Patterned decorative film coating liquid formula and application thereof

By using reactive photoisomeristic chiral molecules and photoinitiators in the patterned decorative film coating liquid, liquid crystal molecules are induced to form a helical structure and lock the helical structure, which solves the high color saturation and inaccurate color expression in the prior art. The problem of this has achieved a wider color gamut range and more harmonious tone matching, improving the pattern quality and visual effect experience.

CN119081458APending Publication Date: 2024-12-06SICHUAN LONGHUA FILM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411406348.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing patterned decorative films have problems such as excessive color saturation and inaccurate color expression in the mobile phone back cover decoration, resulting in visual fatigue and poor visual effect experience, and it is impossible to achieve a wider color gamut range and a more harmonious tone matching.

Method used

Reactive photoisomerized chiral molecules are used as chiral agents, combined with liquid crystal monomers, photoinitiators and additives, and patterned decorative film coating liquid is prepared by uniformly dispersing it in the solvent, and photoisomerized chiral The reactive nature of the molecule induces the liquid crystal molecules to form a helical structure, and photocures with photoinitiators to lock the helical structure to achieve the expression of colorful colors.

Benefits of technology

The light, thermal stability and chemical stability of the liquid crystal film are improved, the color gamut range is expanded, more harmonious color matching is achieved, pattern quality and visual effect experience are improved, and the problem of poor visual effect experience in the existing technology is solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081458A_ABST
    Figure CN119081458A_ABST
Patent Text Reader

Abstract

The invention discloses a patterned decorative film coating liquid formula and application thereof, and belongs to the technical field of liquid crystal films, the formula comprises the following components by weight: 21-32 parts of a liquid crystal monomer, 1-3 parts of a chiral agent, 1-2 parts of a photoinitiator, 0.1-0.2 part of an auxiliary agent, and 35-85 parts of a solvent. According to the invention, the reactive photoisomeric chiral molecules are adopted as the chiral agent, and are uniformly dispersed in the solvent together with the liquid crystal monomer, the photoinitiator, the auxiliary agent and the like, so that the stability of a liquid crystal system can be improved, and the liquid crystal film which is more stable in performance, resistant to temperature change in color and better in durability can be prepared through subsequent processing; the problem that an existing mobile phone rear cover decorative film is single in aesthetic appreciation is solved, the pattern color gamut range is wide, color matching is more harmonious, the film can be widely applied to 3C rear covers of electronic equipment, and technical processing of downstream products is better facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention discloses a patterned decorative film coating liquid formula and its application, and specifically relates to a patterned decorative film coating liquid formula for 3C back cover, the application of the coating liquid formula in the preparation of 3C back cover, and a composite color decorative film with high-quality patterned effect prepared by coating the coating liquid formula, belonging to the field of liquid crystal film technology. Background Art

[0002] Mobile phones are the most frequently used electronic products in people's daily lives. In recent years, the configuration and performance of mobile phones of the same price have not differed much, and the homogeneity of appearance design has also been more prominent. In the absence of major breakthroughs in screen form, manufacturers have spared no effort in the decoration of mobile phone back covers. The core of mobile phone back cover decoration has evolved from single color, gradient color to transparent back cover, to electrochromic and even the latest photochromic, and the control of color and the pursuit of effect have gradually become mature. However, mobile phones with solid color back covers, gradient color back covers and even transparent back covers are inevitably prone to visual fatigue after being widely used in the market. Therefore, patterned decoration can be achieved through color selection and matching to meet people's diverse aesthetic needs.

[0003] Chinese patent CN112321872A discloses a color optical film and its preparation method, as well as Chinese patent CN114507473A discloses a colorful coating liquid, a colorful hardened film using the colorful coating liquid and its preparation method. The colorful hardened film involved in the colorful hardened film utilizes the principle of light interference. Under the irradiation of light, the refraction and interference between the layers cause the color changes between multiple layers and multiple angles. It can be transformed at different distances, different angles and different substrates to present different fantasy color effects, but the color is single under the same conditions; the colorful optical film involved in the colorful hardened film induces the polymerizable liquid crystal monomer to transform from the nematic phase to the cholesteric phase through a chiral agent, and changes the pitch of the cholesteric phase liquid crystal by the type and amount of the chiral agent. Finally, after the cholesteric phase liquid crystal is coated into a film, a bright color is observed. It can be seen that the above-mentioned colorful optical film and colorful hardened film can only express the color of a single band under specific formulas and processes, and cannot achieve the simultaneous expression of specific pattern shapes and colorful colors.

[0004] Different from the above-mentioned color optical films and colorful hardened films, patterned decorative films can realize the flexible application of various color patterns, including the presentation of any combination of specified shapes and colors. However, existing patterned decorative films often have problems such as excessive color saturation and inaccurate color expression. The strong expression of the picture can easily cause visual fatigue to the eyes and bring a bad visual experience. Therefore, it is more commercially valuable to provide a patterned decorative film with a wider color gamut and more harmonious color matching to express higher pattern quality.

[0005] In the prior art, Chinese patent CN114573599A discloses a photoisomerization chiral molecule and its application in realizing patterning of color liquid crystal film, wherein the competition between photoisomerization and photoinitiated polymerization is utilized for the first time to realize patterning of color liquid crystal film, and the performance of photoisomerization liquid crystal film can be made stable. However, the color liquid crystal film provided by the patent still has the problem of poor visual experience, which is caused by the structure of the photoisomerization chiral molecule, and the coating liquid formula also has objective limitations. Therefore, in the process of film formation by the coating process, it is difficult to accurately control the photoisomerization and curing degree of the film, and it is impossible to lock two or more helical structures, so that it is ultimately unable to express a wider color gamut range and more harmonious color matching in a stable state, resulting in poor pattern quality and poor visual experience. Summary of the invention

[0006] The purpose of the present invention is to provide a patterned decorative film coating liquid formula, which uses reactive photoisomerizable chiral molecules as chiral agents, and can improve the stability of the liquid crystal system by uniformly dispersing them in a solvent with liquid crystal monomers, photoinitiators, additives, etc., which is conducive to the subsequent processing to obtain a liquid crystal film with more stable performance, color temperature resistance, and better durability. At the same time, it solves the problem of the single aesthetic of the existing mobile phone back cover decorative film, and the pattern color gamut range is wide, and the color matching is more harmonious. At the same time, the present invention also provides the use of the patterned decorative film coating liquid formula in the preparation of 3C back covers, and a composite color decorative film prepared by the patterned decorative film coating liquid formula.

[0007] The present invention is achieved by the following technical scheme: a patterned decorative film coating liquid formula, comprising the following components in parts by weight: 21 to 32 parts of liquid crystal monomer, 1 to 3 parts of chiral agent, 1 to 2 parts of photoinitiator, 0.1 to 0.2 parts of auxiliary agent, and 35 to 85 parts of solvent,

[0008] The chiral agent is a photoisomerizable chiral molecule represented by the following formula (1):

[0009]

[0010] Wherein, R is hydrogen, methyl, ethyl or alkoxy;

[0011] R1 is hydrogen, methyl, ethyl, acetyl or alkoxy;

[0012] n is any integer from 1 to 6;

[0013] M* represents a chiral unit, and the chiral unit is selected from one of isosorbide, binaphthyl, cholesterol, menthol or 2-(4, n-propyl)cyclohexyl.

[0014] The structure of the chiral unit is shown in the following formula (2) or (3):

[0015]

[0016] The liquid crystal monomer is selected from 2-methyl-1,4-phenylenebis(4-(((4-(acryloyloxy)butoxy)carbonyl)oxy)benzoate), 1,4-bis-[4-(3-acryloyloxypropoxy)benzoyloxy]-2-methylbenzene, 4-cyano-4'-pentylbiphenyl, 2-fluoro-4-[4-(4-propylphenyl)phenyl]benzonitrile, 4"-ethyl-2'-fluoro-4-propylterphenyl, 4-[(trans-4-butylcyclohexyl)methoxy]-4-ethoxy-2,2',3,3'-tetrafluoro-1,1'-biphenyl, 2,6-difluoro-4-(5-propyl-2-pyrimidinyl)benzonitrile,

[0017] One or more of 1-methoxy-4-[trans-4-[(1E)-2-[trans-4-(1E)-1-propen-1-ylcyclohexyl]vinyl]cyclohexyl]benzene and 1,1'-(1,2-ethynediyl)bis[4-(3-buten-1-yl)benzene].

[0018] The photoinitiator is selected from one or more of 2-hydroxy-methylphenylpropane-1-one, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 4-dimethylamino-benzoic acid ethyl ester, 2-isopropylthioxanthone, 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinephenyl)-1-butanone, 2,4-diethylthiazolone, methyl benzoylformate, 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl)butanone and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.

[0019] The auxiliary agent is selected from one or more of a leveling agent, a defoaming agent, a wetting agent, a matting agent or an inhibitor.

[0020] Optionally, the leveling agent can be selected from one or more of polyether-modified polysiloxane, polyacrylate, polysiloxane-polyether copolymer, polyether-modified dimethylpolysiloxane copolymer or acrylated polysiloxane; the defoaming agent can be selected from one or more of modified polysiloxane, non-silicone polymer, polyether-modified dimethylpolysiloxane copolymer, non-silicone polymer or other organic polymer; the wetting agent can be selected from one or more of polyurethane derivatives, polyacrylate, copolymer containing acidic groups or a mixture of electrically neutral polyamide and polyester.

[0021] The solvent is selected from one or more of ethyl acetate, 2-pentanone and cyclohexanone.

[0022] For example, the above-mentioned patterned decorative film coating liquid formula is used in the preparation of 3C back covers. The preparation is a process in which the coating liquid prepared by the patterned decorative film coating liquid formula is applied to the back of the patterned template, and then dried, LED irradiated, and UV cured to obtain a composite color decorative film.

[0023] During the preparation process, liquid crystal monomers and chiral agents are first added to the solvent, and dispersed at a speed of 500-700 rpm for 50-70 minutes at 35°C. After the solution is cooled to below 25°C, photoinitiators and auxiliary agents are added, and dispersed at a speed of 500-700 rpm for 30-40 minutes to obtain a patterned decorative film coating liquid. The patterned decorative film coating liquid is then coated on the back of a special patterned template by a wire rod or other means, and then sent to an oven for drying, with the temperature controlled at 80-100°C and the drying time being 1-3 minutes. After the solvent is dried, an LED is used to irradiate the film surface, and the irradiation light intensity is greater than 60mw / cm 2 In the process, the irradiation time is adjusted according to the required different wavelengths (such as 1s, 2s, etc.), and finally the mercury lamp is used for curing, and the light intensity is controlled to be > 50mw / cm 2 , energy>100mj / cm 2 , and finally the desired patterned decorative film is obtained.

[0024] The patterned decorative film obtained by the above preparation process meets the following performance indicators: The patterned decorative film meets the following performance indicators:

[0025] Temperature resistance: -20~+80℃;

[0026] Heat and humidity resistance: ≥98℃ (100%RH).

[0027] The 3C back cover includes the back covers of mobile phones, computers, tablets and other electronic devices.

[0028] Furthermore, the present invention also provides a composite color decorative film prepared according to the above-mentioned patterned decorative film coating liquid formula, specifically, the coating liquid prepared by the patterned decorative film coating liquid formula is applied to the back of the patterned template, and then dried, LED irradiated, and UV cured to obtain the composite color decorative film.

[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0030] (1) The formulation of the present invention can induce liquid crystal molecules to form a spiral arrangement by selecting photoisomerizable chiral molecules of specific structure, so that the liquid crystal material has unique optical properties. Since the end group of the photoisomerizable chiral molecule is an acrylate group, it has better compatibility with the main liquid crystal and is reactive, so that its induced pitch P has a smaller temperature dependence. Therefore, after curing into a film, its color expression has better light, thermal and chemical stability, and the overall color can be colorful.

[0031] (2) The formula of the present invention selects a specific chiral agent to cooperate with the liquid crystal monomer, and utilizes the special reactivity of the chiral agent to improve the stability of the liquid crystal system. While inducing the liquid crystal molecules to form a helical structure, it can also participate in the polymerization of liquid crystal molecules under the action of a photoinitiator, and gradually become a component of the liquid crystal system from a free state molecule, making the performance of the liquid crystal film more stable, which is conducive to subsequent processing, and the color temperature change resistance and durability are also better, simplifying the supporting production process.

[0032] (3) The present invention can use a specially made patterned template to provide directional light stimulation to the liquid crystal matrix. When LED light of a specific wavelength irradiates the liquid crystal matrix from the back from top to bottom, a light intensity distribution corresponding to the grayscale resolution of the template pattern is generated inside, thereby bringing about a difference in the degree of isomerization and ultimately leading to a specific distribution of the helical structure. This structure can be locked in the subsequent photocuring process, thereby obtaining a colored patterned film, i.e., a composite color decorative film.

[0033] (4) In the formulation of the present invention, by selecting a specific liquid crystal monomer and a chiral agent, the formation and curing of the liquid crystal spiral structure in the film layer can be carried out simultaneously under the action of the photoinitiator. In the sequential drying, LED irradiation, and UV irradiation stages, the film has an adjustable periodic spiral structure and degree of curing, and ultimately two or more spiral structures can be locked to exhibit a composite color.

[0034] (5) In the composite color decorative film prepared by the present invention, the spectrum of the composite color corresponds to two or more central wavelengths of reflected light, and the corresponding reflectivity is more dispersed than that of a single color, so the color saturation is also lower. A wider color gamut can be obtained under modulation of different proportions, so that the decorative film has a more harmonious color tone combination.

[0035] In summary, the present invention solves the problem of the single aesthetic of the existing mobile phone back cover decorative film, and provides an efficient, flexible and extensive patterned decorative film coating liquid. Due to the reasonable selection of the coating liquid formula, the stability of the liquid crystal system is better, the yield rate of the coated composite color decorative film is higher, the pattern color has better resistance to temperature change and durability, and can be widely used in 3C back covers of electronic equipment, making it more conducive to the technical processing of downstream products. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a picture of composite color decorative film Ⅰ.

[0037] Figure 2 This is a picture of composite color decorative film II.

[0038] Figure 3 This is a picture of composite color decorative film III.

[0039] Figure 4 This is a picture of composite color decorative film IV.

[0040] Figure 5 This is a picture of patterned decorative film 1#.

[0041] Figure 6 This is a picture of patterned decorative film 2#.

[0042] Figure 7 It is the selection of corresponding color blocks on the composite color decorative film Ⅰ and pattern decorative film 1#.

[0043] Figure 8 for Figure 7 Spectral curve of the color block selected in A.

[0044] Fig. 9 for Figure 7 Spectral curve of the color block selected in B. DETAILED DESCRIPTION

[0045] The invention objectives, technical solutions and beneficial effects of the present invention are further described in detail below.

[0046] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the claimed invention, and unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.

[0047] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0048] In the following embodiments, liquid crystal monomer 1 is 2-methyl-1,4-phenylenebis(4-(((4-(acryloyloxy)butoxy)carbonyl)oxy)benzoate), liquid crystal monomer 2 is 1,4-bis-[4-(3-acryloyloxypropoxy)benzoyloxy]-2-methylbenzene, and UB-43048 is a polyether-modified polysiloxane, a leveling agent.

[0049] Embodiment 1:

[0050] Take 30 parts of liquid crystal monomer 1, 2 parts of liquid crystal monomer 2, 1 part of photosensitizing chiral agent, 1.5 parts of 1-hydroxycyclohexyl phenyl ketone and 0.1 parts of UB-43048, and use ethyl acetate, 2-pentanone and cyclohexanone in a mass ratio of 1:2:3.5 as solvent.

[0051] The structure of the photosensitizer is shown in the following formula (1):

[0052]

[0053] Wherein, R is a methyl group; R1 is an acetyl group; n is 6; and the structure of M* is shown in the following formula (2):

[0054]

[0055] A liquid crystal coating liquid was prepared according to the above raw material formula: ethyl acetate, 2-pentanone and cyclohexanone were added to a dispersion kettle, and the pneumatic motor was turned on to keep the solvent in a rotating state. After 20 minutes, liquid crystal monomer 1, liquid crystal monomer 2 and a photosensitive chiral agent were added to the kettle, and then the oil bath heater valve of the dispersion kettle was opened to heat the solution in the kettle with heat-conducting oil. After the temperature in the kettle reached 35° C., the heating state was maintained and the solution in the kettle was dispersed at a speed of 500 rpm. After dispersing for 70 minutes, stirring was stopped, and the solution in the kettle was cooled to below 25° C., and then 1-hydroxycyclohexyl phenyl ketone and UB-43048 were added, and the solution in the kettle was continued to be dispersed at a speed of 500 rpm for 40 minutes to obtain a liquid crystal coating liquid with a solid content of 29.05%.

[0056] The liquid crystal coating liquid is coated on the surface of the PET film with a wire rod, and then sent to the oven for drying. The drying temperature of the oven is controlled to be 90°C, and the drying time is about 2 minutes. After the solvent is dried, the film surface is irradiated with LED, and the irradiation intensity is about 60mw / cm 2 The exposure time is 2s, and then the mercury lamp is used for curing, and the light intensity is about 55mw / cm 2 , energy about 100mj / cm 2 , a composite color decorative film Ⅰ is obtained, such as Figure 1 shown.

[0057] Embodiment 2:

[0058] Take 20 parts of liquid crystal monomer 1, 1 part of liquid crystal monomer 2, 3 parts of photosensitive chiral agent, 1 part of 2-hydroxy-methylphenylpropane-1-one and 0.1 part of UB-43048, and use ethyl acetate, 2-pentanone and cyclohexanone in a mass ratio of 1:2.5:3 as solvent.

[0059] The structure of the photosensitizer is shown in the following formula (1):

[0060]

[0061] Wherein, R is an alkoxy group; R1 is an alkoxy group; n is 4; and the structure of M* is shown in the following formula (3):

[0062]

[0063] A liquid crystal coating liquid was prepared according to the above raw material formula: ethyl acetate, 2-pentanone and cyclohexanone were added to a dispersion kettle, and the pneumatic motor was turned on to keep the solvent in a rotating state. After 15 minutes, liquid crystal monomer 1, liquid crystal monomer 2 and a photosensitive chiral agent were added to the kettle, and then the oil bath heater valve of the dispersion kettle was opened to heat the solution in the kettle with heat-conducting oil. After the temperature in the kettle reached 35° C., the heating state was maintained and the solution in the kettle was dispersed at a speed of 700 rpm. After dispersing for 50 minutes, stirring was stopped, and the solution in the kettle was cooled to below 25° C., and then 2-hydroxy-methylphenylpropane-1-one and UB-43048 were added, and the solution in the kettle was continued to be dispersed at a speed of 700 rpm for 30 minutes to obtain a liquid crystal coating liquid with a solid content of 27.75%.

[0064] The liquid crystal coating liquid is coated on the surface of the PET film with a wire rod, and then sent to the oven for drying. The drying temperature of the oven is controlled to be 80°C, and the drying time is about 3 minutes. After the solvent is dried, the film surface is irradiated with LED, and the irradiation intensity is about 60mw / cm 2 The exposure time is 2s, and then the mercury lamp is used for curing, and the light intensity is about 55mw / cm 2 , energy about 100mj / cm 2 , a composite color decorative film II is obtained, such as Figure 2 shown.

[0065] Embodiment 3:

[0066] Take 25 parts of liquid crystal monomer 1, 1 part of liquid crystal monomer 2, 2 parts of photosensitive chiral agent, 1.5 parts of 2,4-diethylthiazolone and 0.15 parts of UB-43048, and use ethyl acetate, 2-pentanone and cyclohexanone in a mass ratio of 1:2:4 as solvent.

[0067] The structure of the photosensitizer is shown in the following formula (1):

[0068]

[0069] Wherein, R is ethyl; R1 is ethyl; n is 5; and the structure of M* is shown in the following formula (2):

[0070]

[0071] A liquid crystal coating liquid was prepared according to the above raw material formula: ethyl acetate, 2-pentanone and cyclohexanone were added to a dispersion kettle, and the pneumatic motor was turned on to keep the solvent in a rotating state. After 15 minutes, liquid crystal monomer 1, liquid crystal monomer 2 and a photosensitive chiral agent were added to the kettle, and then the oil bath heater valve of the dispersion kettle was opened to heat the solution in the kettle with heat-conducting oil. After the temperature in the kettle reached 35° C., the heating state was maintained and the solution in the kettle was dispersed at a speed of 600 rpm. After dispersing for 55 minutes, stirring was stopped, and the solution in the kettle was cooled to below 25° C., and then 2,4-diethylthiazolone and UB-43048 were added, and the solution in the kettle was continued to be dispersed at a speed of 600 rpm for 35 minutes to obtain a liquid crystal coating liquid with a solid content of 29.75%.

[0072] The liquid crystal coating liquid is coated on the surface of the PET film with a wire rod, and then sent to the oven for drying. The drying temperature of the oven is controlled to be 95°C, and the drying time is about 2 minutes. After the solvent is dried, the film surface is irradiated with LED, and the irradiation intensity is about 60mw / cm 2 The irradiation time is 3s, and then mercury lamp is used for curing, the light intensity is about 55mw / cm2, the energy is about 100mj / cm2, and the composite color decorative film III is obtained. Figure 3 shown.

[0073] Embodiment 4:

[0074] Take 22 parts of liquid crystal monomer 1, 2 parts of liquid crystal monomer 2, 1.5 parts of photosensitizing chiral agent, 1 part of 2-hydroxy-methylphenylpropane-1-one and 0.15 parts of UB-43048, and use ethyl acetate, 2-pentanone and cyclohexanone in a mass ratio of 1:2:2.3 as solvent.

[0075] The structure of the photosensitizer is shown in the following formula (1):

[0076]

[0077] Wherein, R is hydrogen; R1 is hydrogen; n is 6; and the structure of M* is shown in the following formula (3):

[0078]

[0079] A liquid crystal coating liquid was prepared according to the above raw material formula: ethyl acetate, 2-pentanone and cyclohexanone were added to a dispersion kettle, and the pneumatic motor was turned on to keep the solvent in a rotating state. After 20 minutes, liquid crystal monomer 1, liquid crystal monomer 2 and a photosensitive chiral agent were added to the kettle, and then the oil bath heater valve of the dispersion kettle was opened to heat the solution in the kettle with heat-conducting oil. After the temperature in the kettle reached 35° C., the heating state was maintained and the solution in the kettle was dispersed at a speed of 650 rpm. After dispersing for 60 minutes, stirring was stopped, and the solution in the kettle was cooled to below 25° C., and then 2-hydroxy-methylphenylpropane-1-one and UB-43048 were added, and the solution in the kettle was continued to be dispersed at a speed of 650 rpm for 40 minutes to obtain a liquid crystal coating liquid with a solid content of 29.53%.

[0080] The liquid crystal coating liquid is coated on the surface of the PET film with a wire rod, and then sent to the oven for drying. The drying temperature of the oven is controlled to be 85°C, and the drying time is about 3 minutes. After the solvent is dried, the film surface is irradiated with LED, and the irradiation intensity is about 60mw / cm 2 The irradiation time is 3s, and then the mercury lamp is used for curing, and the light intensity is about 55mw / cm 2 , energy about 100mj / cm 2 , a composite color decorative film IV is obtained, such as Figure 4 shown.

[0081] Comparative Example 1:

[0082] The same preparation process and process as in Example 1 were used to prepare patterned decorative film 1# (see Figure 5 ), the only difference is that the formula of the liquid crystal coating liquid is slightly different. Specifically, the formula raw materials of the liquid crystal coating liquid of this comparative example are as follows:

[0083] 35 parts of liquid crystal monomer 1, 1 part of photosensitizing chiral agent, 2 parts of 1-hydroxycyclohexyl phenyl ketone and 0.1 part of UB-43048, and the solvent is ethyl acetate, 2-pentanone and cyclohexanone in a mass ratio of 5:1:4.

[0084] The structure of the photosensitizing chiral agent in the formula raw materials is shown in the following formula (4):

[0085]

[0086] Wherein R1, n and M* are the same as those in Example 1.

[0087] Comparative Example 2:

[0088] The same preparation process and process as in Example 1 were used to prepare patterned decorative film 2# (see Figure 6 ), the only difference is that the formula of the liquid crystal coating liquid is slightly different. Specifically, the formula raw materials of the liquid crystal coating liquid of this comparative example are as follows:

[0089] Take 20 parts of liquid crystal monomer 1, 20 parts of liquid crystal monomer 2, 3 parts of photosensitivity chiral agent (same as comparative example 1), 2 parts of 2-hydroxy-methylphenylpropane-1-one and 0.2 parts of UB-43048, and use ethyl acetate, 2-pentanone and cyclohexanone in a mass ratio of 1:2.5:3 as solvent.

[0090] The composite color decorative films I to IV prepared in the above-mentioned Examples 1 to 4 and the patterned decorative films 1# and 2# prepared in Comparative Examples 1 and 2 were compared as follows:

[0091] (1) Pattern color

[0092] See also Figures 1 to 6 It can be seen that Figures 1 to 4 The composite color decorative films I to IV shown are based on the comprehensive control of the composite ratio of liquid crystal monomers, the selection and dosage of photosensitive chiral agents, the dosage of initiators and the LED irradiation time, which affects the differences in the spectral curves of the composite color decorative films in terms of color bands, wavelength combinations and their proportions. Ultimately, they all present colors with relatively excellent visual effects and have different color styles.

[0093] Figure 5 and Figure 6 In the patterned decorative film 1# and patterned decorative film 2# shown, all color blocks are of a single color, the corresponding spectra are of a single peak, the reflectivity is relatively high, and the color gamut is not comprehensive enough, making the color performance not vivid enough.

[0094] It is known that the reflection wavelength of liquid crystal film materials is positively correlated with the arrangement period of their microstructure. When light is irradiated onto the film material, only light of a specific wavelength can be reflected from the material to form a color, which is commonly known as "structural color". Therefore, the spectrum curve can intuitively reflect the color gamut range and reflectivity of the film.

[0095] It should be noted that Figures 1 to 6 The same template is used in the preparation process, so the corresponding patterns are basically the same, but due to Figures 1 to 4 The color spectrum peak bands of the middle pattern are composed of two or more. Figure 5 and Figure 6 The color of the pattern in is unimodal, therefore, the two categories of pattern decorative films show different color expressions for the same pattern.

[0096] In order to prove that the composite color decorative film of the present invention has a wider color gamut and excellent color matching, the spectral curves of the corresponding color blocks in the composite color decorative film I and the pattern decorative film 1# of Example 1 and Comparative Example 1 are further compared, see Figure 7 As shown, Figure 7 A is the composite color decorative film I, and the spectral curve of the corresponding color block is as follows: Figure 8 As shown; Figure 7 B is the pattern decorative film 1#, and the spectral curve of the corresponding color block is as follows: Fig. 9 As shown, Fig. 9 The three spectral curves from left to right correspond to Figure 7 The three color blocks from top to bottom in middle B.

[0097] through Figure 8 and Fig. 9 From the comparison of the spectral curves, it can be seen that since the present invention can lock two or more spiral structures to show a composite color, its spectral curve corresponds to the superposition of two main reflected light center wavelengths (430nm and 580nm), and the corresponding reflectivity is also lower and more dispersed than that of a single color. Therefore, the color gamut presented in the composite color decorative film is wider, the saturation is lower, the visual effect is softer, and a wider color gamut can be obtained under modulation of different proportions, so that the decorative film has a more harmonious color combination and a stronger expressiveness.

[0098] (2) Stability

[0099] The composite color decorative film I prepared in Example 1 was taken as sample 1, and the patterned decorative film 1# prepared in Comparative Example 1 was taken as sample 2, and a color bleaching test was performed. The position of the central band of the spectral peak was used as an indicator to test the color change of the film before and after lamination and transfer, as well as during boiling and baking, and the corresponding test results were recorded. The results are shown in Tables 1 and 2 below.

[0100] Table 1 Color bleaching results of patterned decorative film of sample 1

[0101]

[0102] Table 2 Color bleaching results of patterned decorative film of sample 2

[0103]

[0104] As can be seen from Table 1 and Table 2, the performance of the composite color decorative film obtained by using the reactive photoisomerizable chiral molecule as a dopant in Example 1 of the present invention is more stable. By comparing the color changes before and after boiling and baking, it can be seen that the color drift corresponding to the photosensitive chiral agent in Example 1 is greatly reduced compared with the photosensitive chiral agent in Comparative Example 1 due to the use of the reactive photosensitive chiral agent, which indicates that the reactive photosensitive chiral agent participates in the liquid crystal system reaction to make the liquid crystal film more stable, and the temperature change resistance and humidity and heat resistance are greatly improved.

[0105] (3) Temperature resistance

[0106] Prepare the liquid crystal film test sample as required, and put the liquid crystal film sample in a -20℃ refrigerator. After 1 hour of treatment, put the sample in a +80℃ oven for 1 hour to complete a test cycle. The liquid crystal film sample surface is considered qualified if there are no defects such as bubbles, wrinkles, cracks, etc. and it meets the inspection standards. Focus on the changes in the color and adhesion of the liquid crystal film (inspection qualification standards: color drift ≤20nm, adhesion ≥4B).

[0107] The test results are shown in Table 3 below.

[0108] Table 3 Test results of liquid crystal film temperature resistance

[0109]

[0110] As can be seen from Table 3 above, Examples 1 to 4 of the present invention, due to the use of reactive photoisomerizable chiral molecules, are better than the qualified standard in terms of temperature resistance during the cycle from -20°C to +80°C, while Comparative Examples 1 and 2 are unqualified in terms of temperature resistance.

[0111] (4) Moisture and heat resistance

[0112] Prepare the liquid crystal film sample as required, and immerse the sample in a constant temperature water bath at 98℃, and take it out after immersion at this temperature for 1 hour. Evaluate the moisture and heat resistance of the liquid crystal film by the changes in color, hardness, adhesion, etc. before and after the test. Focus on the changes in color and adhesion of the liquid crystal film (inspection pass standard: color drift ≤20nm, adhesion ≥4B).

[0113] The test results are shown in Table 4 below.

[0114] Table 4 Test results of the moisture and heat resistance of liquid crystal films

[0115]

[0116] As can be seen from Table 4 above, after being immersed in a constant temperature water bath at 98°C for 1 hour, the moisture and heat resistance of different patterned decorative films was tested. Among them, the moisture and heat resistance of Examples 1 to 3 was qualified, and the moisture and heat resistance of Example 4, Comparative Example 1 and Comparative Example 2 was unqualified. Among them, the reason for the failure of Example 4 may be the different ratios of liquid crystal monomer 1 and liquid crystal monomer 2 and the changes in the ratios of components such as chiral agents and initiators, which may affect the crosslinking degree of the liquid crystal monomer after UV curing, the tightness of the film structure, and the adhesion performance with the substrate, etc., and affect the moisture and heat resistance. Therefore, in Example 4, due to the inappropriate formula ratio, the performance did not meet the standard, but in general, the patterned decorative film with reactive photoisomerizable chiral molecules added has better moisture and heat resistance.

[0117] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.

Claims

1. A patterned decorative film coating liquid formula, characterized in that: The invention comprises the following components in parts by weight: 21 to 32 parts of liquid crystal monomer, 1 to 3 parts of chiral agent, 1 to 2 parts of photoinitiator, 0.1 to 0.2 parts of auxiliary agent, and 35 to 85 parts of solvent. The chiral agent is a photoisomerizable chiral molecule represented by the following formula (1): Wherein, R is hydrogen, methyl, ethyl or alkoxy; R1 is hydrogen, methyl, ethyl, acetyl or alkoxy; n is any integer from 1 to 6; M* represents a chiral unit, and the chiral unit is selected from one of isosorbide, binaphthyl, cholesterol, menthol or 2-(4, n-propyl)cyclohexyl.

2. The patterned decorative film coating liquid formulation according to claim 1, characterized in that: The structure of the chiral unit is shown in the following formula (2) or (3):

3. The patterned decorative film coating liquid formulation according to claim 1, characterized in that: The liquid crystal monomer is selected from 2-methyl-1,4-phenylenebis(4-(((4-(acryloyloxy)butoxy)carbonyl)oxy)benzoate), 1,4-bis-[4-(3-acryloyloxypropoxy)benzoyloxy]-2-methylbenzene, 4-cyano-4'-pentylbiphenyl, 2-fluoro-4-[4-(4-propylphenyl)phenyl] benzonitrile, 4"-ethyl-2'-fluoro-4-propyl terphenyl, 4-[(trans-4-butylcyclohexyl)methoxy]-4-ethoxy-2,2',3,3'-tetrafluoro-1,1'-biphenyl, 2,6-difluoro-4-(5-propyl-2-pyrimidinyl)benzonitrile, 1-methoxy-4-[trans-4-[(1E)-2-[trans-4-(1E)-1-propen-1-ylcyclohexyl]vinyl]cyclohexyl]benzene and 1,1'-(1,2-ethynyl)bis(1,2-difluoro-4-(5-propyl-2-pyrimidinyl)benzonitrile [4-(3-buten-1-yl)benzene] or more.

4. The patterned decorative film coating liquid formulation according to claim 1, characterized in that: The photoinitiator is selected from one or more of 2-hydroxy-methylphenylpropane-1-one, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone, 4-dimethylamino-benzoic acid ethyl ester, 2-isopropylthioxanthone, 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinephenyl)-1-butanone, 2,4-diethylthiazolone, methyl benzoylformate, 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl)butanone and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide.

5. The patterned decorative film coating liquid formulation according to claim 1, characterized in that: The auxiliary agent is selected from one or more of a leveling agent, a defoaming agent, a wetting agent, a matting agent or an inhibitor.

6. The patterned decorative film coating liquid formulation according to claim 1, characterized in that: The solvent is selected from one or more of ethyl acetate, 2-pentanone and cyclohexanone.

7. Application of the patterned decorative film coating liquid formula according to any one of claims 1 to 6 in the preparation of 3C back covers, characterized in that: The preparation is a process of coating a coating liquid prepared by a patterned decorative film coating liquid formula on the back of a patterned template, and then drying, LED irradiation, and UV curing to obtain a composite color decorative film.

8. The use according to claim 7, characterized in that: The composite color decorative film meets the following performance indicators: Temperature resistance: -20~+80℃; Heat and humidity resistance: ≥98℃ (100%RH).

9. The use according to claim 7, characterized in that: The 3C back cover includes the back covers of mobile phones, computers, tablets and other electronic devices.

10. A composite color decorative film prepared by the patterned decorative film coating liquid formula according to any one of claims 1 to 6, characterized in that: The coating liquid prepared by the patterned decorative film coating liquid formula is applied to the back of the patterned template, and then dried, LED irradiated, and UV cured to obtain a composite color decorative film.

Citation Information

Patent Citations

  • Liquid crystal film and preparation method and application thereof

    CN114280860A

  • Photoisomeric chiral molecule and application thereof in realizing patterning of color liquid crystal film

    CN114573599A

  • Photoreactive chiral agent, liquid crystal composition, liquid crystal color filter, optical film, recording medium, and method for changing twist structure of liquid crystal

    JP2002080851A