an automotive interior material, the specific formula is as follows (by weight):

[0068] 100 parts of PVC resin, 2 parts of calcium zinc heat stabilizer, 1 part of polyol phosphate, 2 parts of octa-p-aminophenyl POSS, 5 parts of ACR, 5 parts of CPE, 25 parts of heavy calcium carbonate, 5 parts of titanium dioxide, 0.5 parts of polyethylene wax, and 0.5 parts of paraffin wax;

[0069] Among them, the structural formula of polyol phosphate is as follows:

[0070]

[0071] The preparation method of polyol phosphate is the same as that in Example 1.

[0072] The preparation method of the above-mentioned automobile interior material is as follows:

[0073] Mix PVC resin, calcium zinc heat stabilizer, polyol phosphate, octa-aminophenyl POSS, ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin, and plasticize on a double-roll plasticizer at 160°C for 5 minutes. Then, hot press on a flat vulcanizer at 180°C and 15MPa for 10 minutes, cool to room temperature, demold, and cut.

[0074] Embodiment 5:

[0075] This embodiment provides an automotive interior material, the specific formula is as follows (by weight):

[0076] 100 parts of PVC resin, 2 parts of calcium zinc heat stabilizer, 1 part of polyol phosphate, 1 part of N-phenylamino POSS, 5 parts of ACR, 5 parts of CPE, 25 parts of heavy calcium carbonate, 5 parts of titanium dioxide, 0.5 parts of polyethylene wax, and 0.5 parts of paraffin;

[0077] Among them, the structural formula of polyol phosphate is as follows:

[0078]

[0079] The preparation method of polyol phosphate is the same as that in Example 1.

[0080] The preparation method of the above-mentioned automobile interior material is as follows:

[0081] Mix PVC resin, calcium zinc heat stabilizer, polyol phosphate, N-phenylamino POSS, ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin, and plasticize on a double-roll plasticizer at 160°C for 5 minutes. Then, hot press on a flat vulcanizer at 180°C and 15MPa for 10 minutes, cool to room temperature, demold, and cut.

[0082] Comparative Example 1:

[0083] The method is basically the same as Example 1, except that no polyol phosphate is added.

[0084] Comparative Example 2:

[0085] The method is substantially the same as Example 1, except that diisooctylphenyl phosphite (CAS: 522-21-1) is used instead of polyol phosphate.

[0086] Comparative Example 3:

[0087] The method is substantially the same as Example 1, except that trinonyl phosphite (CAS: 26569-53-9) is used instead of polyol phosphate.

[0088] Comparative Example 4:

[0089] The method is substantially the same as Example 1, except that trioctyl phosphite (CAS: 3028-88-4) is used instead of polyol phosphate.

[0090] Comparative Example 5:

[0091] The method is substantially the same as Example 1, except that octa-p-aminophenyl POSS is not added.

[0092] Comparative Example 6:

[0093] The method is substantially the same as Example 1, except that octa-p-aminophenyl POSS is replaced by octa-epoxysilsesquioxane (CAS: 68611-45-0).

[0094] Performance Test:

[0095] The automobile interior materials in Examples 1-5 and Comparative Examples 1-6 were respectively made into corresponding samples for performance testing.

[0096] The thermal stability test was carried out according to the GB / T 2917.1-2002 method, and the time it took for the Congo red test paper to turn blue was used to characterize the thermal stability.

[0097] The notched impact strength of the sample was tested using a simply supported beam impact tester in accordance with GB / T 1043-1993, and the tensile properties of the sample were tested using an electronic tensile testing machine in accordance with GBT 1040.1-2018, with a tensile speed of 50 mm / min and a test temperature of 23°C;

[0098] Aging resistance test method: Place the sample in a heat aging test oven and heat it at 120°C in air to test the notched impact strength and tensile strength. The test time is 144 hours. After the test, calculate the decline rate of related mechanical properties.

[0099] The test results are shown in Table 1 below:

[0100] Table 1:

[0101]

[0102] It can be seen from Table 1 above that the automotive interior material prepared by the present invention has good thermal stability and mechanical properties, and excellent heat aging resistance.

[0103] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An automobile interior material, characterized in that: Including PVC resin and composite heat stabilizer; The composite heat stabilizer comprises a calcium zinc heat stabilizer, a polyol phosphate ester and an amino POSS.

2. The automotive interior material according to claim 1, characterized in that: The mass ratio of the PVC resin to the composite heat stabilizer is 20-40:

1.

3. The automotive interior material according to claim 1, characterized in that: The mass ratio of the calcium zinc heat stabilizer, the polyol phosphate and the amino POSS is 1-5:1-5:1-5.

4. The automotive interior material according to claim 1, characterized in that: The structural formula of the polyol phosphate is shown below: Wherein, R1 and R2 are each independently a C1-C10 alkyl group or a C6-C30 aromatic group.

5. The automotive interior material according to claim 4, characterized in that: R1 and R2 are each independently a C6-C10 alkyl group, a phenyl group, or a biphenyl group.

6. The automotive interior material according to claim 1, characterized in that: The polyol phosphate is any one or more combinations of the following compounds:

7. The automotive interior material according to claim 1, characterized in that: The amino POSS is octa-p-aminophenyl POSS and / or N-phenylamino POSS.

8. The automotive interior material according to any one of claims 1 to 7, characterized in that: It also includes ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin.

9. A method for preparing an automobile interior material according to claim 8, characterized in that: PVC resin, composite heat stabilizer, ACR, CPE, heavy calcium carbonate, titanium dioxide, polyethylene wax and paraffin are mixed and plasticized on a double-roll plasticizer, and then hot-pressed on a flat vulcanizer before demoulding and cutting.

10. The method for preparing the automotive interior material according to claim 9, characterized in that: The hot pressing temperature is 170-190°C, the hot pressing pressure is 5-15MPa, and the hot pressing time is 5-10min.

Citation Information

Patent Citations

  • Preparation method of PVC (polyvinyl chloride) composition

    CN102604256A

  • Transparent and environment-friendly POSS (Polyhedral Oligomeric Silsesquioxane) modified calcium-zinc stabilizer and preparation method thereof

    CN106189244A

  • Polyvinyl chloride composite material and preparation method and application thereof

    CN109337235A

  • Polyurea resin waterproofing materials and manufacturing method thereof, the waterproof coating method using the same

    KR101974533B1