Environment-friendly moisture-proof cigarette adhesive and preparation method thereof

By modifying bisaldehyde quaternary ammonium silicone and graft copolymerizing starch, environmentally friendly cigarette glue with waterproof, antibacterial and anti-mold properties was prepared, which solved the problem of insufficient moisture-proof performance of cigarette glue and achieved green and environmentally friendly industrial production and high-quality cigarette production.

CN119081603AActive Publication Date: 2024-12-06CHUZHOU GUANGWEI CHEM
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411421702.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06
Estimated Expiration
2044-10-12

AI Technical Summary

Technical Problem

The moisture-proof performance of existing cigarette glue is insufficient, and it cannot effectively prevent cigarette mold, affecting the quality and taste of cigarettes, and contains harmful substances such as formaldehyde and phthalate, making it difficult to meet the needs of modern high-speed cigarette machines.

Method used

By modifying starch with bisaldehyde quaternary ammonium silicone, forming a crosslinked structure, and grafting and copolymerizing with vinyl acetate, acrylic acid, etc., environmentally friendly cigarette glue with waterproof, antibacterial and anti-mold properties is prepared, avoiding harmful effects Use of substances.

Benefits of technology

It has achieved excellent moisture-proof and mildew-proof properties of cigarette glue, has good initial viscosity and adhesive strength, is suitable for industrial production, and does not contain formaldehyde and phthalate substances, and is green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005080999860000051
    Figure BDA0005080999860000051
  • Figure BDA0005080999860000061
    Figure BDA0005080999860000061
  • Figure BDA0005080999860000102
    Figure BDA0005080999860000102
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, and discloses an environment-friendly moisture-proof cigarette adhesive and a preparation method thereof.The environment-friendly moisture-proof cigarette adhesive is characterized in that 5-chlorovaleric acid, 3-dimethylamino acrolein and the like are used as raw materials, a synthesized dialdehyde quaternary ammonium salt organic silicon modifier can be subjected to aldol condensation reaction with starch, organic silicon and alkenyl double bonds are introduced, and graft copolymerization with vinyl acetate and acrylic acid is conducted; the dialdehyde quaternary ammonium salt organic silicon modifier enables a plurality of starch molecules to be crosslinked together to form a spatial network structure, so that the combination of hydroxyl of the starch and water molecules is hindered, and the hydrophobic property of the starch is improved; quaternary ammonium salt can change the permeability of bacterial cell membranes and influence cell transfer activity and energy metabolism, so that cell death is caused; the cigarette adhesive prepared by the invention takes green and environment-friendly starch as a main material, has moisture-proof and mildew-proof properties, has excellent initial viscosity and adhesive strength, and is simple in preparation method and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, in particular to an environmentally friendly moisture-proof cigarette adhesive and a preparation method thereof. Background Art

[0002] Cigarette glue refers to a glue-like substance used in the cigarette production process, which is mainly used for cigarette rolling, cigarette filter connection, cigarette box and strip box packaging, cigarette box packaging and bonding in the filter rod production process. Therefore, the quality of cigarette glue greatly affects the quality level of cigarettes. As high-speed cigarette machines make cigarettes faster and faster, the quality of cigarettes continues to improve. At the same time, higher requirements are placed on the initial viscosity, fluidity, film-forming properties, quick-drying properties, stability and safety of cigarette glue. The original cigarette glue is no longer suitable for the needs of the development of the cigarette industry, and the price of imported high-speed cigarette glue is too high. The moisture-proof performance of some existing cigarette glues is insufficient, which makes cigarettes easily affected by moisture during storage and transportation. Cigarette glue with poor moisture-proof performance cannot effectively prevent cigarettes from mildewing, which in turn affects the quality and taste of cigarettes. Therefore, preparing a moisture-proof and mildew-proof environmentally friendly cigarette glue has become a problem that needs to be solved urgently.

[0003] At present, the cigarette glues used by domestic cigarette factories mainly include plant-based natural polymer adhesives such as starch adhesives, which can be used for cigarettes and packaging, have a wide range of uses, are cheap, non-toxic and tasteless, but starch contains more hydroxyl groups, which are easily combined with water in the form of hydrogen bonds, have low initial viscosity, slow drying speed, poor water resistance, and are prone to mildew, making them difficult to adapt to the continuous industrial production of high-speed cigarette machines; chemical synthetic adhesives are mainly polyvinyl alcohol and polyvinyl acetate emulsions. This type of adhesive has good adhesion, but poor water resistance, high glass transition temperature, and poor adhesion to complex printed packaging materials, which cannot meet the operating requirements of modern high-speed cigarette machines, and the resulting glue is expensive and has low safety.

[0004] Yang Limin mentioned in the article "Research and Development of Corn Starch Modified High-Speed ​​Cigarette Adhesive" that corn starch is oxidized with sodium hypochlorite and borax, then grafted with PVA, then an emulsifier is added for emulsification reaction, and monomers and initiators are added, the reaction is kept warm, and finally filtered to obtain cigarette adhesive; but this method still mainly uses polyvinyl acetate, and the starch content is only 5-15%, which is not a real starch cigarette adhesive. In addition, the residual monomer content of the adhesive is only less than 0.5%, which is far from meeting the current health and safety standards; Patent No. CN110003817A discloses a starch-type cigarette adhesive and a preparation method thereof, including starch raw materials, water-blocking additives, curing accelerators, palatability additives, and antibacterial active agents. The starch is debranched and modified, the branched starch is pretreated, and then acetylated with acetic anhydride to replace the starch. The preparation process is complicated, and it is also necessary to introduce natural antibacterial active agents to prevent the starch adhesive from mildewing, which is not suitable for industrial production.

[0005] In view of the above reasons, the present invention first prepares a dialdehyde cross-linking agent with both waterproof and antibacterial functions, cross-links and modifies the hydroxyl groups of starch, and then grafts vinyl acetate, acrylic acid, etc. with starch through initiation polymerization to form a dense cross-linked network structure. The structure does not contain harmful substances such as formaldehyde and phthalates, and is green and environmentally friendly. Summary of the invention

[0006] The purpose of the present invention is to solve the problems existing in the above-mentioned prior art and to provide an environmentally friendly moisture-proof cigarette glue and a preparation method thereof, which not only has excellent moisture-proof and waterproof properties, but also has antibacterial and mildew-proof effects, and does not contain harmful substances such as formaldehyde and phthalates, and is green and environmentally friendly.

[0007] The present invention is achieved through the following technical solutions:

[0008] A method for preparing an environmentally friendly moisture-proof cigarette adhesive comprises the following steps:

[0009] Step (1), under nitrogen atmosphere, add starch and deionized water to a reaction flask, stir evenly, and then add The dialdehyde quaternary ammonium salt organic silicon modifier is added and stirred for reaction. After the reaction is completed, the pH is adjusted to neutral, and the emulsion is dehydrated, washed, and dried to obtain cross-linked starch.

[0010] Step (2), under a nitrogen atmosphere, add deionized water to a reaction flask, wait until the temperature rises to 40-50° C., add cross-linked starch, stir evenly, heat to 70-90° C., add acrylic acid, vinyl acetate, initiator and composite emulsifier, continue to react for 1-2 hours, cool to 50-60° C., add 20-30% by mass polyvinyl alcohol aqueous solution, adjust the pH to 5-6 with sodium carbonate aqueous solution, cool to below 40° C., filter the material, and obtain an environmentally friendly moisture-proof cigarette adhesive.

[0011] In step (1), the starch is any one of corn starch, tapioca starch or potato starch.

[0012] In step (2), the initiator is any one of ammonium persulfate, potassium persulfate or hydrogen peroxide.

[0013] Furthermore, in step (1), the ratio of starch to dialdehyde quaternary ammonium salt organosilicon modifier is 100g:(5-25)g.

[0014] Furthermore, in step (1), the reaction temperature is 65-80° C. and the reaction time is 2-5 h.

[0015] Furthermore, in step (2), the composite emulsifier is prepared by mixing sodium dodecyl sulfate and octylphenol polyoxyethylene ether in a mass ratio of 1:2.

[0016] Furthermore, in step (2), the ratio of cross-linked starch, acrylic acid, vinyl acetate, initiator, composite emulsifier and polyvinyl alcohol aqueous solution is 100g:(5-10)g:(8-15)g:(0.3-0.8)g:(2-3.5)g:(12-20)g.

[0017] Furthermore, the preparation method of the dialdehyde quaternary ammonium salt organosilicon modifier in step (1) comprises the following steps:

[0018] Step S1, under a nitrogen atmosphere, add 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 5-chlorovaleric acid and dichloromethane to a reaction flask, stir evenly, add 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine, react at 20-35° C. for 12-24 h, extract with deionized water and ethyl acetate, concentrate the organic phase, and purify by column chromatography to obtain a dichloro long-chain organosilicon intermediate.

[0019] Step S2, under a nitrogen atmosphere, add a dichloro long-chain organosilicon intermediate and N,N-dimethylformamide to a reaction flask, stir evenly, add 3-dimethylaminoacrolein, stir to react, and after the reaction is completed, concentrate under reduced pressure to obtain a crude product, dissolve the crude product in methanol, add chloroform to precipitate, filter, wash with deionized water, and dry to obtain a dialdehyde quaternary ammonium salt organosilicon modifier.

[0020] Furthermore, in step S1, the ratio of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 5-chlorovaleric acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole, and triethylamine is 1 mol:(2.05-2.2) mol:(2.5-3.5) mol:(2.8-4.2) mol:(4-6) mol.

[0021] Furthermore, in step S2, the ratio of the dichloro long-chain organosilicon intermediate to 3-dimethylaminoacrolein is 1 mol:(2.1-2.4) mol.

[0022] Furthermore, in step S2, the reaction temperature is 85-100° C., and the reaction time is 16-32 h.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The invention uses 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 5-chlorovaleric acid and 3-dimethylaminoacrolein as raw materials to synthesize a dialdehyde quaternary ammonium salt organosilicon modifier, treats starch to reduce residual hydroxyl groups in the starch, introduces organosilicon and alkenyl double bonds to facilitate graft copolymerization with vinyl acetate and acrylic acid, and uses a polyvinyl alcohol aqueous solution as an adhesive to obtain the dialdehyde quaternary ammonium salt organosilicon modifier.

[0025] The dialdehyde quaternary ammonium salt organosilicon modifier contains dialdehyde groups, which can react with the hydroxyl groups in starch to form an aldol condensation reaction, so that multiple starch molecules are cross-linked together to form a spatial network structure. At the same time, the olefin groups in its structure can initiate polymerization with vinyl acetate and acrylic acid, which is equivalent to bridging to form chemical bonds in the spatial network structure of cross-linked starch, thereby improving the density of the cross-linked structure. The introduction of hydrophobic long-chain alkyl groups can effectively increase the surface tension between starch and water molecules, hinder the combination of starch hydroxyl groups with water molecules, and improve the hydrophobic properties of starch. In addition, the surface energy of organosilicon molecules is low, and the hydrophobic groups such as methyl or other alkyl groups in the molecules are neatly arranged on the outside. When water vapor or raindrops in the air contact the surface of the organosilicon material, the hydrophobicity of the material surface can prevent external moisture from penetrating into the material, and the material has good moisture-proof properties.

[0026] The quaternary ammonium salt in the dialdehyde quaternary ammonium salt organosilicon modifier can reduce surface tension, can be adsorbed on the surface of bacteria, and inserted into the lipid layer of the bacterial cell membrane through its hydrophobic group, changing the permeability of the bacterial cell membrane, causing small molecular metabolites to overflow the cell, affecting the cell transmission activity and energy metabolism, thereby causing cell death; at the same time, after the dialdehyde quaternary ammonium salt organosilicon modifier undergoes aldol condensation with starch, the quaternary ammonium salt group with antibacterial properties is tightly embedded in the cigarette glue structure, and has anti-mildew and antibacterial long-lasting properties. The cigarette glue prepared by the present invention is mainly based on green and environmentally friendly starch, has both moisture-proof and anti-mildew properties, and has excellent initial viscosity and bonding strength, and the preparation method is simple and suitable for industrial production. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Unless otherwise specified, the raw materials and reagents used in this application are commercially available or can be prepared by known methods.

[0029] The composite emulsifier is prepared by mixing sodium lauryl sulfate and octylphenol polyoxyethylene ether in a mass ratio of 1:2.

[0030] 1,3-Bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, CAS number is 2469-55-8.

[0031] 5-Chlorovaleric acid, CAS number is 1119-46-6.

[0032] 1-Ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDCI), CAS number is 25952-53-8.

[0033] 1-Hydroxybenzotriazole (HOBt), CAS number is 2592-95-2.

[0034] 3-Dimethylaminoacrolein, CAS number is 927-63-9.

[0035] Example 1

[0036] (1) Under nitrogen atmosphere, 25 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 54 mmol of 5-chlorovaleric acid and 200 mL of dichloromethane were added to the reaction flask, and after stirring evenly, 75 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 90 mmol of 1-hydroxybenzotriazole and 125 mmol of triethylamine were added, and the mixture was reacted at 25° C. for 16 h, extracted with deionized water and ethyl acetate, and the organic phase was concentrated and purified by column chromatography (silica gel, 2-5% methanol in dichloromethane) to obtain a dichloro long-chain organosilicon intermediate. The preparation reaction formula is as follows:

[0037]

[0038] (2) Under nitrogen atmosphere, 18 mmol of dichloro long-chain organosilicon intermediate and 300 mL of N,N-dimethylformamide were added to the reaction flask, and after stirring, 40.5 mmol of 3-dimethylaminoacrolein was added, and the mixture was reacted at 90° C. for 24 h, and concentrated under reduced pressure to obtain a crude product. The crude product was dissolved in methanol, chloroform was added to precipitate, filtered, washed with deionized water, and dried to obtain a dialdehyde quaternary ammonium salt organosilicon modifier. The preparation reaction formula is as follows:

[0039]

[0040] (3) Under nitrogen atmosphere, 100 g corn starch and 2500 mL deionized water were added to a reaction flask, and after stirring, 5 g dialdehyde quaternary ammonium salt organosilicon modifier was added, and the mixture was reacted at 70° C. for 3 h. The pH was adjusted to neutral, and the emulsion was dehydrated, washed, and dried to obtain cross-linked starch.

[0041] (4) Under nitrogen atmosphere, deionized water was added to the reaction flask, and when the temperature rose to 45°C, 100 g of cross-linked starch was added, and after stirring evenly, the temperature was raised to 80°C, 8 g of acrylic acid, 12 g of vinyl acetate, 0.5 g of ammonium persulfate and 2.5 g of composite emulsifier were added, and the reaction was continued for 2 h. The temperature was lowered to 55°C, 15 g of 25% polyvinyl alcohol aqueous solution was added, the pH was adjusted to 5 with sodium carbonate aqueous solution, the temperature was lowered to below 40°C, and the material was filtered to obtain environmentally friendly moisture-proof cigarette adhesive.

[0042] Example 2

[0043] (1) Under nitrogen atmosphere, 120 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 246 mmol of 5-chlorovaleric acid and 600 mL of dichloromethane were added to a reaction flask, and after stirring evenly, 300 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 336 mmol of 1-hydroxybenzotriazole and 480 mmol of triethylamine were added, and the mixture was reacted at 35° C. for 12 h, extracted with deionized water and ethyl acetate, and the organic phase was concentrated and purified by column chromatography (silica gel, 2-5% methanol in dichloromethane) to obtain a dichloro long-chain organosilicon intermediate.

[0044] (2) Under nitrogen atmosphere, 105 mmol of dichloro long-chain organosilicon intermediate and 1260 mL of N,N-dimethylformamide were added to a reaction flask, stirred evenly, and then 220.5 mmol of 3-dimethylaminoacrolein was added. The mixture was reacted at 100 °C for 16 h, and concentrated under reduced pressure to obtain a crude product. The crude product was dissolved in methanol, chloroform was added for precipitation, filtered, washed with deionized water, and dried to obtain a dialdehyde quaternary ammonium salt organosilicon modifier.

[0045] (3) Under nitrogen atmosphere, 100 g of cassava starch and 2500 mL of deionized water were added to a reaction flask, and after stirring, 10 g of dialdehyde quaternary ammonium salt organosilicon modifier was added, and the mixture was reacted at 80 °C for 2 h. The pH was adjusted to neutral, and the emulsion was dehydrated, washed, and dried to obtain cross-linked starch.

[0046] (4) Under a nitrogen atmosphere, deionized water was added to a reaction flask. When the temperature was raised to 50°C, 100 g of cross-linked starch was added. After stirring, the temperature was raised to 90°C, 5 g of acrylic acid, 8 g of vinyl acetate, 0.3 g of potassium persulfate and 2 g of a composite emulsifier were added, and the reaction was continued for 1 h. The temperature was lowered to 60°C, 12 g of a 30% by mass polyvinyl alcohol aqueous solution was added, the pH was adjusted to 6 with a sodium carbonate aqueous solution, the temperature was lowered to below 40°C, and the material was filtered to obtain an environmentally friendly moisture-proof cigarette adhesive.

[0047] Example 3

[0048] (1) Under nitrogen atmosphere, 50 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 110 mmol of 5-chlorovaleric acid and 500 mL of dichloromethane were added to a reaction flask, and after stirring evenly, 175 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 210 mmol of 1-hydroxybenzotriazole and 300 mmol of triethylamine were added, and the mixture was reacted at 20° C. for 24 h, extracted with deionized water and ethyl acetate, and the organic phase was concentrated and purified by column chromatography (silica gel, 2-5% methanol in dichloromethane) to obtain a dichloro long-chain organosilicon intermediate.

[0049] (2) Under nitrogen atmosphere, 40 mmol of dichloro long-chain organosilicon intermediate and 800 mL of N,N-dimethylformamide were added to a reaction flask, and after stirring, 96 mmol of 3-dimethylaminoacrolein was added, and the mixture was reacted at 85° C. for 32 h. The crude product was concentrated under reduced pressure to obtain a crude product, which was dissolved in methanol, precipitated by adding chloroform, filtered, washed with deionized water, and dried to obtain a dialdehyde quaternary ammonium salt organosilicon modifier.

[0050] (3) Under nitrogen atmosphere, 100 g of potato starch and 2500 mL of deionized water were added to a reaction flask, and after stirring, 15 g of dialdehyde quaternary ammonium salt organosilicon modifier was added, and the mixture was reacted at 65° C. for 5 h. The pH was adjusted to neutral, and the emulsion was dehydrated, washed, and dried to obtain cross-linked starch.

[0051] (4) Under nitrogen atmosphere, deionized water was added to the reaction flask, and when the temperature was raised to 40°C, 100 g of cross-linked starch was added, and after stirring evenly, the temperature was raised to 70°C, 10 g of acrylic acid, 15 g of vinyl acetate, 0.8 g of hydrogen peroxide and 3.5 g of composite emulsifier were added, and the reaction was continued for 1 h. The temperature was lowered to 50°C, 20 g of 20% polyvinyl alcohol aqueous solution was added, the pH was adjusted to 5 with sodium carbonate aqueous solution, the temperature was lowered to below 40°C, and the material was filtered to obtain environmentally friendly moisture-proof cigarette adhesive.

[0052] Example 4

[0053] (1) Under nitrogen atmosphere, 75 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 158 mmol of 5-chlorovaleric acid and 600 mL of dichloromethane were added to a reaction flask, and after stirring evenly, 210 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 240 mmol of 1-hydroxybenzotriazole and 270 mmol of triethylamine were added, and the mixture was reacted at 30° C. for 15 h, extracted with deionized water and ethyl acetate, and the organic phase was concentrated and purified by column chromatography (silica gel, 2-5% methanol in dichloromethane) to obtain a dichloro long-chain organosilicon intermediate.

[0054] (2) Under nitrogen atmosphere, 65 mmol of dichloro long-chain organosilicon intermediate and 920 mL of N,N-dimethylformamide were added to a reaction flask, and after stirring, 145.6 mmol of 3-dimethylaminoacrolein was added, and the mixture was reacted at 95° C. for 28 h. The crude product was concentrated under reduced pressure to obtain a crude product, which was dissolved in methanol, precipitated by adding chloroform, filtered, washed with deionized water, and dried to obtain a dialdehyde quaternary ammonium salt organosilicon modifier.

[0055] (3) Under nitrogen atmosphere, 100 g corn starch and 2500 mL deionized water were added to a reaction flask, and after stirring, 20 g dialdehyde quaternary ammonium salt organosilicon modifier was added, and the mixture was reacted at 70° C. for 4 h. The pH was adjusted to neutral, and the emulsion was dehydrated, washed, and dried to obtain cross-linked starch.

[0056] (4) Under nitrogen atmosphere, deionized water was added to the reaction flask, and when the temperature rose to 45°C, 100 g of cross-linked starch was added, and after stirring evenly, the temperature was raised to 85°C, 9 g of acrylic acid, 13 g of vinyl acetate, 0.6 g of ammonium persulfate and 3 g of composite emulsifier were added, and the reaction was continued for 2 h. The temperature was lowered to 60°C, 16 g of 25% polyvinyl alcohol aqueous solution was added, the pH was adjusted to 6 with sodium carbonate aqueous solution, the temperature was lowered to below 40°C, and the material was filtered to obtain environmentally friendly moisture-proof cigarette adhesive.

[0057] Example 5

[0058] (1) Under nitrogen atmosphere, 35 mmol of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 76.5 mmol of 5-chlorovaleric acid and 285 mL of dichloromethane were added to a reaction flask, and after stirring evenly, 112 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 133 mmol of 1-hydroxybenzotriazole and 170 mmol of triethylamine were added, and the mixture was reacted at 35° C. for 24 h, extracted with deionized water and ethyl acetate, and the organic phase was concentrated and purified by column chromatography (silica gel, 2-5% methanol in dichloromethane) to obtain a dichloro long-chain organosilicon intermediate.

[0059] (2) Under nitrogen atmosphere, 30 mmol of dichloro long-chain organosilicon intermediate and 480 mL of N,N-dimethylformamide were added to a reaction flask, stirred evenly, and then 70 mmol of 3-dimethylaminoacrolein was added. The mixture was reacted at 95 °C for 28 h, and concentrated under reduced pressure to obtain a crude product. The crude product was dissolved in methanol, chloroform was added for precipitation, filtered, washed with deionized water, and dried to obtain a dialdehyde quaternary ammonium salt organosilicon modifier.

[0060] (3) Under nitrogen atmosphere, 100 g of cassava starch and 2500 mL of deionized water were added to a reaction flask, and after stirring, 25 g of dialdehyde quaternary ammonium salt organosilicon modifier was added, and the mixture was reacted at 80° C. for 5 h. The pH was adjusted to neutral, and the emulsion was dehydrated, washed, and dried to obtain cross-linked starch.

[0061] (4) Under nitrogen atmosphere, deionized water was added to the reaction flask, and when the temperature was raised to 50°C, 100 g of cross-linked starch was added, and after stirring evenly, the temperature was raised to 85°C, 8 g of acrylic acid, 12 g of vinyl acetate, 0.7 g of potassium persulfate and 3.5 g of composite emulsifier were added, and the reaction was continued for 1 h. The temperature was lowered to 60°C, 18 g of 22% polyvinyl alcohol aqueous solution was added, the pH was adjusted to 6 with sodium carbonate aqueous solution, the temperature was lowered to below 40°C, and the material was filtered to obtain environmentally friendly moisture-proof cigarette adhesive.

[0062] Comparative Example 1

[0063] (1) Under nitrogen atmosphere, 100 g corn starch and 2500 mL deionized water were added to a reaction flask. After stirring, 5 g of 4,4'-(ethylene-1,2-diyl)benzaldehyde (CAS No. 4720-99-4, structural formula: ), react at 70° C. for 3 h, adjust the pH to neutral, dehydrate, wash and dry the emulsion to obtain cross-linked starch.

[0064] (2) Under nitrogen atmosphere, add deionized water to a reaction flask, wait until the temperature rises to 45°C, add 100 g of cross-linked starch, stir evenly, heat to 80°C, add 8 g of acrylic acid, 12 g of vinyl acetate, 0.5 g of ammonium persulfate and 2.5 g of a composite emulsifier, continue the reaction for 2 h, cool to 55°C, add 15 g of a 25% by mass polyvinyl alcohol aqueous solution, adjust the pH to 5 with a sodium carbonate aqueous solution, cool to below 40°C, filter the material, and obtain cigarette adhesive.

[0065] Comparative Example 2

[0066] (1) Under nitrogen atmosphere, add 100 g corn starch and 2500 mL deionized water to a reaction flask, stir evenly, and then add 5 g glyoxal (CAS No. 107-22-2, structural formula: ), react at 70° C. for 3 h, adjust the pH to neutral, dehydrate, wash and dry the emulsion to obtain cross-linked starch.

[0067] (2) Under nitrogen atmosphere, add deionized water to a reaction flask, wait until the temperature rises to 45°C, add 100 g of cross-linked starch, stir evenly, heat to 80°C, add 8 g of acrylic acid, 12 g of vinyl acetate, 0.5 g of ammonium persulfate and 2.5 g of a composite emulsifier, continue the reaction for 2 h, cool to 55°C, add 15 g of a 25% by mass polyvinyl alcohol aqueous solution, adjust the pH to 5 with a sodium carbonate aqueous solution, cool to below 40°C, filter the material, and obtain cigarette adhesive.

[0068] Hydrophobic performance test: Accurately weigh a cigarette glue sample with a mass of W0, soak it in a beaker filled with deionized water, and ultrasonically treat it at 50°C for 30 minutes. After standing for 3 days and 7 days respectively, the insoluble matter was dried to constant weight and its mass was weighed as W1. The mass loss rate = (W0-W1) / W0×100%.

[0069] Table 1 Hydrophobic performance test

[0070]

[0071]

[0072] As can be seen from the test results in the above table, with the increase of the content of the dialdehyde quaternary ammonium salt organosilicon modifier, the hydrophobicity of the cigarette cross-linking is gradually enhanced. Among them, the mass loss rate of Example 4 after immersion for 3 days is 2.42%. After the extended immersion for 7 days, the mass loss rate is basically not much changed. This is because on the one hand, the dialdehyde quaternary ammonium salt organosilicon modifier contains a dialdehyde group, which can react with the hydroxyl in the starch to form an aldol condensation reaction, so that a plurality of starch molecules are cross-linked to form a spatial network structure; at the same time, the alkenyl in its structure can initiate polymerization with vinyl acetate and acrylic acid, which is equivalent to bridging to form a chemical bond in the spatial network structure of cross-linked starch, thereby improving the density of the cross-linked structure; on the other hand, the introduction of the hydrophobic long-chain alkyl can effectively improve the surface tension between starch and water molecules, hindering the combination of the hydroxyl of starch with water molecules, and improving the hydrophobicity of starch. In addition, the surface energy of the organosilicon molecule is low, and the hydrophobic groups such as the methyl or other alkyl in its molecule are neatly arranged outside. When water vapor or raindrops in the air contact the surface of the organosilicon material, due to the hydrophobicity of the material surface, external moisture can be prevented from penetrating into the material interior, and the hydrophobicity has good hydrophobicity.

[0073] Comparative Example 1 contains a dialdehyde group, which can undergo an aldol condensation reaction with starch, and also contains an olefin group that can be grafted and polymerized with acrylic acid, but does not contain a hydrophobic long chain and silicone, and the hydrophobic performance is not as good as that of the embodiment; Comparative Example 2 contains a dialdehyde group, but does not contain an olefin group that can undergo graft copolymerization, nor does it contain a hydrophobic long chain and silicone, and the hydrophobic performance is the worst.

[0074] Anti-mildew and antibacterial performance test: The prepared cigarette glue was evenly coated on the paper surface using a glue metering rod, and then the glued surface was placed close to another paper. After drying, it was cut into 10mm×10mm paper samples and placed in a triangular flask. 70mL PBS and 5mL bacterial suspension (Escherichia coli and Staphylococcus aureus) were added respectively, so that the concentration of the bacterial suspension in PBS was 1×10 4 -5×10 4 CFU / mL, fix the conical flask on an oscillating shaker, shake at 300r / min for 2min at a working temperature of 25℃, draw 1mL of sample solution and dilute it 100 times with PBS as the sample solution before shaking of the experimental group, continue shaking for 1h and draw 1mL of sample solution as the sample solution after shaking of the experimental group; draw 1mL of sample solution before and after shaking respectively, inoculate plates by agar pouring method, inoculate 2 plates with each sample solution, turn the plates over so that the bottom is facing up, place them in an incubator at 37℃ for 48h, and count the live bacteria according to the prescribed method, inhibition rate = (average number of colonies in sample solution before shaking - average number of colonies in sample solution after shaking) / average number of colonies in sample solution before shaking × 100%.

[0075] Table 2 Anti-mildew and antibacterial performance test

[0076]

[0077] It can be seen from the test results in the above table that with the increase of the content of the dialdehyde quaternary ammonium salt organosilicon modifier, the mildew and antibacterial properties of the cigarette glue are gradually enhanced. This is because the quaternary ammonium salt in the dialdehyde quaternary ammonium salt organosilicon modifier can reduce the surface tension, can be adsorbed on the bacterial surface, and inserted into the lipid layer of the bacterial cell membrane through its hydrophobic group, changing the permeability of the bacterial cell membrane, causing small molecular metabolites to overflow the cell, affecting the cell transmission activity and energy metabolism, thereby causing cell death; at the same time, after the dialdehyde quaternary ammonium salt organosilicon modifier undergoes aldol condensation with starch, the quaternary ammonium salt group with antibacterial properties is tightly embedded in the cigarette glue structure, and has a long-lasting mildew and antibacterial performance. Comparative Examples 1 and 2 do not contain quaternary ammonium salt antibacterial groups and do not have antibacterial properties.

[0078] Initial adhesion test: using the inclined ball rolling method, when the steel ball and the test surface of the sample are in brief contact with a small pressure, the initial adhesion is evaluated based on the rolling distance of the steel ball on the test surface. 2mm thick cigarette glue is evenly scraped on the surface of the paper, and the steel ball is released to roll on the surface of the paper sample. The smaller the rolling distance, the greater the initial adhesion. Record the data of the steel ball rolling distance between 30-200mm.

[0079] Adhesion strength test: Evenly apply 2mm thick cigarette glue on the surface of paper, cover it with another paper, use a smooth roller to roll the adhesive part of the sample at a uniform speed, cure it at room temperature, leave it for 24 hours, and then use a universal testing machine to perform a 90° peel strength test.

[0080] Table 3 Mechanical properties test

[0081] Rolling distance(mm) Adhesion strength (N) Example 1 102.3 2.01 Example 2 85.4 2.23 Example 3 62.1 2.48 Example 4 41.8 2.65 Example 5 35.6 2.70 Comparative Example 1 133.2 1.82 Comparative Example 2 185.4 1.39

[0082] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing environmentally friendly moisture-proof cigarette adhesive, It is characterized in that The preparation method comprises the following steps: Step (1), under nitrogen atmosphere, add starch and deionized water to a reaction flask, stir evenly, and then add The dialdehyde quaternary ammonium salt organic silicon modifier is added, stirred for reaction, after the reaction is completed, the pH is adjusted to neutral, and the emulsion is dehydrated, washed, and dried to obtain cross-linked starch; Step (2), under a nitrogen atmosphere, add deionized water to a reaction flask, wait until the temperature rises to 40-50° C., add cross-linked starch, stir evenly, heat to 70-90° C., add acrylic acid, vinyl acetate, initiator and composite emulsifier, continue to react for 1-2 hours, cool to 50-60° C., add 20-30% polyvinyl alcohol aqueous solution, adjust the pH to 5-6 with sodium carbonate aqueous solution, cool to below 40° C., filter the material, and obtain environmentally friendly moisture-proof cigarette adhesive; In step (1), the starch is any one of corn starch, tapioca starch or potato starch; In the step (2), the initiator is any one of ammonium persulfate, potassium persulfate or hydrogen peroxide.

2. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 1, It is characterized in that In the step (1), the ratio of starch to dialdehyde quaternary ammonium salt organosilicon modifier is 100g:(5-25)g.

3. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 1, It is characterized in that In the step (1), the reaction temperature is 65-80° C. and the reaction time is 2-5 h.

4. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 1, It is characterized in that The composite emulsifier in step (2) is prepared by mixing sodium lauryl sulfate and octylphenol polyoxyethylene ether in a mass ratio of 1:

2.

5. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 1, It is characterized in that In the step (2), the ratio of cross-linked starch, acrylic acid, vinyl acetate, initiator, composite emulsifier and polyvinyl alcohol aqueous solution is 100g:(5-10)g:(8-15)g:(0.3-0.8)g:(2-3.5)g:(12-20)g.

6. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 1, It is characterized in that The preparation method of the dialdehyde quaternary ammonium salt organosilicon modifier in step (1) comprises the following steps: Step S1, under a nitrogen atmosphere, add 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 5-chlorovaleric acid and dichloromethane to a reaction flask, stir evenly, add 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine, react at 20-35° C. for 12-24 hours, extract with deionized water and ethyl acetate, concentrate the organic phase, and purify by column chromatography to obtain a dichloro long-chain organosilicon intermediate; Step S2, under a nitrogen atmosphere, add a dichloro long-chain organosilicon intermediate and N,N-dimethylformamide to a reaction flask, stir evenly, add 3-dimethylaminoacrolein, stir to react, and after the reaction is completed, concentrate under reduced pressure to obtain a crude product, dissolve the crude product in methanol, add chloroform to precipitate, filter, wash with deionized water, and dry to obtain a dialdehyde quaternary ammonium salt organosilicon modifier.

7. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 6, It is characterized in that In the step S1, the ratio of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 5-chlorovaleric acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole, and triethylamine is 1 mol:(2.05-2.2) mol:(2.5-3.5) mol:(2.8-4.2) mol:(4-6) mol.

8. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 6, It is characterized in that In the step S2, the ratio of the dichloro long-chain organosilicon intermediate to 3-dimethylaminoacrolein is 1 mol:(2.1-2.4) mol.

9. The method for preparing the environmentally friendly moisture-proof cigarette adhesive according to claim 6, It is characterized in that In step S2, the reaction temperature is 85-100° C. and the reaction time is 16-32 hours.

10. An environmentally friendly moisture-proof cigarette glue, It is characterized in that Obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of environment-friendly modified starch adhesive for cigarette

    CN103242786A

  • Preparation method for environment-friendly starch cigarette adhesive

    CN103773276A

  • Starch type cigarette adhesive and preparation method thereof

    CN110003817A

  • High-viscosity high-molecular polymer waterproof coating and preparation method thereof

    CN118344806A

  • Water-based paint for spraying soft stone surface and preparation method of water-based paint

    CN118599382A