Seepage crack testing device and method for basement waterproof material
A multi-scenario testing method and device for basement waterproofing materials simulate various conditions to accurately assess their anti-seepage and cracking performance, addressing the limitations of single-scenario tests and enhancing evaluation accuracy.
Patent Information
- Application Number
- CN202411152215.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-06
AI Technical Summary
Existing methods for testing basement waterproofing materials are inadequate, as they only simulate a single scenario, failing to comprehensively evaluate the materials' anti-seepage and cracking performance under various complex conditions.
A multi-scenario testing method and device that includes exterior wall, interior wall, and roof waterproofing, pressure, capillary, and flushing tests, with single and comprehensive scenario groups, using characteristic parameters to assess waterproof strength and cracking intensity, and a grey comprehensive evaluation model for accurate evaluation.
The method and device provide comprehensive and accurate testing of basement waterproof materials, reflecting their true performance and facilitating evaluation of actual use effects by simulating multiple scenarios and adjusting test parameters for accuracy.
Smart Images

Figure CN119086387A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof material testing, in particular to a seepage crack testing device and a testing method for basement waterproof materials. Background Art
[0002] Basement waterproofing materials are building materials specially designed to resist groundwater penetration. There are many types of basement waterproofing materials on the market, including polymer modified asphalt (APP) waterproofing membranes, polyurethane waterproofing materials, polymer modified cement-based coatings, and rubber waterproofing sheets. During the production and use of these materials, their anti-seepage and cracking performance is crucial, so they need to be strictly tested.
[0003] At present, the common method for testing the penetration of basement waterproof materials is relatively simple, usually injecting clean water into the pressing cylinder on one side of the material. However, the test scenario of this method is relatively single, while in actual use environment, basement waterproof materials need to deal with water penetration in various complex situations.
[0004] Therefore, the test results obtained through only a single test scenario are often difficult to fully evaluate the anti-seepage and cracking performance of waterproof materials. Summary of the invention
[0005] The purpose of the present invention is to provide a seepage and crack testing device, a testing method and a system for basement waterproof materials, which solve the technical problem of incomplete testing during the seepage and crack testing of basement waterproof materials in the prior art.
[0006] In a first aspect, the present invention provides a method for testing cracking of basement waterproof materials, the testing method comprising:
[0007] Based on several design application scenarios of waterproof materials, several test scenarios are confirmed; several design application scenarios include exterior wall waterproofing, interior wall waterproofing, ground waterproofing and roof waterproofing; several test scenarios include pressure test scenarios, capillary test scenarios and flushing test scenarios;
[0008] Based on several test scenarios, several test groups are identified; the several test groups include single scenario test groups and comprehensive scenario test groups;
[0009] Based on the characteristic parameters of the waterproof material, confirm the group test parameters corresponding to each test group;
[0010] Based on several test groups and group test parameters of each test group, the waterproof material constructed according to the standard construction process is tested and the test results are obtained.
[0011] Furthermore, based on several design application scenarios of waterproof materials, several test scenarios are confirmed, including:
[0012] Based on several design application scenarios, multiple fracturing causes for each design application scenario are identified; the multiple fracturing causes include pressure fracturing, capillary fracturing, and scour fracturing;
[0013] Based on the multiple causes of cracking in each design application scenario, several test scenarios for current waterproofing materials are identified.
[0014] Furthermore, based on several test scenarios, several test groups are identified, including:
[0015] According to several test scenarios, several single-scenario test groups are determined, and the several single-scenario test groups are set in one-to-one correspondence with the several test scenarios;
[0016] Sort several test scenarios according to preset sorting conditions and confirm several comprehensive test sequences;
[0017] Based on several comprehensive test sequences, several comprehensive scenario test groups are identified.
[0018] Furthermore, several test scenarios are sorted according to preset sorting conditions to determine several comprehensive test sequences, including:
[0019] Each test scenario is set with a corresponding cracking intensity, and multiple comprehensive test sequences are obtained according to the cracking intensity sequence from high to low, from low to high, and several random sequences.
[0020] Further, based on the characteristic parameters of the waterproof material, the group test parameters corresponding to each test group are confirmed, including:
[0021] Each test scenario is equipped with a corresponding waterproof strength assessment model;
[0022] Input characteristic parameters of the waterproof material into the waterproof strength evaluation model corresponding to each test scenario to confirm the waterproof strength of the waterproof material in each test scenario;
[0023] According to the waterproof strength of the waterproof material in each test scenario, confirm the standard test parameters corresponding to the waterproof material in each test scenario;
[0024] The standard test parameters of each test scenario are used as the group test parameters of the corresponding single-scenario test group;
[0025] Based on the comprehensive test sequence of the comprehensive scenario test group and the standard test parameters corresponding to each test scenario, confirm the actual test parameters under each test scenario in the comprehensive scenario test group;
[0026] Based on the actual test parameters in each test scenario in the comprehensive scenario test group, confirm the group test parameters of the comprehensive scenario test group.
[0027] Furthermore, based on the comprehensive test sequence of the comprehensive scenario test group and the standard test parameters corresponding to each test scenario, the actual test parameters of each test scenario in the comprehensive scenario test group are confirmed, including:
[0028] Based on the comprehensive test sequence, confirm the associated test scenario of each test scenario and the associated coefficient; the associated test scenario includes the next test scenario of the current test scenario;
[0029] Based on the correlation coefficient and the standard test parameters corresponding to the current test scenario, the actual test parameters corresponding to the current test scenario are confirmed.
[0030] Furthermore, the test results include the anti-seepage and cracking time of each test group of waterproof materials.
[0031] Furthermore, the testing method further includes:
[0032] Based on the anti-seepage and cracking time of the waterproof materials in each test group, a comprehensive evaluation of the anti-seepage and cracking performance of the waterproof materials is carried out.
[0033] Furthermore, the waterproof strength evaluation model includes a grey comprehensive evaluation model.
[0034] In a second aspect, the present invention provides a seepage crack testing device for basement waterproof materials, which is used to perform a seepage crack testing method for basement waterproof materials. The device comprises:
[0035] A scenario confirmation module is used to confirm several test scenarios based on several design application scenarios of waterproof materials; the several design application scenarios include exterior wall waterproofing, interior wall waterproofing, ground waterproofing and roof waterproofing; the several test scenarios include pressure test scenarios, capillary test scenarios and flushing test scenarios;
[0036] A test group division module is used to confirm a number of test groups based on a number of test scenarios; the number of test groups includes a single scenario test group and a comprehensive scenario test group;
[0037] A parameter setting module, which confirms the group test parameters corresponding to each test group based on the characteristic parameters of the waterproof material;
[0038] The test module is used to test the waterproof material constructed according to the standard construction process based on a number of test groups and group test parameters of each test group, and obtain the test results.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] In the present invention, several test scenarios are obtained through several design application scenarios of waterproof materials to test the waterproof materials, so that the seepage and cracking test of the waterproof materials is more comprehensive and accurate; the waterproof materials are comprehensively tested by dividing the single scenario test group and the comprehensive scenario test group, so that the test results can better reflect the true performance of the waterproof materials, and it is convenient to evaluate the actual use effect. The group test parameters of each test group are confirmed according to the characteristic parameters of the waterproof material, which further improves the accuracy of the test results. The technical problem of incomplete testing in the seepage and cracking test of basement waterproof materials in the prior art is solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a method step diagram of the method for testing the cracking of basement waterproof materials according to the present invention.
[0042] Figure 2 The present invention is a principle block diagram of a seepage and crack testing device for basement waterproof materials. DETAILED DESCRIPTION
[0043] In order to more clearly illustrate the technical solutions of the embodiments of this specification, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some examples or embodiments of this specification. For ordinary technicians in this field, this specification can also be applied to other similar scenarios based on these drawings without creative work. Unless it is obvious from the language environment or otherwise explained, the same reference numerals in the figures represent the same structure or operation.
[0044] It should be understood that the "system", "device", "unit" and / or "module" used herein are a method for distinguishing different components, elements, parts, portions or assemblies at different levels. However, if other words can achieve the same purpose, the words can be replaced by other expressions.
[0045] First, as Figure 1 As shown, the present invention provides a method for testing the cracking of basement waterproof materials, the testing method comprising:
[0046] S1: Based on several design application scenarios of waterproof materials, confirm several test scenarios; several design application scenarios include exterior wall waterproofing, interior wall waterproofing, ground waterproofing and roof waterproofing; several test scenarios include pressure test scenarios, capillary test scenarios and flushing test scenarios;
[0047] During the research and development and production process of waterproof materials, multiple usage scenarios, namely, design application scenarios, will be designed to meet the waterproofing needs of various locations in the basement; for example, waterproofing of exterior walls, interior walls, floors, and ceilings; in actual use, each design application scenario corresponds to at least one cause of seepage and cracking; for example, the cause of seepage and cracking of ground waterproofing includes the capillary action of groundwater.
[0048] S2: Based on several test scenarios, confirm several test groups; the several test groups include single scenario test groups and comprehensive scenario test groups;
[0049] The single-scenario test group includes testing the waterproof material through a single test scenario; the comprehensive scenario test group includes testing the same waterproof material through multiple test scenarios in a cycle, making the penetration and cracking test of the waterproof material more comprehensive and accurate;
[0050] S3: based on the characteristic parameters of the waterproof material, confirm the group test parameters corresponding to each test group;
[0051] At the beginning of the research and development, each waterproof material is designed with corresponding characteristic parameters; the characteristic parameters include material type, waterproof material content, bonding strength, processing technology, structure, thickness and tensile strength, etc.; according to the characteristic parameters, the corresponding group test parameters are determined;
[0052] S4: Based on a number of test groups and group test parameters of each test group, the waterproof material constructed according to the standard construction process is tested and the test results are obtained.
[0053] Obtain multiple sets of waterproof materials according to standard construction techniques, and distribute them to various test groups. Each test group tests the waterproof materials according to its corresponding test scenario and group test parameters to obtain test results, which include the anti-seepage and cracking time.
[0054] The specific implementation process of this embodiment includes:
[0055] In this embodiment, through several design application scenarios of waterproof materials, several test scenarios are obtained to test the waterproof materials, making the seepage and cracking test of waterproof materials more comprehensive and accurate; by dividing the waterproof materials into single-scenario test groups and comprehensive scenario test groups, the waterproof materials are comprehensively tested, so that the test results can better reflect the true performance of the waterproof materials and facilitate the evaluation of the actual use effect. The group test parameters of each test group are confirmed according to the characteristic parameters of the waterproof materials, further improving the accuracy of the test results. The technical problem of incomplete testing in the seepage and cracking test of basement waterproof materials in the prior art is solved.
[0056] In this embodiment, based on several design application scenarios of waterproof materials, several test scenarios are confirmed, including:
[0057] Based on several design application scenarios, multiple fracturing causes for each design application scenario are identified; the multiple fracturing causes include pressure fracturing, capillary fracturing, and scour fracturing;
[0058] The structure of the basement determines the actual use scenario of the waterproof material, and also determines that the types of water that affect the seepage of the waterproof material include at least groundwater, surface water, and capillary water. Groundwater has the characteristics of long-term stable infiltration, surface water has the characteristics of intermittent scouring, and capillary water is distributed in the soil, can transmit hydrostatic pressure, and is not affected by gravity. According to the design application scenario of the waterproof material, the use location of the waterproof material in the basement is determined, and the cause of the seepage of the waterproof material is determined according to the use location. In this embodiment, the causes of the seepage include pressure seepage, capillary seepage, and stamping seepage.
[0059] Based on the multiple causes of cracking in each design application scenario, several test scenarios for current waterproofing materials are identified.
[0060] When the cause of cracking is pressure cracking, the test scenario is a pressure test scenario, and the specific test includes: applying a fixed pressure to the water used to test the waterproof material; when the cause of cracking is capillary cracking, the test scenario corresponds to the capillary test scenario, and the specific test includes: maintaining a stable capillary water effect on the waterproof material, such as covering the waterproof material with soil according to preset requirements, and keeping the soil at a fixed humidity, the preset requirements include thickness, weight, etc.; when the cause of cracking is stamping cracking, the test scenario.
[0061] In this embodiment, based on several test scenarios, several test groups are identified, including:
[0062] According to several test scenarios, several single-scenario test groups are determined, and the several single-scenario test groups are set in one-to-one correspondence with the several test scenarios;
[0063] According to the preset sorting conditions, several test scenarios are sorted to determine several comprehensive test sequences; including: each test scenario is provided with a corresponding seepage fracture strength, and multiple comprehensive test sequences are obtained according to the seepage fracture strength sequence from high to low, from low to high, and several random sequences; based on the several comprehensive test sequences, several comprehensive scenario test groups are determined. In this embodiment, the sequence of seepage fracture strength from high to low is pressure test scenario, flushing test scenario, and capillary test scenario.
[0064] In this embodiment, the penetration ability of each test scenario to the waterproof material is analyzed through big data; the greater the penetration crack strength, the stronger the penetration ability to the waterproof material in the test scenario. Designing several comprehensive test sequences can test the anti-seepage cracking ability of the waterproof material in all aspects, so that the final test results are comprehensive and accurate.
[0065] It should be noted that, in this embodiment, when the comprehensive test scenario is tested, multiple test scenarios are cyclically tested in the comprehensive test sequence, and the single test time of each test scenario is the same.
[0066] According to another embodiment of the present invention, based on the characteristic parameters of the waterproof material, confirming the group test parameters corresponding to each test group includes:
[0067] SS1: Each test scenario is equipped with a corresponding waterproof strength assessment model;
[0068] The waterproof strength evaluation model includes a grey comprehensive evaluation model; each waterproof strength evaluation model is provided with multiple groups of standard control groups; the design parameters of the current waterproof material are comprehensively evaluated with the multiple groups of standard control groups in the same waterproof strength evaluation model to obtain a ranking, and the waterproof strength corresponding to the current waterproof material is obtained according to the ranking;
[0069] SS2: Input the characteristic parameters of the waterproof material into the waterproof strength evaluation model corresponding to each test scenario to confirm the waterproof strength of the waterproof material in each test scenario;
[0070] The waterproof ability of the same waterproof material in different test scenarios is different; therefore, in this embodiment, a waterproof strength evaluation model is provided corresponding to each test scenario to evaluate the waterproof strength of the waterproof material in each test scenario according to the characteristic parameters of the waterproof material; in this embodiment, the waterproof strength includes level one, level two, level three, level four and level five from high to low; in some other embodiments, the waterproof strength includes level A, level B and level C from high to low.
[0071] SS3: According to the waterproof strength of the waterproof material in each test scenario, confirm the standard test parameters corresponding to the waterproof material in each test scenario;
[0072] In this embodiment, different waterproof strengths are all set with corresponding standard test parameters. For example, if the waterproof strength of the current waterproof material is Class B in a test scenario, the standard test parameters corresponding to Class B waterproof strength are obtained.
[0073] Each test scenario sets multiple standard test parameters according to the waterproof strength, which can make the test results of waterproof materials more accurate and avoid mismatch of standard test parameters, which may cause distortion of test results.
[0074] SS4: The standard test parameters of each test scenario are used as the group test parameters of the corresponding single scenario test group;
[0075] For a single-scenario test group, the standard test parameters corresponding to the current waterproof material in the test scenario are directly used as the group test parameters;
[0076] SS5: Based on the comprehensive test sequence of the comprehensive scenario test group and the standard test parameters corresponding to each test scenario, confirm the actual test parameters under each test scenario in the comprehensive scenario test group;
[0077] For the comprehensive scenario test group, it is necessary to adjust the standard test parameters of the current waterproof material in each test scenario to obtain the actual test parameters; in this embodiment, the adjustment includes lowering the standard test parameters according to a set percentage;
[0078] SS6: Confirm the group test parameters of the comprehensive scenario test group based on the actual test parameters of each test scenario in the comprehensive scenario test group.
[0079] The specific implementation process of this embodiment includes:
[0080] In this embodiment, the waterproof strength of the waterproof material in each test scenario is evaluated by characteristic parameters, so as to obtain the corresponding standard test parameters in each test scenario, so that the group test parameters of each single-scenario test group and each comprehensive scenario test group are more accurate and reasonable, avoiding the inaccuracy of the test results caused by unreasonable group test parameter settings.
[0081] According to another embodiment of the present invention, based on the comprehensive test sequence of the comprehensive scenario test group and the standard test parameters corresponding to each test scenario, confirming the actual test parameters under each test scenario in the comprehensive scenario test group;
[0082] Based on the comprehensive test sequence, confirm the associated test scenario of each test scenario and the associated coefficient; the associated test scenario includes the next test scenario of the current test scenario;
[0083] Based on the correlation coefficient and the standard test parameters corresponding to the current test scenario, the actual test parameters corresponding to the current test scenario are confirmed.
[0084] The specific implementation process of this embodiment includes:
[0085] In this embodiment, the next test scene is used as an associated test scene of the current test scene. Since each test scene tests the waterproof material in a cycle when performing a comprehensive scene test, each scene has a corresponding associated test scene.
[0086] In this embodiment, the correlation coefficient is greater than zero and less than or equal to one. In this embodiment, when the permeation strength of the associated test scene is greater than the permeation strength of the current test scene, the correlation coefficient is between 0.4 and 0.6; when the permeation strength of the associated test scene is less than the permeation strength of the current test scene, the correlation coefficient is between 0.6 and 0.8; when the permeation strength of the associated test scene is equal to the permeation strength of the current test scene, the correlation coefficient is 1;
[0087] Compared with the single-scenario test that tests the waterproof material's ability to prevent seepage and cracking in a certain aspect, the comprehensive scenario test tests the waterproof material's ability to prevent seepage and cracking in multiple aspects. Therefore, in the comprehensive scenario test, the actual test parameters in each test scenario need to be adjusted down to a certain extent from the corresponding standard test parameters. In this embodiment, by setting the correlation coefficient, the connection between adjacent test scenarios can be enhanced, and the adjustment range of the standard test parameters in each test scenario can be determined; so that the test intensity of the waterproof material is kept within a reasonable range, making the test results more authentic.
[0088] It should be noted that, in this embodiment, the occurrence ratio of each cause of seepage cracking in the overall basement seepage cracking phenomenon is statistically analyzed through big data; the higher the occurrence ratio is, the greater the seepage cracking intensity is.
[0089] According to another embodiment of the present invention, the test results include the anti-cracking time of each test group of waterproof materials.
[0090] The specific implementation process of this embodiment includes:
[0091] In some other embodiments, the test result also includes the water penetration rate of the waterproof material, wherein the unit of the water penetration rate includes milliliters per second.
[0092] In this embodiment, the testing method further includes:
[0093] Based on the anti-seepage and cracking time of the waterproof materials in each test group, a comprehensive evaluation of the anti-seepage and cracking performance of the waterproof materials is carried out.
[0094] Comprehensive evaluation based on the test results of each test group of waterproof materials can comprehensively and accurately assess the anti-seepage and cracking performance of waterproof materials.
[0095] In some embodiments, the anti-seepage cracking performance of the waterproof material is evaluated by inputting the test results into a comprehensive evaluation model; the comprehensive evaluation model includes:
[0096] Second, as Figure 2 As shown, the present invention provides a seepage crack testing device for basement waterproof materials, which is used to perform a seepage crack testing method for basement waterproof materials. The device comprises:
[0097] A scenario confirmation module is used to confirm several test scenarios based on several design application scenarios of waterproof materials; the several design application scenarios include exterior wall waterproofing, interior wall waterproofing, ground waterproofing and roof waterproofing; the several test scenarios include pressure test scenarios, capillary test scenarios and flushing test scenarios;
[0098] A test group division module is used to confirm a number of test groups based on a number of test scenarios; the number of test groups includes a single scenario test group and a comprehensive scenario test group;
[0099] A parameter setting module, which confirms the group test parameters corresponding to each test group based on the characteristic parameters of the waterproof material;
[0100] The test module is used to test the waterproof material constructed according to the standard construction process based on several test groups and group test parameters of each test group, and obtain the test results. Grey comprehensive evaluation model.
[0101] The above embodiments are only used to illustrate the technical method of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical method of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical method of the present invention.
Claims
1. A method for testing the cracking of basement waterproof materials, characterized in that: Test methods include: Based on several design application scenarios of waterproof materials, several test scenarios are confirmed; several design application scenarios include exterior wall waterproofing, interior wall waterproofing, ground waterproofing and roof waterproofing; several test scenarios include pressure test scenarios, capillary test scenarios and flushing test scenarios; Based on several test scenarios, several test groups are identified; the several test groups include single scenario test groups and comprehensive scenario test groups; Based on the characteristic parameters of the waterproof material, confirm the group test parameters corresponding to each test group; Based on several test groups and group test parameters of each test group, the waterproof material constructed according to the standard construction process is tested and the test results are obtained.
2. The method for testing cracking of basement waterproof materials according to claim 1, characterized in that: Based on several design application scenarios of waterproof materials, several test scenarios are confirmed, including: Based on several design application scenarios, multiple fracturing causes for each design application scenario are identified; the multiple fracturing causes include pressure fracturing, capillary fracturing, and scour fracturing; Based on the multiple causes of cracking in each design application scenario, several test scenarios for current waterproofing materials are identified.
3. The method for testing cracking of basement waterproof materials according to claim 2, characterized in that: Based on several test scenarios, several test groups were identified, including: According to several test scenarios, several single-scenario test groups are determined, and the several single-scenario test groups are set in one-to-one correspondence with the several test scenarios; Sort several test scenarios according to preset sorting conditions and confirm several comprehensive test sequences; Based on several comprehensive test sequences, several comprehensive scenario test groups are identified.
4. The method for testing cracking of basement waterproof materials according to claim 3, characterized in that: Sort several test scenarios according to preset sorting conditions and confirm several comprehensive test sequences, including: Each test scenario is set with a corresponding cracking intensity, and multiple comprehensive test sequences are obtained according to the cracking intensity sequence from high to low, from low to high, and several random sequences.
5. The method for testing cracking of basement waterproof materials according to claim 3, characterized in that: Based on the characteristic parameters of the waterproof material, confirm the group test parameters corresponding to each test group, including: Each test scenario is equipped with a corresponding waterproof strength assessment model; Input characteristic parameters of the waterproof material into the waterproof strength evaluation model corresponding to each test scenario to confirm the waterproof strength of the waterproof material in each test scenario; According to the waterproof strength of the waterproof material in each test scenario, confirm the standard test parameters corresponding to the waterproof material in each test scenario; The standard test parameters of each test scenario are used as the group test parameters of the corresponding single-scenario test group; Based on the comprehensive test sequence of the comprehensive scenario test group and the standard test parameters corresponding to each test scenario, confirm the actual test parameters under each test scenario in the comprehensive scenario test group; Based on the actual test parameters in each test scenario in the comprehensive scenario test group, confirm the group test parameters of the comprehensive scenario test group.
6. The method for testing cracking of basement waterproof materials according to claim 5, characterized in that: Based on the comprehensive test sequence of the comprehensive scenario test group and the standard test parameters corresponding to each test scenario, confirm the actual test parameters of each test scenario in the comprehensive scenario test group, including: Based on the comprehensive test sequence, confirm the associated test scenario of each test scenario and the associated coefficient; the associated test scenario includes the next test scenario of the current test scenario; Based on the correlation coefficient and the standard test parameters corresponding to the current test scenario, the actual test parameters corresponding to the current test scenario are confirmed.
7. The method for testing cracking of basement waterproof materials according to claim 1, characterized in that: The test results include the anti-cracking time of each test group of waterproof materials.
8. The method for testing cracking of basement waterproof materials according to claim 7, characterized in that: The test method also includes: Based on the anti-seepage and cracking time of the waterproof materials in each test group, a comprehensive evaluation of the anti-seepage and cracking performance of the waterproof materials is carried out.
9. The method for testing cracking of basement waterproof materials according to claim 5, characterized in that: The waterproof strength evaluation model includes a grey comprehensive evaluation model.
10. A seepage crack testing device for basement waterproofing materials, characterized in that: For performing the test method according to any one of claims 1 to 9, the device comprises: A scenario confirmation module is used to confirm several test scenarios based on several design application scenarios of waterproof materials; the several design application scenarios include exterior wall waterproofing, interior wall waterproofing, ground waterproofing and roof waterproofing; the several test scenarios include pressure test scenarios, capillary test scenarios and flushing test scenarios; A test group division module is used to confirm a number of test groups based on a number of test scenarios; the number of test groups includes a single scenario test group and a comprehensive scenario test group; A parameter setting module, which confirms the group test parameters corresponding to each test group based on the characteristic parameters of the waterproof material; The test module is used to test the waterproof material constructed according to the standard construction process based on a number of test groups and group test parameters of each test group, and obtain the test results.