Outer packaging material for electricity storage device
The packaging material for lithium-ion batteries addresses insulation loss by using a polypropylene resin and incompatible component sealant layer with a sea-island structure and low-shrinkage properties to maintain insulation despite thinning, effectively preventing electrolyte contact and void formation.
Patent Information
- Application Number
- CN202411205835.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-11-22
- Filing Date
- 2018-05-18
- Publication Date
- 2024-12-06
AI Technical Summary
Existing outer packaging materials for lithium-ion batteries face insulation reduction due to damage to the sealant layer during degassing heat sealing, which is exacerbated by the thinning of the sealant layer, leading to electrolyte contact with the metal layer and reduced insulation.
The packaging material includes a sealant layer composed of polypropylene resin and an incompatible component, with specific strength and shrinkage properties to maintain insulation, featuring a sea-island structure and a low-shrinkage sealant layer to prevent void formation during electrolyte foaming.
The solution effectively maintains insulation properties after degassing and heat sealing, even with a thin sealant layer, by enhancing cohesive force and preventing electrolyte contact with the metal layer.
Smart Images

Figure CN119092909A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese application No. 201880003311.X, whose application date is May 18, 2018 and whose invention name is “Outer packaging material for power storage device”. Technical Field
[0002] The present invention relates to an outer packaging material for an electric storage device. Background Art
[0003] As a power storage device, for example, secondary batteries such as lithium ion batteries, nickel-metal hydride batteries and lead storage batteries and electrochemical capacitors such as double electric layer capacitors are known. Due to the miniaturization of portable devices or the limitation of installation space, further miniaturization of power storage devices is sought, and lithium ion batteries with high energy density have attracted attention. As an outer packaging material used in lithium ion batteries, metal cans have been used in the past, but multilayer films (such as films composed of substrate layers / metal foil layers / sealant layers, etc.) that are lightweight, have high heat dissipation, and can be produced at low cost are beginning to be used.
[0004] In lithium-ion batteries using the above-mentioned multilayer film as an outer packaging material, in order to prevent moisture from invading the interior, an outer packaging material containing an aluminum foil layer is used as a metal foil layer to cover the battery contents. A lithium-ion battery using this structure is called an aluminum laminated lithium-ion battery. The battery contents of a lithium-ion battery contain an electrolyte solution in which a lithium salt as an electrolyte is dissolved in a non-protonic solvent having permeability such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, or an electrolyte layer formed by a polymer gel impregnated with the electrolyte solution together with a positive electrode, a negative electrode and a separator.
[0005] For example, an embossed lithium-ion battery is known as an aluminum laminated lithium-ion battery in which a concave portion is formed in a portion of an outer packaging material by cold rolling, the battery contents are stored in the concave portion, the remaining portion of the outer packaging material is folded back, and the edge portion is sealed by heat sealing. For the outer packaging material constituting such a lithium-ion battery, it is required that the lamination strength between the aluminum foil layer and the sealant layer is not easily reduced by the electrolyte in the battery contents while showing stable sealing properties by heat sealing.
[0006] In addition, as smartphones, tablet PCs, etc. become thinner, thinner products are also required for the power storage devices installed. As the power storage devices become thinner, the base layer, metal foil layer, and sealant layer of the outer packaging materials for power storage devices are becoming thinner, so the reduction in insulation and lamination strength caused by the thinning of the sealant layer has become a problem.
[0007] Therefore, for example, Patent Document 1 proposes an outer packaging material having a heat-sealing layer (sealant layer) containing an adhesive polymethylpentene layer, which can utilize the heat and pressure of heat sealing to stably seal without short-circuiting the barrier layer of the outer packaging material and the tab.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2002-245983 Summary of the invention
[0011] Technical problem to be solved by the invention
[0012] The existing outer packaging material described in the above-mentioned patent document 1 is a countermeasure for the reduction in insulation caused by the contact between the tab conductor and the metal foil layer. However, it is believed that there are other reasons for the reduction in insulation. As a lithium-ion battery, in order to store energy, it is necessary to charge and discharge under specified conditions such as current value or voltage value, ambient temperature, etc. to cause chemical changes (chemical conversion). The chemical conversion process is carried out in the state of a temporary battery injected with an electrolyte. Then, in order to remove the gas generated by the chemical conversion or replenish the electrolyte, the battery is opened once, and then the final seal is performed to complete the battery. Since the final seal is a seal of the part that was once immersed in the electrolyte, it becomes a degassing seal (degassing heat seal) that is heat-sealed in a state where the electrolyte is swallowed.
[0013] The present inventors have verified that the reduction in insulation is often caused by damage to the sealant layer due to degassing heat sealing, and countermeasures are very important. Patent Document 1 does not discuss the damage to the sealant layer due to degassing heat sealing.
[0014] In degassing heat sealing, when the outer packaging material containing the battery contents is sealed by heat sealing, the electrolyte is swallowed while heat sealing is performed, so there are cases where the electrolyte foams and the sealant layer is damaged. Then, the electrolyte enters from the damaged part of the sealant layer and contacts the metal layer, thereby reducing the insulation.
[0015] Furthermore, the reduction in insulation due to the destruction of the sealant layer caused by degassing heat sealing is easily affected by the thinning of the sealant layer, and therefore, countermeasures are particularly needed in the future in improving the insulation.
[0016] The present invention has been made in view of the technical problems of the prior art described above, and an object of the present invention is to provide an outer packaging material for a power storage device that can sufficiently maintain insulation properties after degassing and heat sealing.
[0017] Means for solving technical problems
[0018] The present invention provides an outer packaging material for a power storage device, which comprises at least a base material layer, a metal foil layer provided with an anti-corrosion treatment layer on one or both surfaces, and a sealant layer in order.
[0019] In the outer packaging material for a storage device according to one aspect of the present invention, the sealant layer contains a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin, and the content of the incompatible component (B) is 1 to 40% by mass based on the total amount of the sealant layer. Furthermore, for the bonded portion formed by heat-sealing and bonding the outer packaging materials overlapped in a manner such that the sealant layers face each other under the conditions of a temperature of 190° C., a pressure of 0.5 MPa, and 3 seconds, in a curve showing the relationship between the displacement from the one end and the sealant strength when the sealant strength is continuously measured from one end to the other end, the maximum seal strength S M It is 35N / 15mm or more and satisfies the following conditions (1) or (2).
[0020] (1) After obtaining the above maximum sealing strength S M After the displacement of , there is a stable region of sealing strength, and the sealing strength S in this stable region S With the above maximum sealing strength S M Ratio S S / S M It is above 0.3.
[0021] (2) There is no stable region, and the maximum sealing strength S is obtained. M The average sealing strength S between the displacement of the other end and the displacement of the other end A With the above maximum sealing strength S M Ratio S A / S M It is above 0.3.
[0022] According to the outer packaging material for a storage device having the above-mentioned structure, even when the sealant layer is thinned, the insulation after degassing heat sealing can be fully maintained. The present inventors speculate the reason why the outer packaging material for a storage device exerts such an effect as follows. The sealant layer of the outer packaging material for a storage device is prone to defects in the production process of the storage device such as heat sealing, degassing heat sealing and molding. In particular, due to the thin filmization of the sealant layer, in the degassing sealing in which the sealant layer is heat-sealed in a state of swallowing an electrolyte, it is believed that the deformation of the sealant layer due to volatilization (foaming) of the electrolyte increases and the insulation is easily reduced. As a reason for the reduction in insulation due to this deformation, it is believed that, for example, the vicinity of the metal foil layer is easily exposed due to foaming, and the electrolyte contacts the exposed part. In the present invention, the maximum sealing strength S MThe outer packaging material satisfies the above conditions (1) or (2) and is 35 N / 15 mm or more. This is believed to provide a strong cohesive force for the sealant resin and prevent voids from forming during electrolyte foaming. As a result, insulation is unlikely to decrease.
[0023] In the above curve, the maximum sealing strength S M 40N / 15mm or more, the above ratio S S / S M Or the above ratio S A / S M This makes it easier to further suppress a decrease in insulation properties.
[0024] Since the sealant layer contains the polypropylene resin (A) and the incompatible component (B) incompatible therewith, an island structure composed of these is formed in the sealant layer. By forming this island structure, the sealant layer can be given impact resistance and the sealing strength can be improved.
[0025] The above-mentioned incompatible component (B) preferably contains a compound (B1) having a compatible portion with the above-mentioned polypropylene resin (A). The present inventors believe that when the electrolyte foams during degassing heat sealing, voids are easily formed starting from the sea-island interface. Therefore, in the sealant layer, the above-mentioned sea-island interface can be improved by the above-mentioned incompatible component (B) containing a compound (B1) having a compatible portion with the above-mentioned polypropylene resin (A), and the formation of voids accompanying the foaming of the electrolyte can be suppressed, thereby further improving the insulation. In addition, the improvement in the sealing strength of the sea-island interface brought about by the above-mentioned compound (B1) can also improve the above-mentioned sealing strength S M , S S or S A .
[0026] The above-mentioned sealant layer can be composed of multiple layers, in which case at least one layer is a layer containing the above-mentioned polypropylene resin (A) and the above-mentioned incompatible component (B) that is incompatible with the above-mentioned polypropylene resin, and the above-mentioned incompatible component (B) contains the above-mentioned compound (B1).
[0027] The incompatible component (B) may contain an ethylene-α-olefin copolymer. In addition, the sealant layer may further contain a compatible elastomer (C) compatible with the polypropylene resin (A), and the compatible elastomer (C) may contain a propylene-α-olefin copolymer.
[0028] In the outer packaging material for a storage device according to another aspect of the present invention, the sealant layer contains a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin, and has a region where the polypropylene resin (A) exists and a plurality of regions where the incompatible component (B) exists surrounded by the polypropylene resin (A). Furthermore, the sealant layer contains a low-shrinkage sealant layer, and the low-shrinkage sealant layer is an average length LAh of the region where the incompatible component (B) exists in the cross section along the thickness direction and the MD direction of the sealant layer after the outer packaging material for a storage device is heated at 190°C for 30 seconds. MD The average length LA of the region where the incompatible component (B) exists in the cross section along the thickness direction and the MD direction in the MD direction is MD Ratio (LAh MD / LA MD ) is 0.20 or more. MD / LA MD ) is simply called the shrinkage ratio.
[0029] According to the outer packaging material for the above-mentioned storage device, even when the sealant layer is made into a thin film, the insulation after degassing and heat sealing can be fully maintained. The present inventors speculate the reasons why the outer packaging material for the storage device exerts such an effect as follows. During degassing and heat sealing, the sealant layer swells due to the electrolyte, and heat sealing is performed in a state where the electrolyte is swallowed, so deformation of the sealant layer occurs, which is believed to be caused by volatilization (foaming) of the electrolyte. The foaming of the electrolyte is likely to form voids in the interface of the sea-island structure formed by the polypropylene resin (A) and the incompatible component (B) possessed by the sealant layer, and the metal foil layer is likely to be exposed to the void inside the sealant layer, and the electrolyte invades the void, and the electrolyte contacts the exposed part of the metal foil layer, thereby reducing the insulation. In particular, when the sealant layer is made into a thin film, the deformation of the sealant layer caused by foaming increases relative to the thickness, and the possibility of reduced insulation is further increased. As a result, according to the present invention, the sealant layer contains a low-shrinkage sealant layer having a shrinkage ratio of more than a certain value. In the outer packaging material having such a low shrinkage sealant layer, the polypropylene resin (A) and the incompatible component (B) at the interface of the sea-island structure have high adhesion, and even when the electrolyte foams, it is difficult to generate gaps starting from the interface. Therefore, in the outer packaging material for the storage device of the present invention, even when the sealant layer is made into a thin film, the insulation after degassing and heat sealing can be fully maintained.
[0030] The average length LAh in the MD direction of the region where the incompatible component (B) exists in the cross section along the thickness direction and the MD direction of the sealant layer after the outer packaging material for the storage device is heated at 190°C for 30 seconds is MD The average length LAh in the thickness direction VD Ratio (LAh MD / LAh VD ) is preferably 2.50 or more. When the region of existence of the incompatible component (B) after heating satisfies the above, there is a tendency to further maintain good insulation after degassing and heat sealing.
[0031] In the outer packaging material for the power storage device, the sealant layer may be composed of a plurality of layers, and at least one of the layers is the low-shrinkage sealant layer. In this case, the layer closest to the metal foil layer among the plurality of sealant layers is preferably the low-shrinkage sealant layer. The layer closest to the metal foil layer through the sealant layer is a low-shrinkage sealant layer, which has a tendency to further suppress the reduction in insulation after degassing heat sealing. Since the foaming of the electrolyte during degassing heat sealing mostly occurs in the portion of the sealant layer close to the metal foil layer and the shrinkage ratio in the layer closest to the metal foil layer is large (the shrinkage of the incompatible component (B) is small), it has a tendency to more efficiently suppress the reduction in insulation.
[0032] In the outer packaging material for the power storage device, the sealant layer may further contain a compatible elastomer (C) compatible with the polypropylene resin (A), and the compatible elastomer (C) may contain a propylene-α-olefin copolymer. By containing the compatible elastomer (C) compatible with the polypropylene resin (A), the sealant layer can be given flexibility, and the outer packaging material can be given functions such as molding whitening suppression and impact resistance, thereby improving the functionality as the outer packaging material.
[0033] In addition, the sealant layer may be composed of a plurality of layers, and in the layer closest to the metal foil layer, the polypropylene resin (A) may contain acid-modified polypropylene, and the compatible elastomer (C) may contain atactic polypropylene or atactic propylene-α-olefin copolymer. According to this outer packaging material for a storage battery device, it is easy to maintain the close adhesion between the sealant layer and the metal foil layer, prevent the occurrence of poorly bonded portions that become the starting point of electrolyte foaming, and tend to further suppress the reduction of insulation after degassing and heat sealing.
[0034] In any aspect of the packaging material for a power storage device of the present invention, the thickness of the sealant layer may be 10 to 45 μm. Even if the sealant layer is thinned, the insulation after degassing and heat sealing can be sufficiently maintained.
[0035] The outer packaging material for a storage device in any aspect of the present invention may further include an adhesive layer between the metal foil layer and the sealant layer, and the adhesive layer may contain an acid-modified polyolefin and at least one curing agent selected from a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxyl group, a compound having an oxazoline group and a carbodiimide compound.
[0036] Effects of the Invention
[0037] According to the present invention, it is possible to provide an outer packaging material for a power storage device that can sufficiently maintain insulation properties after degassing and heat sealing. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a schematic cross-sectional view of an outer packaging material for a power storage device according to one embodiment of the present invention.
[0039] Figure 2 This is a schematic cross-sectional view of the outer packaging material after the outer packaging materials are overlapped and heat-sealed so that the sealant layers face each other.
[0040] Figure 3 This is a graph showing an example of measurement results of the sealing strength of the adhesive portion of the outer packaging material being measured continuously from one end to the other end, and is a graph showing the relationship between the displacement from one end of the adhesive portion and the sealing strength.
[0041] Figure 4 This is a graph showing another example of the measurement results of the sealing strength of the adhesive portion of the outer packaging material being measured continuously from one end to the other end, and is a graph showing the relationship between the displacement from one end of the adhesive portion and the sealing strength.
[0042] Figure 5 The enlarged cross-sectional views schematically show the cross-sectional structure of the sealant layer in the outer packaging material for a storage device according to one embodiment of the present invention along the thickness direction and the MD direction, wherein (a) is a view before heating at 190°C for 30 seconds, and (b) is a view after heating at 190°C for 30 seconds.
[0043] Figure 6 This is a schematic cross-sectional view of an outer packaging material for a power storage device according to one embodiment of the present invention.
[0044] Figure 7 This is a schematic cross-sectional view of an outer packaging material for a power storage device according to one embodiment of the present invention.
[0045] Figure 8 This is a schematic diagram for explaining the method of preparing the evaluation sample in the example.
[0046] Fig. 9 This is a schematic diagram for explaining the method of preparing the evaluation sample in the example.
[0047] Fig.10 This is a schematic diagram for explaining the method of preparing the evaluation sample in the example.
[0048] Fig.11 This is a schematic diagram for explaining the method of preparing the evaluation sample in the example.
[0049] Fig.12 These are SEM images of the cross-sections along the VD direction (thickness direction) and MD direction of the sealant layer of the outer packaging material for the storage device obtained in Example 2-7, (a) is the image before heating at 190°C for 30 seconds, and (b) is the image after heating at 190°C for 30 seconds. DETAILED DESCRIPTION
[0050] The following is a reference to the attached Figure 1 The preferred embodiment of the present invention will be described in detail. In addition, in the drawings, the same or corresponding parts are marked with the same symbols, and repeated descriptions are omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0051] [Outer packaging materials for power storage devices]
[0052] Figure 1 2 is a cross-sectional view schematically showing an embodiment of an outer packaging material for a power storage device according to the present embodiment. Figure 1 As shown, the outer packaging material (outer packaging material for a power storage device) 10 of the present embodiment is a laminated body in which the following layers are laminated in order: a base material layer 11; an adhesive layer 12 (sometimes referred to as a first adhesive layer 12) formed on one surface of the base material layer 11; a metal foil layer 13 formed on the surface of the first adhesive layer 12 opposite to the base material layer 11; an anticorrosion treatment layer 14 formed on the surface of the metal foil layer 13 opposite to the first adhesive layer 12; an adhesive layer 17 (sometimes referred to as a second adhesive layer 17) formed on the surface of the anticorrosion treatment layer 14 opposite to the metal foil layer 13; and a sealant layer 16 formed on the surface of the second adhesive layer 17 opposite to the anticorrosion treatment layer 14. In the outer packaging material 10, the base material layer 11 is the outermost layer and the sealant layer 16 is the innermost layer. That is, the outer packaging material 10 is used with the base material layer 11 facing the outside of the power storage device and the sealant layer 16 facing the inside of the power storage device.
[0053] The sealant layer 16 is a layer that imparts sealing properties to the outer packaging material 10 by heat sealing. The sealant layer 16 contains a polypropylene resin (A) and an incompatible component (B) that is incompatible with the above-mentioned polypropylene resin. Hereinafter, depending on the circumstances, the above-mentioned polypropylene resin (A) is sometimes referred to as "component (A)", and the incompatible component (B) that is incompatible with the above-mentioned component (A) is sometimes referred to as "component (B)". Here, in this specification, "no compatibility with component (A)", "incompatible with component (A)" (incompatible system) means that the dispersed phase size is greater than 200nm and less than 50μm and is dispersed in the polypropylene resin constituting component (A). In addition, "compatible with component (A)", "having compatibility with component (A)" (compatible system) means that the dispersed phase size is greater than 1nm and less than 200nm and is dispersed in the polypropylene resin constituting component (A).
[0054] (I) First Aspect
[0055] The outer packaging materials 10 are overlapped so that the sealant layers 16 face each other, and are heat-sealed using a sealing bar so that the sealant layers 16 are thermally melt-bonded and bonded to each other. Figure 2 It is a cross-sectional view of the outer packaging material after heat sealing, and the heat sealing part P H Indicates the part that is directly heat-sealed by the sealing strip. In addition, Figure 2 The heat-sealed portion P is shown as a portion of the sealant layer 16 melted by heating. H Start to move, forming sealant melt bonding part 16 M By forming the sealant melt bonding portion 16 M , even in the unsealed melt-bonded area P M In other words, the outer packaging materials 10 are also bonded to each other at the heat-sealed portion P. H And the fusion bonding part P M The heat seal strength of the outer packaging materials 10 bonded in this way can be measured as the load per unit width required to peel off one outer packaging material 10 from the other outer packaging material 10 after bonding. The bonded outer packaging materials 10 are used as samples for heat seal strength measurement. The width direction of the heat seal is the length direction, and the outer packaging materials 10 are cut into the molten bonded part P including the side where the electrolyte is to be injected. M And heat sealing part P H Long strips. Figure 3 The graph is a graph showing an example of the measurement results of the sealing strength of the bonding portion of the outer packaging material continuously measured from one end to the other end, and is a graph showing the sealing strength of the outer packaging material from the molten bonding portion P which is one end of the bonding portion. M A graph showing the relationship between the displacement required for peeling and the seal strength. Figure 3In the graph of , the left end represents one end in the width direction of the bonding portion, and the point where the sealing strength decreases represents the other end. Figure 3 In the curve diagram, the curve rises from one end of the bonding portion, and the sealing strength shows the maximum value. The peeling of the outer packaging material 10 is first accompanied by the melting of the sealant bonding portion 16 at one end of the bonding portion. M Destruction of the sealant melt bonding portion 16 M The maximum value in the curve is considered to be due to the sealant melt bonding portion 16. M The maximum seal strength is usually the maximum seal strength S. M In one aspect (first aspect) of the present embodiment, the maximum seal strength S when heat-sealed under the conditions of a temperature of 190° C., a pressure of 0.5 MPa, and a period of 3 seconds is 200° C. M It is 35 N / 15 mm or more, preferably 40 N / 15 mm or more, and more preferably 50 N / 15 mm or more.
[0056] Figure 3 In the curve graph, when the displacement to obtain the above maximum value is passed, the sealing strength gradually becomes stable. In this specification, the area where the sealing strength in the above curve graph is stabilized is called a stable area. The stable area is an area where the variation of the sealing strength during the measurement is less than ±3N / 15mm, and is defined as an area with a length of more than 5mm. In the first aspect of the present embodiment, when there is a stable area in the above curve graph, the outer packaging material 10 satisfies the following condition (1).
[0057] (1) The seal strength S in the above stable region when heat-sealed under the conditions of temperature 190°C, pressure 0.5 MPa, and 3 seconds S With maximum sealing strength S M Ratio S S / S M It is above 0.3.
[0058] The above ratio S S / S M It is preferably 0.5 or more, and more preferably 0.6 or more. M 35N / 15mm or more and better than S S / S M When the value is 0.3 or more, the insulation after degassing and heat sealing can be sufficiently maintained. S It is the average value of the sealing strength in the above stable area.
[0059] on the other hand, Figure 3The graph of exemplifies the measurement results when a stable region exists, but there are also cases where a stable region does not exist. Figure 4 This is a graph showing another example of the measurement results of the sealing strength of the adhesive portion of the outer packaging material measured continuously from one end to the other end, and is a graph showing the relationship between the displacement of peeling from the end of the adhesive portion and the sealing strength. Figure 4 In the curve graph of , there is no stable region after the displacement of the maximum seal strength. In the first aspect of the present embodiment, when there is no stable region in the curve graph showing the measurement result of the seal strength, the outer packaging material 10 satisfies the following condition (2).
[0060] (2) Average seal strength S from the displacement at which the maximum value is obtained to the displacement at the other end when heat sealing is performed under the conditions of a temperature of 190°C, a pressure of 0.5 MPa, and a period of 3 seconds. A With maximum sealing strength S M Ratio S A / S M It is above 0.3.
[0061] The above ratio S A / S M It is preferably 0.5 or more, and more preferably 0.6 or more. M 35N / 15mm or more and higher than S A / S M When the average seal strength S is 0.3 or more, the insulation after degassing and heat sealing can be sufficiently maintained. A The sealing strength per 1 mm displacement after the displacement of the above maximum value is measured (for example Figure 4 The sealing strengths S1, S2, S3, S4, S5, S6 in the curve diagram are obtained by calculating their average value.
[0062] In the first aspect of this embodiment, the above curve diagram may be as follows Figure 3 There is a stable region, or it can be Figure 4 There is no stable region. It is preferred that there is a stable region in the above curve graph. When the above stable region exists in the curve graph, the outer packaging material 10 satisfies the above condition (1), and when the above stable region does not exist in the curve graph, the outer packaging material 10 satisfies the above condition (2).
[0063] The improvement of the sealing strength when the outer packaging material 10 is heat-sealed is generally referred to as the sealing strength S M With sealing strength S S Or sealing strength S A However, the maximum sealing strength S M The value also varies with the sealant melt bonded portion 16 formed at the end of the bonded portion.M Therefore, the maximum sealing strength S M The value of also varies with, for example, the melt flow rate (MFR), crystallinity, thickness, etc. of the sealant layer 16, and also with the heat sealing conditions (temperature, pressure, time). S , S A And control the maximum sealing strength S M , the above ratio S can also be controlled S / S M Or the above ratio S A / S M .
[0064] (II) Second Aspect
[0065] Figure 5 The enlarged cross-sectional views schematically show the cross-sectional structure of the surface along the VD direction and the MD direction of the sealant layer of the outer packaging material for the storage device according to another aspect (the second aspect) of the present embodiment. (a) is a view before heating at 190°C for 30 seconds, and (b) is a view after heating at 190°C for 30 seconds. The MD direction is the flow direction when the sealant layer is formed, and corresponds to the so-called Machine direction. In addition, the VD direction represents the thickness direction of the sealant layer 16 (or the stacking direction of the outer packaging material 10), which is perpendicular to the surface of the sealant layer including the MD direction. In addition, the direction perpendicular to the MD direction and the VD direction is sometimes referred to as the TD direction, which corresponds to the so-called Transverse direction. The surfaces along the MD direction and the TD direction are parallel to the surface of the sealant layer, and are perpendicular to the surfaces along the VD direction and the MD direction.
[0066] Figure 5 In (a), the sealant layer 16 has a polypropylene resin (A) existence region 162 and a plurality of incompatible component (B) existence regions 164 surrounded by the polypropylene resin (A). The (B) component existence region 164 has a needle-like shape that is long in the MD direction of the sealant layer 16 and short in the VD direction. Figure 5 In (a), the length L of the region 164 containing the component (B) in the MD direction is MD and the length L in the VD direction VDis very large in comparison. The above-mentioned shape of the region 164 where the (B) component exists is derived from the method of forming the sealant layer 16. The sealant layer 16 is formed, for example, by continuously supplying, conveying or laminating a resin composition for forming a sealant layer that has been dry-mixed and melted. When a thin layer such as a sealant layer is formed, each material in the resin composition constitutes the sealant layer in a state of being thinly stretched in the MD direction. From the perspective of productivity, the formation speed (processing speed) of the sealant layer 16 can be, for example, 80 m / min or more. In this way, when the formation speed of the sealant layer 16 is above a certain level, the state in which each material is stretched in the MD direction becomes more significant. When the (B) component dispersed in the (A) component is thinly stretched in the MD direction when forming the sealant layer 16, the (B) component becomes, for example, a plurality of elliptical shapes in the cross-section along the MD direction and the TD direction, and they exist overlapping in the VD direction. Furthermore, in the cross-section along the VD direction and the MD direction of the sealant layer 16, the (B) component is as Figure 5 As shown in (a) of FIG. 1 , the existence area 164 appears in the above-mentioned needle-like shape.
[0067] (B) Average length LA of the component existence region 164 in the MD direction MD For example, it may be 2.0 to 20.0 μm, or 3.0 to 15.0 μm. In addition, the average length LA of the region 164 containing the component (B) in the VD direction is VD For example, it can be 0.1 to 1.0 μm. In addition, the average length LA of the region 164 containing the component (B) is MD , LA VD The length L of 10 or more randomly selected existing regions 164 is measured by observing the cross section along the VD direction and the MD direction of the sealant layer 16 at a magnification of about 3000 times using a scanning electron microscope (SEM) or the like. MD , L VD The average value of time.
[0068] (B) Average length LA of the component existence region 164 in the MD direction MD and the average length LA in the VD direction VD Ratio (LA MD / LA VD ) may be 10.0 or more, or 20.0 or more. The fact that the average length of the region 164 containing the component (B) satisfies the above ratio means that sufficient productivity can be ensured in the formation of the sealant layer 16.
[0069] The shape of the stretched component (B) as described above tends to be deformed into a nearly spherical shape by heating. That is, the region of the component (B) that is needle-shaped in the cross section along the VD direction and the MD direction tends to be deformed short in the MD direction and long in the VD direction when heated. In other words, the region of the component (B) may also shrink in the MD direction. Figure 5 In (b), the sealant layer 16h represents the sealant layer after being heated at 190°C for 30 seconds. The heated sealant layer 16h has a region 162h containing the heated polypropylene resin (A) and a plurality of regions 164h containing the heated incompatible components (B) surrounded by the polypropylene resin (A). The region 164h containing the component (B) is smaller in the MD direction and larger in the VD direction than the region 164 containing the component (B) before heating.
[0070] In the second aspect of the present embodiment, the outer packaging material 10 for a power storage device comprises a low-shrinkage sealant layer having a small degree of deformation and shrinkage. Figure 5 As shown in (b), the length Lh of the region 164h containing the component (B) after heating in the MD direction is MD Length L before heating MD Specifically, in the above-mentioned low shrinkage sealant layer, the average length LAh of the region where the (B) component exists after heating in the cross section along the VD direction and the MD direction in the MD direction is MD The average length LAh of the region where the (B) component exists before heating in the cross section along the VD direction and the MD direction in the MD direction MD Ratio (LAh MD / LA MD ) is 0.20 or more, preferably 0.30 or more, and more preferably 0.35 or more. MD / LA MD ) is simply referred to as the shrinkage ratio. When the shrinkage ratio is 0.20 or more, the sea-island structure composed of component (A) and component (B) has a high adhesion strength at the interface, and even when the electrolyte foams, it is difficult to generate voids in the above interface, which can suppress the reduction of insulation after degassing and heat sealing.
[0071] The average length LAh of the region 164h containing the component (B) after heating in the low-shrinkage sealant layer in the MD direction is MD For example, it may be 1.0 to 20.0 μm, or 2.0 to 15.0 μm. In addition, the average length LAh of the region 164h containing the component (B) after heating in the VD direction is VDFor example, it can be 0.1 to 2.0 μm. In addition, the average length LAh of the region 164h containing the component (B) after heating is MD LAh VD The cross section of the heated sealant layer 16h along the VD direction and the MD direction is observed using a scanning electron microscope (SEM) at a magnification of about 3000 times, and the length Lh of 10 or more randomly selected existing regions 164h is measured. MD , Lh VD The average value of time.
[0072] The average length LAh of the region 164h containing the component (B) after heating in the low-shrinkage sealant layer in the MD direction is MD and the average length LAh in the VD direction VD Ratio (LAh MD / LAh VD ) is preferably 2.50 or more, more preferably 3.00 or more, and even more preferably 5.00 or more. MD / LAh VD ) is simply referred to as aspect ratio or length-to-width ratio. The fact that the average length of the region 164 of the component (B) after heating satisfies the above ratio means that the shape of the component (B) stretched during the formation of the sealant layer is maintained after heating, and the adhesion strength of the interface of the sea-island structure is high. As a result, even when the electrolyte foams, it is difficult to generate voids in the above interface, which has a tendency to further suppress the reduction of insulation after degassing and heat sealing.
[0073] Each layer constituting the outer packaging material 10 will be described in detail below.
[0074] <Base material layer 11>
[0075] The substrate layer 11 is provided for the purpose of imparting heat resistance in the sealing process during the manufacture of the storage device, and for the purpose of preventing pinholes that may be caused during processing or circulation, and preferably a resin layer having insulating properties is used. As such a resin layer, for example, a stretched or unstretched film such as a polyester film, a polyamide film, or a polypropylene film can be used as a single layer or as a multilayer film having two or more layers stacked. In addition, a coextruded multilayer stretched film obtained by coextruding a polyethylene terephthalate (PET) film and a nylon (Ny) film using an adhesive resin and then stretching the film can also be used.
[0076] The base material layer 11 can also be provided by directly coating on the metal foil layer 13 described later. In this case, the first adhesive layer 12 described later is unnecessary. As a method for forming the base material layer by coating, a method of coating a resin coating liquid of a polyurethane resin, an acrylic resin, a polyester resin, etc., and curing it by ultraviolet irradiation, high temperature heating, aging (ripening) treatment, etc. can be adopted. The coating method is not particularly limited, and various methods such as gravure coating, reverse coating, roller coating, and rod coating can be adopted.
[0077] The thickness of the base layer 11 is preferably 3 to 40 μm, more preferably 5 to 25 μm. When the thickness of the base layer 11 is 3 μm or more, the pinhole resistance and insulation properties of the power storage device packaging material 10 tend to be improved.
[0078] <First Adhesive Layer 12>
[0079] The first adhesive layer 12 is a layer for bonding the substrate layer 11 to the metal foil layer 13. Specific examples of the material constituting the first adhesive layer 12 include polyurethane resins obtained by allowing a bifunctional or higher-functional isocyanate compound to act on a main agent such as polyester polyol, polyether polyol, acrylic polyol, carbonate polyol, and the like.
[0080] The above-mentioned various polyols can be used alone or in combination of two or more kinds depending on the function or performance required of the outer packaging material.
[0081] Furthermore, various other additives or stabilizers may be blended into the polyurethane resin according to the performance required for the adhesive.
[0082] The thickness of the first adhesive layer 12 is not particularly limited, but is preferably 1 to 10 μm, more preferably 3 to 7 μm, for example, from the viewpoint of obtaining desired adhesive strength, followability, and processability.
[0083] <Metal foil layer 13>
[0084] The metal foil layer 13 has water vapor barrier properties to prevent moisture from penetrating into the internal part of the power storage device. In addition, the metal foil layer 13 has ductility for deep drawing. As the metal foil layer 13, various metal foils such as aluminum, stainless steel, and copper can be used. From the aspects of quality (specific gravity), moisture resistance, processability, and cost, aluminum foil is preferred.
[0085] As the aluminum foil, from the aspect of being able to impart the desired ductility during molding, it is particularly preferred to use a soft aluminum foil that has been subjected to annealing treatment, and it is more preferred to use an aluminum foil containing iron in order to further impart pinhole resistance and ductility during molding. The iron content in the aluminum foil is preferably 0.1 to 9.0% by mass, more preferably 0.5 to 2.0% by mass in 100% by mass of the aluminum foil. When the iron content is 0.1% by mass or more, an outer packaging material 10 having more excellent pinhole resistance and ductility can be obtained. When the iron content is 9.0% by mass or less, an outer packaging material 10 having more excellent softness can be obtained.
[0086] The thickness of the metal foil layer 13 is not particularly limited, but is preferably 9 to 200 μm, more preferably 15 to 100 μm, in consideration of barrier properties, pinhole resistance, and processability.
[0087] When aluminum foil is used for the metal foil layer 13 , untreated aluminum foil may be used as the aluminum foil, but from the viewpoint of imparting electrolyte resistance, it is preferable to use aluminum foil subjected to a degreasing treatment.
[0088] When the aluminum foil is degreased, the degreasing treatment may be performed on only one side of the aluminum foil or on both sides.
[0089] <Anti-corrosion treatment layer 14>
[0090] The anti-corrosion treatment layer 14 is provided to prevent the electrolytic solution or hydrofluoric acid generated by the reaction between the electrolytic solution and water from corroding the metal foil layer 13. The anti-corrosion treatment layer 14 is formed, for example, by degreasing treatment, hot water deterioration treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.
[0091] As degreasing treatment, acid degreasing or alkali degreasing can be mentioned. As acid degreasing, methods using inorganic acids such as sulfuric acid, nitric acid, hydrochloric acid, and hydrofluoric acid alone or using a mixture thereof can be mentioned. In addition, as acid degreasing, by using an acid degreasing agent obtained by dissolving a fluorine-containing compound such as monosodium ammonium difluoride with the above-mentioned inorganic acid, especially when aluminum foil is used in the metal foil layer 13, not only can the degreasing effect of aluminum be obtained, but also a passive aluminum fluoride can be formed, which is effective from the aspect of hydrofluoric acid resistance. As alkali degreasing, methods using sodium hydroxide and the like can be mentioned.
[0092] Examples of the hot water modification treatment include a boehmite treatment in which the aluminum foil is immersed in boiling water to which triethanolamine is added.
[0093] Examples of the anodizing treatment include an alumite treatment.
[0094] As chemical conversion treatment, there can be cited an immersion type and a coating type. As an immersion type chemical conversion treatment, for example, there can be cited various chemical conversion treatments consisting of chromate treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment or a mixed phase thereof. On the other hand, as a coating type chemical conversion treatment, there can be cited a method of coating a coating agent having anticorrosive properties on the metal foil layer 13.
[0095] Among these anti-corrosion treatments, when at least a portion of the anti-corrosion treatment layer is formed by any of hot water deterioration treatment, anodic oxidation treatment, and chemical conversion treatment, it is preferred to perform the above-mentioned degreasing treatment in advance. In addition, when a degreased metal foil such as a metal foil that has undergone an annealing process is used as the metal foil layer 13, it is not necessary to perform degreasing treatment again in the formation of the anti-corrosion treatment layer 14.
[0096] The coating agent used in the coating type chemical conversion treatment preferably contains trivalent chromium. In addition, the coating agent may further contain at least one polymer selected from the cationic polymer and the anionic polymer described below.
[0097] In addition, in the above-mentioned treatment, especially in the hot water deterioration treatment and the anodizing treatment, the surface of the aluminum foil is dissolved by the treatment agent to form an aluminum compound (boehmite, anodic aluminum) with excellent corrosion resistance. Therefore, the metal foil layer 13 using the aluminum foil to the anti-corrosion treatment layer 14 becomes a form of a co-continuous structure, and the above-mentioned treatment is included in the definition of the chemical conversion treatment. On the other hand, as described later, the anti-corrosion treatment layer 14 can also be formed only by a pure coating technique that is not included in the definition of the chemical conversion treatment. As this method, for example, a method of using a sol of a rare earth element oxide such as cerium oxide with an average particle size of less than 100nm, which is a material having an anti-corrosion effect (inhibitor effect) of aluminum and suitable for the environment, can be cited. By using this method, even a general coating method can be used to impart an anti-corrosion effect to a metal foil such as aluminum foil.
[0098] Examples of the rare earth element oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, and ether-based solvents. Among them, water-based sols are preferred.
[0099] In the sol of the rare earth element oxide, inorganic acids such as nitric acid, hydrochloric acid, phosphoric acid or their salts, and organic acids such as acetic acid, malic acid, ascorbic acid, and lactic acid are usually used as dispersion stabilizers to stabilize the dispersion. Among these dispersion stabilizers, phosphoric acid is particularly expected to have the following effects in the outer packaging material 10: (1) stabilization of the dispersion of the sol; (2) improvement of adhesion with the metal foil layer 13 by utilizing the aluminum chelating ability of phosphoric acid; (3) imparting electrolyte resistance by capturing aluminum ions dissolved by the influence of hydrofluoric acid (forming a passive state); (4) improvement of the cohesion of the anti-corrosion treatment layer 14 (oxide layer) due to the dehydration condensation of phosphoric acid that is easy to occur even at low temperatures, etc.
[0100] As the above-mentioned phosphoric acid or its salt, orthophosphoric acid, pyrophosphoric acid, metaphosphoric acid or their alkali metal salts or ammonium salts can be cited. Among them, for the functional performance in the outer packaging material 10, condensed phosphoric acids such as trimetaphosphoric acid, tetrametaphosphoric acid, hexametaphosphoric acid, and permetaphosphoric acid or their alkali metal salts or ammonium salts are preferred. In addition, considering the dry film-forming properties (drying capacity, heat) when the anti-corrosion treatment layer 14 composed of rare earth element oxides is formed by using the sol of the above-mentioned rare earth element oxides and various coating methods, sodium salts are more preferred from the aspect of excellent dehydration condensation properties at low temperatures. As phosphates, water-soluble salts are preferred.
[0101] Regarding the ratio of phosphoric acid (or its salt) to rare earth element oxide, it is preferably 1 to 100 parts by mass relative to 100 parts by mass of rare earth element oxide. When the above ratio is 1 part by mass or more relative to 100 parts by mass of rare earth element oxide, the rare earth element oxide sol becomes more stable and the function of the outer packaging material 10 becomes better. The above ratio is more preferably 5 parts by mass or more relative to 100 parts by mass of rare earth element oxide. In addition, when the above ratio is less than 100 parts by mass relative to 100 parts by mass of rare earth element oxide, the function of the rare earth element oxide sol is improved and the performance of preventing electrolyte corrosion is excellent. The above ratio is more preferably less than 50 parts by mass, and more preferably less than 20 parts by mass relative to 100 parts by mass of rare earth element oxide.
[0102] Since the anti-corrosion treatment layer 14 formed by the rare earth element oxide sol is an aggregate of inorganic particles, there is a risk that the cohesive force of the layer itself will decrease even after the drying and curing process. Therefore, for the anti-corrosion treatment layer 14 in this case, in order to strengthen the cohesive force, it is preferably compounded with the following anionic polymer or cationic polymer.
[0103] Examples of the anionic polymer include polymers having a carboxyl group, such as poly(meth)acrylic acid (or its salt), or copolymers obtained by copolymerizing poly(meth)acrylic acid as a main component. Examples of the copolymer components of the copolymer include (meth)acrylic acid alkyl ester monomers (as the alkyl group, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, 2-ethylhexyl, cyclohexyl, etc.); (meth)acrylamide, N-alkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide (as the alkyl group, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, 2-ethylhexyl, cyclohexyl, etc.), N-alkoxy (meth)acrylamide, N,N-dialkoxy (meth)acrylamide (as the alkoxy , such as methoxy, ethoxy, butoxy, isobutoxy, etc.), amide-containing monomers such as N-hydroxymethyl (meth) acrylamide and N-phenyl (meth) acrylamide; hydroxyl-containing monomers such as 2-hydroxyethyl (meth) acrylate and 2-hydroxypropyl (meth) acrylate; glycidyl (meth) acrylate and allyl glycidyl ether; silane-containing monomers such as (meth) acryloxypropyl trimethoxysilane and (meth) acryloxypropyl triethoxysilane; isocyanate-containing monomers such as (meth) acryloxypropyl isocyanate, etc.
[0104] These anionic polymers have the effect of improving the stability of the anticorrosion treatment layer 14 (oxide layer) obtained using the rare earth element oxide sol. This is achieved through the following effects: the effect of protecting the hard and brittle oxide layer with the acrylic resin component; and the effect of capturing phosphate-derived ionic pollutants (especially sodium ions) contained in the rare earth element oxide sol (cation capture agent). That is, when the anticorrosion treatment layer 14 obtained using the rare earth element oxide sol contains alkali metal ions or alkaline earth metal ions, especially sodium, the anticorrosion treatment layer 14 becomes easy to deteriorate starting from the position containing the ions. Therefore, by fixing the sodium ions and the like contained in the rare earth element oxide sol using anionic polymers, the tolerance of the anticorrosion treatment layer 14 is improved.
[0105] The anti-corrosion treatment layer 14 composed of anionic polymer and rare earth element oxide sol has the same anti-corrosion performance as the anti-corrosion treatment layer 14 formed by chromate treatment of aluminum foil. The anionic polymer is preferably a structure formed by cross-linking a polyanionic polymer that is essentially water-soluble. As a cross-linking agent used when forming this structure, for example, compounds having an isocyanate group, a glycidyl group, a carboxyl group, and an oxazoline group can be cited.
[0106] Examples of the compound having an isocyanate group include diisocyanates such as tolylene diisocyanate, xylene diisocyanate or hydrides thereof, hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate or hydrides thereof, and isophorone diisocyanate; or polyisocyanates such as adducts obtained by reacting these isocyanates with polyols such as trimethylolpropane, biuret bodies obtained by reacting these isocyanates with water, or isocyanurate bodies as trimers; or blocked polyisocyanates obtained by blocking these polyisocyanates with alcohols, lactams, oximes, and the like.
[0107] Examples of the compound having a glycidyl group include epoxy compounds formed by reacting epichlorohydrin with diols such as ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, 1,4-butanediol, 1,6-hexanediol, and neopentyl glycol; epoxy compounds formed by reacting epichlorohydrin with polyols such as glycerol, polyglycerol, trimethylolpropane, pentaerythritol, and sorbitol; and epoxy compounds formed by reacting epichlorohydrin with dicarboxylic acids such as phthalic acid, terephthalic acid, oxalic acid, and adipic acid.
[0108] Examples of the compound having a carboxyl group include various aliphatic or aromatic dicarboxylic acids, etc. In addition, poly(meth)acrylic acid and alkali (earth) metal salts of poly(meth)acrylic acid can also be used.
[0109] Examples of the compound having an oxazoline group include compounds obtained by copolymerizing an acrylic monomer such as (meth)acrylic acid, an alkyl (meth)acrylate, or a hydroxyalkyl (meth)acrylate with a low molecular weight compound having two or more oxazoline units or a polymerizable monomer such as isopropenyl oxazoline.
[0110] In addition, the anionic polymer can also be reacted with a silane coupling agent, more specifically, the carboxyl group of the anionic polymer is selectively reacted with the functional group of the silane coupling agent to make the crosslinking point a siloxane bond. At this time, γ-glycidyloxypropyl trimethoxysilane, γ-glycidyloxypropyl triethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, γ-chloropropyl methoxysilane, vinyl trichlorosilane, γ-mercaptopropyl trimethoxysilane, γ-aminopropyl triethoxysilane, N-β (aminoethyl) -γ-aminopropyl trimethoxysilane, γ-isocyanate propyl triethoxysilane, etc. can be used. Among them, especially considering the reactivity with anionic polymers or copolymers thereof, epoxy silane, amino silane, and isocyanate silane are preferred.
[0111] The ratio of these crosslinking agents to the anionic polymer is preferably 1 to 50 parts by mass, more preferably 10 to 20 parts by mass, relative to 100 parts by mass of the anionic polymer. When the ratio of the crosslinking agent is 1 part by mass or more relative to 100 parts by mass of the anionic polymer, a crosslinked structure is easily formed sufficiently. When the ratio of the crosslinking agent is 50 parts by mass or less relative to 100 parts by mass of the anionic polymer, the pot life of the coating solution is improved.
[0112] The method of cross-linking the anionic polymer is not limited to the above-mentioned cross-linking agent, and a method of forming ionic cross-linking using titanium or zirconium compounds may be used.
[0113] As cationic polymers, polymers with amines can be cited, such as polyethyleneimine, ionic polymer complexes formed by polyethyleneimine and polymers with carboxylic acids, primary amine-grafted acrylic resins grafted with primary amines on the main acrylic acid skeleton, polyallylamine or their derivatives, cationic polymers such as aminophenol. As polyallylamine, for example, homopolymers or copolymers of allylamine, allylamine amide sulfate, diallylamine, dimethylallylamine, etc. can be cited. These amines can be free amines, or stabilized products formed by acetic acid or hydrochloric acid. In addition, maleic acid, sulfur dioxide, etc. can be used as copolymer components. Furthermore, types that are given thermal crosslinking properties by partially methoxylating primary amines can also be used, and aminophenol can also be used. Allylamine or its derivatives are particularly preferred.
[0114] The cationic polymer is preferably used in combination with a crosslinking agent having a functional group such as a carboxyl group or a glycidyl group that can react with an amine / imine. As a crosslinking agent used in combination with the cationic polymer, a polymer having a carboxylic acid that forms an ionic polymer complex with polyethyleneimine can also be used, for example, polycarboxylic acids (salts) such as polyacrylic acid or its ionic salts, or copolymers into which a comonomer is introduced, polysaccharides having a carboxyl group such as carboxymethyl cellulose or its ionic salts, etc. can be cited.
[0115] In this embodiment, the cationic polymer is also described as a component constituting the anti-corrosion treatment layer 14. This is because: when various compounds were used for in-depth research in order to impart electrolyte tolerance and hydrofluoric acid tolerance required for the outer packaging material for the storage device, it was found that the cationic polymer itself is also a compound that can impart electrolyte tolerance and hydrofluoric acid resistance. The main reason is presumed to be that the cationic group is used to capture fluoride ions (anion capture agent), thereby suppressing damage to the aluminum foil.
[0116] Cationic polymers are more preferred materials in terms of improving adhesion. In addition, cationic polymers are also water-soluble like the above-mentioned anionic polymers, so it is more preferred to form a cross-linked structure to impart water resistance. The cross-linking agent for forming a cross-linked structure in the cationic polymer can use the cross-linking agent described in the anionic polymer. When a rare earth element oxide sol is used as the anti-corrosion treatment layer 14, a cationic polymer can be used as its protective layer instead of the above-mentioned anionic polymer.
[0117] The anti-corrosion treatment layer formed by the chemical conversion treatment represented by chromate treatment is required to form an inclined structure with the aluminum foil, so the aluminum foil is treated with a chemical conversion treatment agent containing phosphoric acid, hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid or their salts, and then chromium or a chromium-free compound is allowed to act with it to form a chemical conversion treatment layer on the aluminum foil. However, since the above-mentioned chemical conversion treatment uses acid in the chemical conversion treatment agent, it will be accompanied by the deterioration of the operating environment or the corrosion of the coating device. On the other hand, the above-mentioned coating type anti-corrosion treatment layer 14 is different from the chemical conversion treatment represented by chromate treatment, and it is not necessary to form an inclined structure for the metal foil layer 13 using aluminum foil. Therefore, the properties of the coating agent will not be restricted by acidity, alkalinity, neutrality, etc., and a good operating environment can be achieved. Furthermore, from the perspective of expecting an alternative solution to the chromate treatment using chromium compounds in terms of environmental hygiene, the coating type anti-corrosion treatment layer 14 is also preferred.
[0118] Based on the above, examples of combinations of the above-mentioned coating-type anti-corrosion treatments include (1) rare earth element oxide sol only, (2) anionic polymer only, (3) cationic polymer only, (4) rare earth element oxide sol + anionic polymer (laminated composite), (5) rare earth element oxide sol + cationic polymer (laminated composite), (6) (rare earth element oxide sol + anionic polymer: laminated composite) / cationic polymer (multilayer), (7) (rare earth element oxide sol + cationic polymer: laminated composite) / anionic polymer (multilayer), etc. Among them, (1) and (4) to (7) are preferred, and (4) to (7) are particularly preferred. However, the present embodiment is not limited to the above combinations. For example, as an example of the selection of anti-corrosion treatment, cationic polymers are very preferred materials from the perspective of good adhesion to the modified polyolefin resin listed in the description of the second adhesive layer or sealant layer described later. Therefore, when the second adhesive layer or sealant layer is composed of a modified polyolefin resin, a design in which a cationic polymer is provided on the surface in contact with the second adhesive layer or sealant layer (for example, compositions (5) and (6) etc.) can be adopted.
[0119] In addition, the anti-corrosion treatment layer 14 is not limited to the aforementioned layer. For example, it can also be formed by using a treatment agent in which phosphoric acid and a chromium compound are mixed in a resin binder (aminophenol, etc.), as in the coating type chromate of the known technology. When using this treatment agent, a layer having both anti-corrosion function and tight adhesion can be made. In addition, although it is necessary to consider the stability of the coating liquid, a coating agent in which a rare earth element oxide sol and a polycationic polymer or a polyanionic polymer are made into a single liquid in advance can also be used to make a layer having both anti-corrosion function and tight adhesion.
[0120] The mass per unit area of the anticorrosion treatment layer 14 is preferably 0.005 to 0.200 g / m regardless of whether it is a multilayer structure or a single layer structure. 2 , more preferably 0.010 to 0.100 g / m 2 The mass per unit area is 0.005 g / m 2 When the weight per unit area exceeds 0.200 g / m 2 , the anti-corrosion function remains basically unchanged. When rare earth element oxide sol is used, when the coating is thick, the curing by the heat during drying becomes insufficient, and there is a risk of reduced cohesion. In addition, the thickness of the anti-corrosion treatment layer 14 can be converted by its specific gravity.
[0121] From the viewpoint of further maintaining the close adhesion between the sealant layer and the metal foil layer, preventing the occurrence of the starting point of foaming of the electrolyte, and further suppressing the reduction in insulation after degassing and heat sealing, the anti-corrosion treatment layer 14 can be, for example, a method containing cerium oxide, 1 to 100 parts by mass of phosphoric acid or phosphate relative to 100 parts by mass of the cerium oxide, and a cationic polymer. It can also be a method in which the metal foil layer 13 is subjected to a chemical conversion treatment. It can also be a method in which the metal foil layer 13 is subjected to a chemical conversion treatment and contains a cationic polymer.
[0122] <Second Adhesive Layer 17>
[0123] The second adhesive layer 17 is a layer for bonding the metal foil layer 13 on which the anticorrosion treatment layer 14 is formed and the sealant layer 16. For the second adhesive layer 17, a general adhesive for bonding a metal foil layer and a sealant layer can be used.
[0124] When the anticorrosion layer 14 has a layer containing at least one polymer selected from the cationic polymer and the anionic polymer, the second adhesive layer 17 is preferably a layer containing a compound reactive with the polymer contained in the anticorrosion layer 14 (hereinafter also referred to as a “reactive compound”).
[0125] For example, when the anticorrosion treatment layer 14 contains a cationic polymer, the second adhesive layer 17 contains a compound reactive with the cationic polymer. When the anticorrosion treatment layer 14 contains an anionic polymer, the second adhesive layer 17 contains a compound reactive with the anionic polymer. In addition, when the anticorrosion treatment layer 14 contains a cationic polymer and an anionic polymer, the second adhesive layer 17 contains a compound reactive with the cationic polymer and a compound reactive with the anionic polymer. However, the second adhesive layer 17 does not necessarily contain the above two compounds, and may also contain a compound reactive with both the cationic polymer and the anionic polymer. Here, "reactive" means forming a covalent bond with a cationic polymer or an anionic polymer. In addition, the second adhesive layer 17 may further contain an acid-modified polyolefin resin.
[0126] Examples of the compound reactive with the cationic polymer include at least one compound selected from the group consisting of a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxyl group, and a compound having an oxazoline group.
[0127] As these polyfunctional isocyanate compounds, glycidyl compounds, compounds having carboxyl groups, and compounds having oxazoline groups, polyfunctional isocyanate compounds, glycidyl compounds, compounds having carboxyl groups, and compounds having oxazoline groups, which are crosslinking agents for converting cationic polymers into crosslinked structures, can be cited. Among them, polyfunctional isocyanate compounds are preferred because of their high reactivity with cationic polymers and their ease in forming crosslinked structures.
[0128] As the compound reactive with anionic polymer, at least one compound selected from glycidyl compounds and compounds with oxazoline groups can be enumerated. As these glycidyl compounds and compounds with oxazoline groups, glycidyl compounds and compounds with oxazoline groups illustrated above as crosslinking agents for making cationic polymers into crosslinked structures can be enumerated. Among them, glycidyl compounds are preferred from the aspect of high reactivity with anionic polymers.
[0129] When the second adhesive layer 17 contains an acid-modified polyolefin resin, the reactive compound preferably also has reactivity with the acidic group in the acid-modified polyolefin resin (i.e., forms a covalent bond with the acidic group). Thus, the adhesion to the anti-corrosion treatment layer 14 is further improved. Furthermore, the acid-modified polyolefin resin becomes a cross-linked structure, and the solvent resistance of the outer packaging material 10 is further improved.
[0130] The content of the reactive compound is preferably the same equivalent to 10 times the equivalent of the acidic group in the acid-modified polyolefin resin. When it is the same equivalent or more, the reactive compound reacts sufficiently with the acidic group in the acid-modified polyolefin resin. When it exceeds 10 times the equivalent, the crosslinking reaction with the acid-modified polyolefin resin has been fully saturated, so there is a risk of unreacted products and various performance reductions. Therefore, for example, the content of the reactive compound is preferably 5 to 20 parts by mass (solid content ratio) relative to 100 parts by mass of the acid-modified polyolefin resin.
[0131] The acid-modified polyolefin resin is a resin obtained by introducing an acidic group into a polyolefin resin. Examples of the acidic group include a carboxyl group, a sulfonic acid group, an anhydride group, and the like, and maleic anhydride groups or (meth) acrylic acid groups are particularly preferred. As the acid-modified polyolefin resin, for example, the same resin as the modified polyolefin resin (a) used in the first sealant layer 16a and described later can be used.
[0132] The second adhesive layer 17 may further contain various additives such as a flame retardant, a slip agent, an anti-blocking agent, an antioxidant, a light stabilizer, and an adhesion-imparting agent.
[0133] From the viewpoint of suppressing the reduction in lamination strength when the electrolyte is involved and further suppressing the reduction in insulation, the second adhesive layer 17 may contain, for example, an acid-modified polyolefin and at least one curing agent selected from a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxyl group, a compound having an oxazoline group and a carbodiimide compound. Examples of the carbodiimide compound include N,N'-di-o-toluoylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-di-2,6-dimethylphenylcarbodiimide, N,N'-bis(2,6-diisopropylphenyl)carbodiimide, N,N'-dioctadecylcarbodiimide, N-tolyl-N'-cyclohexylcarbodiimide, N,N'-di-2,2-di-tert-butylphenylcarbodiimide, N-tolyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-cyclohexylcarbodiimide, and N,N'-di-p-toluoylcarbodiimide.
[0134] As the adhesive forming the second adhesive layer 17 , for example, a polyurethane-based adhesive in which polyester polyol composed of hydrogenated dimer fatty acid and diol and polyisocyanate are blended may be used.
[0135] The thickness of the second adhesive layer 17 is not particularly limited, but is preferably 1 to 10 μm, more preferably 3 to 7 μm, from the viewpoint of obtaining desired adhesive strength and processability.
[0136] <Sealing adhesive layer 16>
[0137] The sealant layer 16 is a layer that imparts sealing properties to the outer packaging material 10 by heat sealing.
[0138] (I) First Aspect
[0139] The sealant layer 16 of the outer packaging material of the first aspect of this embodiment is as follows. Figure 3 or Figure 4 The maximum sealing strength S M 35N / 15mm or more, and better than S S / S M Or S A / S M The following describes an example of the sealant layer 16 constituting the outer packaging material according to the first aspect of the present embodiment.
[0140] The sealant layer 16 contains a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin. The sealant layer 16 may further contain a compatible elastomer (C) that is compatible with the polypropylene resin (A). Hereinafter, depending on the circumstances, the polypropylene resin (A) is sometimes referred to as "component (A)", the incompatible component (B) that is incompatible with the component (A) is referred to as "component (B)", and the compatible elastomer (C) that is compatible with the component (A) is referred to as "compatible elastomer (C)" or "component (C)". Here, "no compatibility with component (A)", "incompatible with component (A)" (incompatible) means that the dispersed phase size is greater than 200 nm and less than 50 μm and is dispersed in the polypropylene resin constituting component (A). “Compatible with component (A)” or “compatible with component (A)” (compatible) means being dispersed in the polypropylene resin constituting component (A) with a dispersed phase size of 1 nm or more and less than 200 nm.
[0141] In the sealant layer 16, the incompatible component (B) preferably contains a compound (B1) having a compatible portion with the polypropylene resin (A). Hereinafter, the compound (B1) having a compatible portion with the above-mentioned component (A) may be referred to as "compound (B1)" or "(B1) component", etc., depending on the circumstances. The incompatible component (B) may also be composed of only the compound (B1).
[0142] The sealant layer 16 contains the above-mentioned (A) component and the above-mentioned (B) component, and forms an island structure in the sealant layer 16, which can improve the sealing strength after heat sealing. The sealant layer 16 further contains the above-mentioned (C) component, which can further impart flexibility to the sealant layer 16. The sealant layer 16 has flexibility, and can impart functions such as molding whitening inhibition, so that an outer packaging material with further improved functionality can be provided.
[0143] An example of the sealant layer 16 will be described below.
[0144] (Polypropylene resin (A))
[0145] The polypropylene resin (A) is a resin obtained from a polymerized monomer containing propylene. Examples of the polypropylene resin (A) include homopolypropylene and random polypropylene. From the perspective of basic performance of outer packaging materials such as heat seal strength, the polypropylene resin (A) is preferably random polypropylene, and more preferably a propylene-ethylene random copolymer. The propylene-ethylene random copolymer has excellent heat sealability at low temperatures and can improve the sealing properties related to the electrolyte.
[0146] In the propylene-ethylene random copolymer, the ethylene content is preferably 0.1 to 10% by mass, more preferably 1 to 7% by mass, and further preferably 2 to 5% by mass. When the ethylene content is 0.1% by mass or more, the melting point lowering effect caused by ethylene copolymerization can be fully obtained, the sealing characteristics related to the electrolyte can be further improved, and the impact resistance can be obtained, and there is a tendency to improve the sealing strength or the resistance to molding whitening. When the ethylene content is 10% by mass or less, the melting point can be suppressed from being excessively lowered, and the maximum sealing strength S can be suppressed. M Too high (that is, it can increase the ratio S S / S M In addition, the ethylene content can be calculated from the mixing ratio of the monomers during polymerization.
[0147] The melting point of the propylene-ethylene random copolymer is preferably 120 to 145° C., more preferably 125 to 140° C. When the melting point is 120° C. or higher, the maximum seal strength S M becomes too high (i.e., it can increase the ratio S S / S M When the melting point is 145° C. or lower, there is a tendency that the sealing properties related to the electrolyte can be further improved.
[0148] The propylene-ethylene random copolymer may be an acid-modified copolymer, for example, an acid-modified propylene-ethylene random copolymer obtained by grafting maleic anhydride. By using the acid-modified propylene-ethylene random copolymer, even without the tab sealant, the adhesion with the tab wire can be maintained.
[0149] The propylene-ethylene random copolymer may be used alone or in combination of two or more.
[0150] In the sealant layer 16, the content of the component (A) can be 50 to 99% by mass, 50 to 95% by mass, or 50 to 85% by mass, based on the total solid content of the sealant layer 16. By making the content of the component (A) 50% by mass or more, the sealing properties can be improved by utilizing the effect of using the component (A) itself. In addition, by making the content of the component (A) 50% by mass or more, since the excessive presence of the component (B) can be prevented, the reduction of the heat resistance and cohesion of the sealant layer 16 can be suppressed. On the other hand, by making the content of the component (A) 99% by mass or less, since the component (B) of 1% or more by mass can be contained, the sealing strength and insulation brought by the component (B) can be improved.
[0151] (Incompatible component (B))
[0152] Examples of the incompatible component (B) include graft copolymers, block copolymers, and random copolymers, etc. At least a part of these copolymers has an incompatible portion with the component (A).
[0153] The incompatible component (B) preferably contains a compound (B1) having a compatible portion with the polypropylene resin (A). In other words, the compound (B) preferably has a compatible portion and an incompatible portion with the polypropylene resin (A). By containing the compound (B1), the incompatible component (B) can improve the adhesion strength of the above-mentioned sea-island interface of the sea-island structure formed by the components (A) and (B), and inhibit the formation of voids accompanying the foaming of the electrolyte, thereby further improving the insulation. In addition, due to the improvement in the adhesion strength of the sea-island interface generated by the compound (B1), the above-mentioned sealing strength S can also be improved. M , S S or S A . Such a compound (B1) can be obtained, for example, when the incompatible component (B) is a graft copolymer or a block copolymer. Preferred graft copolymers of the compound (B1) include graft copolymers formed by the main chain of a polyolefin and the side chain of polystyrene, graft copolymers formed by the main chain of a polyolefin and the side chain of a styrene-acrylonitrile copolymer, and the like. As the above-mentioned graft copolymer, for example, "Modiper" manufactured by NOF Corporation is suitable.
[0154] As the preferred block copolymer of compound (B1), there can be enumerated a block copolymer having a block consisting of styrene units and a block consisting of ethylene-butylene units, a block copolymer having a block consisting of styrene units, a block copolymer having a block consisting of ethylene-butylene units and a block copolymer consisting of crystalline olefin units, a block copolymer having a block consisting of crystalline ethylene units and a block copolymer consisting of ethylene-butylene units, a block copolymer having a block consisting of ethylene and a block consisting of ethylene-octene 1, and a block copolymer having a block consisting of propylene units and a block copolymer consisting of ethylene units. For example, the block consisting of propylene units is a compatible portion with the above-mentioned (A) component, and the block consisting of ethylene units is an incompatible portion with the above-mentioned (A) component. As the above-mentioned block copolymer, for example, "DYNARON" made by JSR Corporation, "INTUNE" and "INFUSE" made by DOW Corporation are suitable.
[0155] The incompatible component (B) may also contain an incompatible elastomer. As an incompatible elastomer, a polyolefin elastomer with an alpha olefin as a comonomer may be cited. In particular, by using an ethylene-alpha olefin copolymer, there is a tendency to impart functionality to the sealant layer 16 without reducing the electrolyte lamination strength or various sealing strengths related to the electrolyte. As an ethylene-alpha olefin copolymer, a compound obtained by copolymerizing at least one alpha olefin selected from 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene with ethylene may be used, and an ethylene-butene-1 random copolymer obtained by copolymerizing 1-butene with ethylene may be preferably used. As an ethylene-alpha olefin copolymer, "TAFMER" manufactured by Mitsui Chemicals, "EXCELLEN" manufactured by Sumitomo Chemical, etc. are suitable.
[0156] The sealant layer 16 can contain the polypropylene resin (A) and the incompatible component (B) by preparing a dispersion in which an incompatible component (B) is dispersed in a polypropylene resin (A), and by using the dispersion. As such a dispersion, a dispersion in which an elastomer is finely dispersed in a polypropylene resin can be cited. The sealant layer 16 contains a dispersion in which the incompatible component (B) is pre-dispersed in a polypropylene resin (A), and has a tendency to further improve the insulation and sealing strength. The incompatible component (B) in the above-mentioned dispersion preferably contains a graft copolymer or a block copolymer. The incompatible component (B) in the dispersion has a tendency to further improve the adhesion of the sea-island interface by containing a graft copolymer or a block copolymer.
[0157] As an example of a dispersion in which an incompatible component (B) is dispersed in a polypropylene resin (A), and the incompatible component (B) contains a graft copolymer, a dynamically crosslinked PP elastomer (TPV) (using peroxide) and the like can be cited. A dynamically crosslinked PP elastomer (TPV) is a dispersion in which a crosslinked elastomer is finely dispersed in polypropylene, and the crosslinked elastomer is grafted, and the grafted portion constitutes an interface with the polypropylene. In the dynamically crosslinked PP elastomer (TPV), polypropylene is equivalent to the component (A), and the grafted elastomer is equivalent to the compound (B1). In addition, as an example of a dispersion in which an incompatible component (B) is dispersed in a polypropylene resin (A), block polypropylene and the like can be cited. Block polypropylene is composed of homopolypropylene and an ethylene elastomer component that is incompatible with it. In block polypropylene, homopolypropylene is equivalent to the component (A), and the ethylene elastomer component is equivalent to the component (B). Furthermore, as a dispersion formed by finely dispersing an elastomer in a polypropylene resin, a reactor-type TPO can be cited. In the reactor-type TPO, the polypropylene resin corresponds to the component (A), and the elastomer corresponds to the component (B). As reactor-type TPO, for example, "Zelas" manufactured by Mitsubishi Chemical Corporation, "Catalloy" manufactured by Montell, "WELNEX" manufactured by Japan Polypropylene Co., Ltd., and "PRIME TPO" manufactured by Prime Polymer Co., Ltd. are suitable.
[0158] As the incompatible component (B), olefin-based materials and styrene-based materials are described above. From the viewpoint of electrolyte resistance, the incompatible component (B) is preferably an olefin-based material.
[0159] (Compatible elastomer (C))
[0160] As the compatible elastomer (C), for example, propylene-α-olefin copolymers can be cited. By using propylene-α-olefin copolymers, functionality can be imparted to the sealant layer 16 without reducing the electrolyte lamination strength and various sealing strengths related to the electrolyte. As the propylene-α-olefin copolymer, a polymer obtained by copolymerizing propylene with an α-olefin selected from 1-butene, 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene can be used, and a propylene-butene-1 random copolymer obtained by copolymerizing 1-butene can be preferably used.
[0161] The melting point of the polyolefin elastomer is preferably below 150°C. S / S M, suppressing molding whitening and improving the sealing properties related to the electrolyte, it is preferably 60 to 120°C, and more preferably 65 to 90°C. By setting the melting point to 150°C or less, the sealing properties related to the electrolyte, especially the degassing heat seal strength, can be improved. In addition, when the melting point is above 60°C, the ratio S S / S M is beneficial from the point of view.
[0162] The polyolefin-based elastomer may be used alone or in combination of two or more.
[0163] In the sealant layer 16, the content of the component (B) is 1 to 40% by mass, preferably 5 to 25% by mass, based on the total solid content of the sealant layer 16. By making the content of the component (B) 1% or more by mass, the sealant layer 16 can be given impact resistance, and the sealing strength and insulation can be improved. On the other hand, by making the content of the component (B) 40% or less by mass, the overall cohesion of the sealant layer 16 can be improved, and the sealing strength and insulation can be improved. In addition, for convenience, a dispersion in which an elastomer is finely dispersed in a polypropylene resin is recorded as an incompatible component (B), but in the above-mentioned dispersion, the elastomer portion is classified as the component (B) and the polypropylene resin is classified as the above-mentioned component (A).
[0164] When the sealant layer 16 contains the component (C), the content of the component (C) in the sealant layer 16 is 5 to 30% by mass, preferably 10 to 25% by mass, based on the total solid content of the sealant layer 16. When the content of the component (C) is 5% by mass or more, the sealant layer 16 is easily flexible, and functions such as whitening suppression can be imparted to the molded product, so that an outer packaging material with further improved functionality can be provided. When the content of the component (C) is 30% by mass or less, the cohesive force of the entire sealant layer 16 can be increased, and the sealing strength and insulation can be increased.
[0165] In addition, the content ratio (M) of the compatible elastomer (C) to the incompatible component (B) is C / M B ) is preferably 0.2 to 3.0, more preferably 0.3 to 2.0 in terms of mass ratio. C / M B ) is within the above range, the maximum sealing strength S can be improved with good balance M With sealing strength S S , S A .
[0166] When the incompatible component (B) contains the compound (B1), the content of the compound (B1) in the sealant layer 16 is preferably 1 to 40% by mass, more preferably 2 to 25% by mass, based on the total amount of the sealant layer. When the content of the compound (B1) is 1% by mass or more, it is easy to improve the adhesion strength of the sea-island interface, and it is easy to obtain the effect of improving the sealing strength and insulation. When the content of the compound (B1) is 40% by mass or less, it is easy to suppress the reduction of the cohesive force of the sealant layer 16 as a whole and the sealing strength and insulation.
[0167] (Added Ingredients)
[0168] The sealant layer 16 may further contain other ingredients in addition to the above-mentioned (A) to (C) components. As other ingredients in addition to the (A) to (C) components, for example, in order to improve the receiving property and processability, other resins such as LDPE (low-density polyethylene) may be added. The content of the other added resin components is preferably 10 parts by mass or less when the total mass of the sealant layer 16 is 100 parts by mass. In addition, as ingredients other than the resin, for example, slip agents, anti-blocking agents, antioxidants, light stabilizers, flame retardants, etc. can be cited. The content of other ingredients other than these resins is preferably 5 parts by mass or less when the total mass of the sealant layer 16 is 100 parts by mass.
[0169] The presence of α-olefin in the sealant layer 16 can be confirmed by attribution using FT-IR (Fourier transform infrared spectrophotometer). In addition, the content of α-olefin can be confirmed by using a sealant layer 16 formulated with a known amount of an elastomer containing a known amount of α-olefin and preparing a standard curve using the transmittance or absorbance of the characteristic absorption bands of components (A) to (C). Furthermore, the α-olefin content of each of the incompatible component (B) and the compatible elastomer (C) can also be confirmed by imaging using the characteristic absorption bands of FT-IR and mapping using the absorption bands caused by butene-1 using microscopic FT-IR (transmission method). In addition, in addition to FT-IR, the presence and content of butene-1 can also be confirmed by measuring the sealant layer 16 using NMR.
[0170] The thickness of the sealant layer 16 is not particularly limited, and is, for example, 5 to 100 μm. Based on the requirement for miniaturization of the power storage device, it can be 10 to 80 μm, 10 to 60 μm, 10 to 45 μm, or less than 30 μm. Even if the outer packaging material for the power storage device of this embodiment is made of such a film, it can suppress the reduction of insulation after heat sealing, molding, and degassing heat sealing.
[0171] Preferred embodiments of the packaging material for a power storage device according to the first aspect of the present embodiment have been described in detail above, but the present invention is not limited to the specific embodiments, and various modifications and changes can be made within the scope of the gist of the present invention described in the claims.
[0172] For example, Figure 1 Although the case where the anti-corrosion treatment layer 14 is formed on the surface of the second adhesive layer 17 side of the metal foil layer 13 is shown, the anti-corrosion treatment layer 14 may be formed on the surface of the first adhesive layer 12 side of the metal foil layer 13, or may be formed on both surfaces of the metal foil layer 13. When the anti-corrosion treatment layer 14 is formed on both surfaces of the metal foil layer 13, the structure of the anti-corrosion treatment layer 14 formed on the first adhesive layer 12 side of the metal foil layer 13 and the structure of the anti-corrosion treatment layer 14 formed on the second adhesive layer 17 side of the metal foil layer 13 may be the same as or different from each other.
[0173] Figure 1 FIG. 4 shows a case where the metal foil layer 13 and the sealant layer 16 are laminated using the second adhesive layer 17. Figure 6 The outer packaging material 20 for the power storage device shown in FIG. Figure 7 As shown in the outer packaging material 30 for a power storage device, the sealant layer 16 may be formed directly on the metal foil layer 13 without passing through the second adhesive layer 17. Figure 6 The outer packaging material 20 for the power storage device shown in FIG. Figure 7 The illustrated power storage device packaging material 30 may include a second adhesive layer 17 between the metal foil layer 13 and the sealant layer 16 .
[0174] Figure 1 The sealant layer 16 is shown as a single layer, but the sealant layer 16 can also be formed as Figure 6 The outer packaging material 20 for the power storage device shown in FIG. Figure 7 The sealant layer 16 is formed of a plurality of layers, such as the outer packaging material 30 for a storage device shown in FIG. 1 . The configurations of the layers forming the sealant layer 16 may be the same or different. In addition, when the sealant layer 16 is a plurality of layers, at least one of the layers is preferably a layer containing a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin, and the incompatible component (B) contains the compound (B1).
[0175] Figure 6In the outer packaging material 20 for a power storage device shown, the sealant layer 16 is composed of a first sealant layer 16a and a second sealant layer 16b. Here, the first sealant layer 16a is the outermost layer of the sealant layer, and the second sealant layer 16b is the innermost layer of the sealant layer. At least one layer selected from the first sealant layer 16a and the second sealant layer 16b is preferably a layer containing a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin, and the incompatible component (B) contains a compound (B1).
[0176] The second sealant layer 16b (innermost layer) can be formed using, for example, the same constituent components as the sealant layer 16 of the outer packaging material 10. When the incompatible component (B) in the second sealant layer 16b contains the compound (B1), a decrease in insulation properties can be easily suppressed.
[0177] In addition, in the second sealant layer 16 b , the incompatible component (B) may not contain the compound (B1).
[0178] The thickness of the second sealant layer 16 b may be, for example, 5 to 100 μm, and from the viewpoint of thinning, may be 10 to 60 μm, 10 to 40 μm, 10 to 30 μm, or 20 μm or less.
[0179] The first sealant layer 16a (outermost layer, layer on one side of the metal foil) can be formed, for example, using the same constituents as the second sealant layer 16b, but in the first sealant layer 16a, instead of the same constituents as the second sealant layer 16b, it is preferred to use an adhesive constituent containing an additive component as required in consideration of aluminum treatment and adhesion. As the first sealant layer 16a, by using the above-mentioned adhesive constituent, a sealant layer can be formed on the metal foil layer without an adhesive layer. When the first sealant layer 16a and the second sealant layer 16b contain components equivalent to the above-mentioned (A) component and (B) component, the first sealant layer 16a forms an island structure, and the incompatible component (B) in the first sealant layer 16a contains a compound (B1), the adhesion of the island interface can be improved, and it is easy to maintain the adhesion of the sealant layer and the metal foil layer, prevent the occurrence of voids associated with the foaming of the electrolyte, and have a tendency to further suppress the reduction of insulation after degassing heat sealing.
[0180] The adhesive constituents in the first sealant layer 16a are not particularly limited, and preferably contain a modified polypropylene resin (i) component as component (A) and a macroscopic phase separation thermoplastic elastomer (ii) component as component (B). In addition, the additive component preferably contains atactic polypropylene or atactic propylene-α-olefin copolymer (iii). Each component is described below.
[0181] (Modified polypropylene resin (i))
[0182] The modified polyolefin resin (i) is preferably a resin obtained by graft-modifying a polypropylene-based resin with an unsaturated carboxylic acid derivative component derived from any of an unsaturated carboxylic acid, an anhydride of an unsaturated carboxylic acid, and an ester of an unsaturated carboxylic acid.
[0183] Examples of the polypropylene-based resin include homopolypropylene and random polypropylene.
[0184] Examples of the compound used when graft-modifying these polypropylene-based resins include unsaturated carboxylic acid derivative components derived from any of unsaturated carboxylic acids, anhydrides of unsaturated carboxylic acids, and esters of unsaturated carboxylic acids.
[0185] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid.
[0186] Examples of the anhydride of unsaturated carboxylic acid include anhydrides of unsaturated carboxylic acids such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride.
[0187] Examples of the ester of unsaturated carboxylic acid include esters of unsaturated carboxylic acids such as methyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, dimethyl maleate, monomethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconic acid, dimethyl tetrahydrophthalic anhydride, and dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate.
[0188] The modified polypropylene resin (i) can be manufactured by graft polymerization (graft modification) of 0.2 to 100 parts by mass of the unsaturated carboxylic acid derivative component in the presence of a free radical initiator relative to 100 parts by mass of the polypropylene resin serving as the matrix. The reaction temperature of the graft modification is preferably 50 to 250° C., more preferably 60 to 200° C. In addition, the reaction time is appropriately set according to the manufacturing method. For example, when melt graft polymerization is performed using a twin-screw extruder, the residence time of the extruder is specifically preferably 2 to 30 minutes, more preferably 5 to 10 minutes. In addition, the graft modification can be implemented under any condition of normal pressure or pressurization.
[0189] Examples of the radical initiator used for graft modification include organic peroxides such as alkyl peroxides, aryl peroxides, acyl peroxides, ketone peroxides, peroxyketals, peroxycarbonates, peroxyesters, and hydrogen peroxide.
[0190] These organic peroxides can be appropriately selected and used according to the above-mentioned reaction temperature or reaction time conditions. For example, in the case of melt graft polymerization using a twin-screw extruder, alkyl peroxides, peroxyketals, and peroxyesters are preferred, and specifically, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di-tert-butyl peroxy-hexyne-3, diisopropylphenyl peroxide, etc. are preferred.
[0191] As the modified polypropylene resin (i), it is preferred that it is modified with maleic anhydride, such as "ADMER" manufactured by Mitsui Chemicals, "Modic" manufactured by Mitsubishi Chemical Corporation. Such modified polyolefin resin (i) has excellent reactivity with various metals or polymers having various functional groups, and thus the reactivity can be utilized to impart adhesion to the first sealant layer 16a, thereby improving electrolyte resistance.
[0192] (Macroscopic phase separation thermoplastic elastomer (ii))
[0193] The macro-phase-separated thermoplastic elastomer (ii) forms a macro-phase-separated structure with respect to the modified polyolefin resin (i) in which the dispersed phase size is in the range of more than 200 nm and 50 μm or less.
[0194] The first sealant layer 16a can release the residual stress generated when laminating the modified polyolefin resin (i) component that can become the main component of the first sealant layer 16a by containing the macro-phase separation thermoplastic elastomer (ii), and can impart viscoelastic adhesion to the first sealant layer 16a. Therefore, the adhesion of the first sealant layer 16a is further improved, and an outer packaging material 20 with better electrolyte resistance can be obtained. By containing the macro-phase separation thermoplastic elastomer (ii) in the first sealant layer 16a, the sealant layer 16 can be given impact resistance, and the sealing strength and insulation can be improved.
[0195] The macroscopic phase separation thermoplastic elastomer (ii) exists in the modified polypropylene resin (i) in the form of an island, but when the dispersed phase size is below 200nm, it is difficult to impart viscoelastic adhesion improvement. On the other hand, when the dispersed phase size exceeds 50μm, since the modified polypropylene resin (i) and the macroscopic phase separation thermoplastic elastomer (ii) are essentially incompatible, the lamination suitability (processability) is significantly reduced, and the physical strength of the first sealant layer 16a is easily reduced. Therefore, the dispersed phase size is preferably 500nm to 10μm.
[0196] Examples of such macro-phase-separated thermoplastic elastomers (ii) include polyethylene-based thermoplastic elastomers obtained by copolymerizing ethylene with an α-olefin selected from 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene.
[0197] As the macro-phase separation thermoplastic elastomer (ii), commercially available products can be used, and suitable examples include "TAFMER" manufactured by Mitsui Chemicals, Inc., "Zelas" manufactured by Mitsubishi Chemical Corporation, and "Catalloy" manufactured by Montell Corporation.
[0198] In the first sealant layer 16a, the content of the macro-phase separation thermoplastic elastomer (ii) relative to the modified polypropylene resin (i) is preferably 1 to 40 parts by mass, more preferably 5 to 30 parts by mass relative to 100 parts by mass of the modified polypropylene resin (i) component. Here, when the content of the macro-phase separation thermoplastic elastomer (ii) is less than 1 part by mass, it is impossible to expect an improvement in the adhesion of the first sealant layer. When the content of the macro-phase separation thermoplastic elastomer (ii) exceeds 40 parts by mass, since the compatibility of the modified polypropylene resin (i) and the macro-phase separation thermoplastic elastomer (ii) is low, the processability is easy to be significantly reduced. In addition, since the macro-phase separation thermoplastic elastomer (ii) component is not a resin showing adhesion, the adhesion of the first sealant layer 16a to other layers such as the second sealant layer 16b or the anti-corrosion treatment layer 14 becomes easy to be reduced.
[0199] (Atactic polypropylene or atactic propylene-α-olefin copolymer (iii))
[0200] The first sealant layer 16a preferably contains atactic polypropylene or atactic propylene-α-olefin copolymer (hereinafter referred to as "component (iii)") as an additive component. Here, component (iii) is a completely amorphous resin component. By containing component (iii), the first sealant layer 16a can impart flexibility to the sealant layer 16. By making the sealant layer 16 flexible, functions such as molding whitening inhibition can be imparted to the outer packaging material 10, and an outer packaging material with further improved functionality can be provided.
[0201] Furthermore, the first sealant layer 16a may further contain, as an additive component, a propylene-α-olefin copolymer having an isotactic structure corresponding to the component (C) in addition to the component (iii) in order to impart flexibility.
[0202] In the first sealant layer 16a, the total mass of the components (i) and (ii) may be, for example, 60% to 95% by mass, or 70% to 90% by mass, based on the total mass of the first sealant layer 16a.
[0203] In the first sealant layer 16a, the mass of the component (iii) is preferably 5% by mass or more and 40% by mass or less based on the total mass of the components (i), (ii) and (iii). When the mass of the component (iii) is 5% by mass or more based on the total mass of the components (i), (ii) and (iii), there is a tendency to easily obtain the effect brought about by adding the above-mentioned additive. On the other hand, when the mass of the component (iii) is 40% by mass or less based on the total mass of the components (i), (ii) and (iii), there is a tendency that the adhesion of the first sealant layer 16a to other layers such as the second sealant layer 16b or the anti-corrosion treatment layer 14 is easily reduced. From these viewpoints, in the first sealant layer 16a, the total mass of the components (i) and (ii) is preferably 60 to 95% by mass based on the total mass of the components (i), (ii) and (iii).
[0204] In addition, as a method for analyzing the component (iii) as an additive component in the first sealant layer 16a, for example, it is possible to quantify the amount by evaluating stereoregularity using nuclear magnetic resonance spectroscopy (NMR).
[0205] In addition to the adhesive constituent components (i.e., modified polypropylene resin (i) and macro-phase separated thermoplastic elastomer (ii)) and additive components (i.e., component (iii)), the first sealant layer 16a may also contain various additives as needed, such as flame retardants, slip agents, anti-blocking agents, antioxidants, light stabilizers, adhesion agents, etc.
[0206] The thickness of the first sealant layer 16 a is not particularly limited, but is preferably the same as or less than the thickness of the second sealant layer 16 b from the viewpoint of stress relaxation and water / electrolyte permeation.
[0207] In addition, in the outer packaging material 20 for storage device, from the viewpoint of thin film, the thickness of the sealant layer 16 (the total thickness of the first sealant layer 16a and the second sealant layer 16b) can be 10 to 80 μm, 10 to 60 μm, 10 to 45 μm, or less than 30 μm. Even if the outer packaging material for storage device of the present embodiment is such a thin film, the decrease in insulation after heat sealing, molding and degassing heat sealing can be suppressed.
[0208] Figure 6 The sealant layer 16 is shown as being formed of two layers, but the sealant layer 16 may also be formed of two layers. Figure 7 The outer packaging material 30 for a power storage device shown in the figure is formed of three layers. Figure 7In the outer packaging material 30 for a storage device shown, the sealant layer 16 is composed of a first sealant layer 16a, a second sealant layer 16b and a third sealant layer 16c. Here, the first sealant layer 16a is the outermost layer of the sealant layer (the layer on the metal foil side), the third sealant layer 16c is the middle layer of the sealant layer, and the second sealant layer 16b is the innermost layer of the sealant layer. At least one layer selected from these three layers is preferably a layer containing a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin, and the incompatible component (B) contains a compound (B1).
[0209] Examples and preferred aspects of the material constituting the first sealant layer 16 a of the power storage device packaging material 30 are the same as those of the first sealant layer 16 a of the power storage device packaging material 20 .
[0210] Examples and preferred aspects of the materials constituting the second sealant layer 16 b and the third sealant layer 16 c of the power storage device packaging material 30 are the same as those of the second sealant layer 16 b of the power storage device packaging material 20 .
[0211] In the outer packaging material 30 for the storage device, the thickness of the first sealant layer 16a can be, for example, 2 to 30 μm, 5 to 20 μm, or 8 to 10 μm, the thickness of the second sealant layer 16b can be, for example, 5 to 80 μm, 13 to 40 μm, or 15 to 20 μm, and the thickness of the third sealant layer 16c can be, for example, 2 to 30 μm, 5 to 20 μm, or 8 to 10 μm.
[0212] In the outer packaging material 30 for storage device, from the viewpoint of thin film, the thickness of the sealant layer 16 (the total thickness of the first sealant layer 16a, the second sealant layer 16b and the third sealant layer 16c) can be 30 μm or less. Even if the outer packaging material for storage device of this embodiment is such a thin film, it is possible to suppress the reduction of insulation after heat sealing, molding and degassing heat sealing.
[0213] When the sealant layer is composed of a plurality of layers as in the outer packaging materials 20 and 30 for power storage devices, the content of the incompatible component (B) in the sealant layer 16 is 1 to 40% by mass, preferably 1 to 35% by mass, and more preferably 2 to 25% by mass based on the total amount of the sealant layer 16. The content of the components of each layer is adjusted so that the content of the component (B) in the entire sealant layer 16 is within the above range.
[0214] When the sealant layer is composed of multiple layers, such as the outer packaging materials 20 and 30 for storage devices, it is preferred that the incompatible component (B) contains the compound (B1) in the first sealant layer 16a closest to the metal foil layer 13. In the first sealant layer 16a, the incompatible component (B) contains the compound (B1), which can improve the adhesion strength of the sea-island interface and inhibit the formation of voids accompanied by electrolyte foaming, so there is a tendency to further improve the insulation after degassing heat sealing. Electrolyte foaming during degassing heat sealing often occurs in the portion of the sealant layer 16 close to the metal foil layer 13. In the layer closest to the metal foil layer 13, the incompatible component (B) contains the compound (B1), which has a tendency to more effectively inhibit the reduction of insulation. In the first sealant layer 16a, when the incompatible component (B) contains the compound (B1), the content of the compound (B1) is preferably 1 to 40 parts by mass, and more preferably 2 to 25 parts by mass based on the total amount of the first sealant layer 16a.
[0215] When the content of the compound (B1) in the first sealant layer 16a is 1 part by mass or more, sealing strength and insulation are easily obtained. In addition, when the content of the compound (B1) is 40 parts by mass or less, it is easy to suppress the reduction of the cohesive force of the entire sealant layer and the sealing strength and insulation.
[0216] In addition, in the second sealant layer 16b or the third sealant layer 16c, the incompatible component (B) may also contain a compound (B1). By containing the compound (B1) in the second sealant layer 16b or the third sealant layer 16c, the adhesion strength of the sea-island interface formed by the components (A) and (B) can be improved, and the formation of voids accompanying the foaming of the electrolyte can be suppressed, thereby further improving the insulation. In the second sealant layer 16b, when the incompatible component (B) contains the compound (B1), the content of the compound (B1) in the second sealant layer 16b is preferably 1 to 40 parts by mass, more preferably 2 to 20 parts by mass, and further preferably 2 to 15 parts by mass, based on the total amount of the second sealant layer 16b.
[0217] The content of the compound (B1) in the third sealant layer 16c is preferably 1 to 40 parts by mass, more preferably 2 to 20 parts by mass, and even more preferably 2 to 15 parts by mass, based on the total amount of the third sealant layer 16c.
[0218] In addition, in either case where the sealant layer is composed of a single layer or a plurality of layers, the content of compound (B1) in the sealant layer is preferably 1 to 40 parts by mass, more preferably 2 to 20 parts by mass, and even more preferably 2 to 15 parts by mass based on the total amount of the sealant layer, from the viewpoint of suppressing the reduction in insulation after degassing and heat sealing while maintaining many other properties.
[0219] (II) Second Aspect
[0220] The sealant layer 16 of the outer packaging material of the second aspect of the present embodiment comprises a low shrinkage sealant layer. The low shrinkage sealant layer has a ratio (LAh MD / LA MD ) is configured to be 0.20 or more. An example of the sealant layer 16 constituting the outer packaging material of the second aspect of the present embodiment will be described below.
[0221] The sealant layer 16 is a layer that imparts sealing properties to the outer packaging material 10 by heat sealing. The sealant layer 16 contains a polypropylene resin (A) and an incompatible component (B) that is incompatible with the above-mentioned polypropylene resin. The sealant layer 16 may further contain a compatible elastomer (C) that is compatible with the polypropylene resin (A). Hereinafter, depending on the circumstances, the above-mentioned polypropylene resin (A) is sometimes referred to as "(A) component", the incompatible component (B) that is incompatible with the above-mentioned (A) component is referred to as "(B) component", and the compatible elastomer (C) that is compatible with the above-mentioned (A) component is referred to as "(C) component", etc.
[0222] In the sealant layer 16, the incompatible component (B) preferably contains a compound (B1) having a compatible portion with the polypropylene resin (A). Hereinafter, the compound (B1) having a compatible portion with the above-mentioned component (A) may be referred to as "compound (B1)" or "(B1) component", etc., depending on the circumstances. The incompatible component (B) may also be composed of only the compound (B1).
[0223] The sealant layer 16 contains the above-mentioned (A) component and the above-mentioned (B) component, and forms an island structure in the sealant layer 16. That is, the sealant layer 16 has a region where the polypropylene resin (A) exists and a plurality of regions where the incompatible components (B) exist surrounded by the above-mentioned polypropylene resin (A). In this way, the sealing strength after heat sealing can be improved. The sealant layer 16 can be further given flexibility by further containing the above-mentioned (C) component. The sealant layer 16 can be given functions such as molding whitening inhibition by having flexibility, and can provide an outer packaging material with further improved functionality.
[0224] An example of the sealant layer 16 will be described below.
[0225] (Polypropylene resin (A))
[0226] The polypropylene resin (A) is a resin obtained from a polymerization monomer containing propylene. Examples of the polypropylene resin (A) include homopolypropylene and random polypropylene. From the perspective of basic performance of outer packaging materials such as heat seal strength, the polypropylene resin (A) is preferably random polypropylene, and more preferably a propylene-ethylene random copolymer. The propylene-ethylene random copolymer has excellent heat sealability at low temperatures and can improve the sealing properties related to the electrolyte.
[0227] In the propylene-ethylene random copolymer, the ethylene content is preferably 0.1 to 10% by mass, more preferably 1 to 7% by mass, and further preferably 2 to 5% by mass. When the ethylene content is 0.1% by mass or more, the melting point reduction effect caused by ethylene copolymerization can be fully obtained, the sealing characteristics related to the electrolyte can be further improved, and the impact resistance can be obtained, and there is a tendency to improve the sealing strength or the resistance to molding whitening. When the ethylene content is 10% by mass or less, the melting point can be suppressed from being too low, and there is a tendency to be able to further fully suppress the generation of the excess sealing part. In addition, the ethylene content can be calculated from the mixing ratio of the monomers during polymerization.
[0228] The melting point of the propylene-ethylene random copolymer is preferably 120 to 145° C., more preferably 125 to 140° C. When the melting point is 120° C. or higher, the occurrence of excess sealing portions tends to be further sufficiently suppressed. When the melting point is 145° C. or lower, the sealing properties related to the electrolyte tend to be further improved.
[0229] The propylene-ethylene random copolymer may be an acid-modified copolymer, for example, an acid-modified propylene-ethylene random copolymer obtained by grafting maleic anhydride. By using the acid-modified propylene-ethylene random copolymer, the adhesion to the tab lead can be ensured even without the tab sealant.
[0230] The propylene-ethylene random copolymer may be used alone or in combination of two or more.
[0231] In the sealant layer 16, the content of the component (A) can be 50 to 99% by mass, 50 to 95% by mass, or 50 to 85% by mass, based on the total solid content of the sealant layer 16. By making the content of the component (A) 50% by mass or more, the sealing properties can be improved by utilizing the effect of using the component (A) itself. In addition, by making the content of the component (A) 50% by mass or more, it is easy to form a good sea island structure because the component (B) can be prevented from being present excessively, and the reduction of the heat resistance and cohesion of the sealant layer 16 can be suppressed. On the other hand, by making the content of the component (A) 99% by mass or less, since the component (B) can be made to contain more than 1% by mass, the sealing strength and insulation brought by the component (B) can be improved.
[0232] (Incompatible component (B))
[0233] Examples of the incompatible component (B) include graft copolymers, block copolymers, and random copolymers, etc. At least a part of these copolymers has an incompatible portion with the component (A).
[0234] The incompatible component (B) preferably contains a compound (B1) having a compatible portion with the polypropylene resin (A). In other words, the compound (B) preferably has a compatible portion and an incompatible portion with the polypropylene resin (A). By containing the compound (B1), the incompatible component (B) can improve the shrinkage ratio of the sealant layer 16, improve the adhesion strength of the interface of the sea-island structure, and inhibit the formation of voids accompanying the foaming of the electrolyte, thereby further improving the insulation. In addition, the adhesion strength of the sea-island interface generated by the compound (B1) is improved, and the sealing strength can also be improved. Such a compound (B1) can be obtained, for example, when the incompatible component (B) is a graft copolymer or a block copolymer. Preferred graft copolymers of the compound (B1) include graft copolymers formed by the main chain of a polyolefin and the side chain of polystyrene, graft copolymers formed by the main chain of a polyolefin and the side chain of a styrene-acrylonitrile copolymer, and the like. As the above-mentioned graft copolymer, for example, "Modiper" manufactured by NOF Corporation is suitable.
[0235] As the preferred block copolymer of compound (B1), there can be enumerated a block copolymer having a block consisting of styrene units and a block consisting of ethylene-butylene units, a block copolymer having a block consisting of styrene units, a block copolymer having a block consisting of ethylene-butylene units and a block copolymer consisting of crystalline olefin units, a block copolymer having a block consisting of crystalline ethylene units and a block copolymer consisting of ethylene-butylene units, a block copolymer having a block consisting of ethylene and a block consisting of ethylene-octene 1, and a block copolymer having a block consisting of propylene units and a block copolymer consisting of ethylene units. For example, the block consisting of propylene units is a compatible portion with the above-mentioned (A) component, and the block consisting of ethylene units is an incompatible portion with the above-mentioned (A) component. As the above-mentioned block copolymer, for example, "DYNARON" made by JSR Corporation, "INTUNE" and "INFUSE" made by DOW Corporation are suitable.
[0236] The incompatible component (B) may also contain an incompatible elastomer. As an incompatible elastomer, a polyolefin elastomer with alpha olefin as a comonomer may be cited. In particular, by using ethylene-alpha olefin copolymers, there is a tendency to impart functionality to the sealant layer 16 without reducing the electrolyte lamination strength or various sealing strengths related to the electrolyte. As ethylene-alpha olefin copolymers, a compound obtained by copolymerizing at least one alpha olefin selected from 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene with ethylene may be used, and an ethylene-butene-1 random copolymer obtained by copolymerizing 1-butene with ethylene may be preferably used. As ethylene-alpha olefin copolymers, "TAFMER" manufactured by Mitsui Chemicals, "EXCELLEN" manufactured by Sumitomo Chemical, etc. are suitable.
[0237] The sealant layer 16 can contain the polypropylene resin (A) and the incompatible component (B) by preparing a dispersion in which an incompatible component (B) is dispersed in a polypropylene resin (A), and by using the dispersion. As such a dispersion, a dispersion in which an elastomer is finely dispersed in a polypropylene resin can be cited. The sealant layer 16 contains the incompatible component (B) by using a dispersion in which the incompatible component (B) is pre-dispersed in a polypropylene resin (A), which has a tendency to further improve the insulation and sealing strength. The incompatible component (B) in the above-mentioned dispersion preferably contains a graft copolymer or a block copolymer. The incompatible component (B) in the dispersion has a tendency to further improve the adhesion of the sea-island interface by containing a graft copolymer or a block copolymer.
[0238] As the incompatible component (B), olefin-based and styrene-based materials have been described above, but from the viewpoint of electrolyte resistance, the incompatible component (B) is preferably an olefin-based material.
[0239] (Compatible elastomer (C))
[0240] As the compatible elastomer (C), for example, propylene-α-olefin copolymers can be cited. By using propylene-α-olefin copolymers, functionality can be imparted to the sealant layer 16 without reducing the electrolyte lamination strength and various sealing strengths related to the electrolyte. As the propylene-α-olefin copolymer, a polymer obtained by copolymerizing propylene with an α-olefin selected from 1-butene, 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene can be used, and a propylene-butene-1 random copolymer obtained by copolymerizing 1-butene can be preferably used.
[0241] The melting point of the polyolefin elastomer is preferably 150°C or less, and is preferably 60 to 120°C, more preferably 65 to 90°C, from the viewpoint of suppressing the excess sealing portion, suppressing molding whitening, and improving the sealing properties related to the electrolyte. When the melting point is 150°C or less, the sealing properties related to the electrolyte, especially the degassing heat seal strength, can be improved. In addition, when the melting point is 60°C or more, it is advantageous from the viewpoint of suppressing the occurrence of the excess sealing portion.
[0242] The polyolefin-based elastomer may be used alone or in combination of two or more.
[0243] In the sealant layer 16, the content of the component (B) is preferably 1 to 40% by mass, and more preferably 5 to 25% by mass, based on the total solid content of the sealant layer 16. By making the content of the component (B) 1% or more by mass, the sealant layer 16 can be given impact resistance, and the sealing strength and insulation can be improved. On the other hand, by making the content of the component (B) 40% or less by mass, it is easy to form a good sea island structure, which can improve the overall cohesion of the sealant layer 16, and improve the sealing strength and insulation. In addition, for convenience, the dispersion formed by the elastomer being finely dispersed in the polypropylene resin is recorded as the incompatible component (B), but in the above-mentioned dispersion, the elastomer part is classified as the (B) component, and the polypropylene resin is classified as the above-mentioned (A) component.
[0244] When the sealant layer 16 contains component (C), the content of component (C) in the sealant layer 16 is preferably 5 to 30% by mass, more preferably 10 to 25% by mass, based on the total solid content of the sealant layer 16. When the content of component (C) is 5% by mass or more, the sealant layer 16 is easily flexible, and functions such as whitening inhibition can be imparted during molding, so that an outer packaging material with further improved functionality can be provided. When the content of component (C) is 30% by mass or less, the cohesive force of the entire sealant layer 16 can be improved, and the sealing strength and insulation can be improved.
[0245] In addition, the content ratio (M) of the compatible elastomer (C) to the incompatible component (B) is C / M B ) is preferably 0.2 to 3.0, more preferably 0.3 to 2.0 in terms of mass ratio. C / M B ) is within the above range, it is easy to improve the sealing strength.
[0246] When the incompatible component (B) contains the compound (B1), the content of the compound (B1) in the sealant layer 16 is preferably 1 to 40% by mass, more preferably 2 to 25% by mass, based on the total amount of the sealant layer. When the content of the compound (B1) is 1% by mass or more, it is easy to increase the adhesion strength of the sea-island interface, and it is easy to obtain the effect of improving the sealing strength and insulation. When the content of the compound (B1) is 40% by mass or less, it is easy to suppress the reduction of the cohesive force of the sealant layer 16 as a whole, as well as the sealing strength and insulation.
[0247] (Added Ingredients)
[0248] The sealant layer 16 may further contain other ingredients in addition to the above-mentioned (A) to (C) components. As other ingredients in addition to the (A) to (C) components, for example, in order to improve the receiving property and processability, other resins such as LDPE (low-density polyethylene) may be added. The content of the other added resin components is preferably 10 parts by mass or less when the total mass of the sealant layer 16 is 100 parts by mass. In addition, as ingredients other than the resin, for example, slip agents, anti-blocking agents, antioxidants, light stabilizers, flame retardants, etc. can be cited. The content of other ingredients other than these resins is preferably 5 parts by mass or less when the total mass of the sealant layer 16 is 100 parts by mass.
[0249] The presence of α-olefin in the sealant layer 16 can be confirmed by attribution using FT-IR (Fourier transform infrared spectrophotometer). In addition, the content of α-olefin can be confirmed by using a sealant layer 16 formulated with a known amount of an elastomer containing a known amount of α-olefin and preparing a standard curve using the transmittance or absorbance of the characteristic absorption bands of components (A) to (C). Furthermore, the α-olefin content of each of the incompatible component (B) and the compatible elastomer (C) can also be confirmed by imaging using the characteristic absorption bands of FT-IR and mapping using the absorption bands caused by butene-1 using microscopic FT-IR (transmission method). In addition, in addition to FT-IR, the presence and content of butene-1 can also be confirmed by measuring the sealant layer 16 using NMR.
[0250] The thickness of the sealant layer 16 is, for example, 5 to 100 μm. In view of the requirement for miniaturization of the power storage device, it can be 10 to 80 μm, 10 to 60 μm, 10 to 45 μm, or less than 30 μm. Even if the outer packaging material for the power storage device of this embodiment is composed of such a film, it can suppress the reduction of insulation after degassing, molding, and degassing heat sealing.
[0251] Preferred embodiments of the packaging material for a power storage device of the present invention have been described in detail above, but the present invention is not limited to the specific embodiments, and various modifications and changes can be made within the scope of the gist of the present invention described in the claims.
[0252] For example, Figure 1 Although the case where the anti-corrosion treatment layer 14 is formed on the surface of the second adhesive layer 17 side of the metal foil layer 13 is shown, the anti-corrosion treatment layer 14 may be formed on the surface of the first adhesive layer 12 side of the metal foil layer 13, or may be formed on both surfaces of the metal foil layer 13. When the anti-corrosion treatment layer 14 is formed on both surfaces of the metal foil layer 13, the structure of the anti-corrosion treatment layer 14 formed on the first adhesive layer 12 side of the metal foil layer 13 and the structure of the anti-corrosion treatment layer 14 formed on the second adhesive layer 17 side of the metal foil layer 13 may be the same as or different from each other.
[0253] Figure 1 FIG. 4 shows a case where the metal foil layer 13 and the sealant layer 16 are laminated using the second adhesive layer 17, but it is also possible to Figure 6 The outer packaging material 20 for the power storage device shown in FIG. Figure 7 As shown in the outer packaging material 30 for a power storage device, the sealant layer 16 is formed directly on the metal foil layer 13 without the second adhesive layer 17. Figure 6 The outer packaging material 20 for the power storage device shown in FIG. Figure 7 The illustrated outer packaging material 30 for a power storage device may further include a second adhesive layer 17 between the metal foil layer 13 and the sealant layer 16 .
[0254] Figure 1 The sealant layer 16 is shown as a single layer, but the sealant layer 16 can also be formed as Figure 6 The outer packaging material 20 for the power storage device shown in FIG. Figure 7 The sealant layer 16 may be formed of multiple layers, such as the outer packaging material 30 for power storage devices shown in FIG. The configurations of the multiple layers forming the sealant layer 16 may be the same or different. In addition, when the sealant layer 16 is multiple layers, at least one of the layers is preferably a low shrinkage sealant layer.
[0255] Figure 6 In the outer packaging material 20 for a power storage device shown in the figure, the sealant layer 16 is composed of a first sealant layer 16a and a second sealant layer 16b. Here, the first sealant layer 16a is the outermost layer of the sealant layer, and the second sealant layer 16b is the innermost layer of the sealant layer. At least one layer selected from the first sealant layer 16a and the second sealant layer 16b is preferably a low-shrinkage sealant layer.
[0256] The second sealant layer 16b (innermost layer) can be formed of the same constituent components as the sealant layer 16 of the outer packaging material 10. When the second sealant layer 16b is a low-shrinkage sealant layer, it is easy to suppress the decrease in insulation when the electrolyte is present.
[0257] The thickness of the second sealant layer 16 b may be, for example, 5 to 100 μm, and from the viewpoint of thinning, may be 10 to 60 μm, 10 to 40 μm, 10 to 30 μm, or 20 μm or less.
[0258] The first sealant layer 16a (outermost layer, layer on one side of the metal foil) can be formed, for example, using the same constituents as the second sealant layer 16b, but in the first sealant layer 16a, it is preferred to replace the same constituents as the second sealant layer 16b with an adhesive constituent containing an additive component as required in consideration of aluminum treatment and adhesion. As the first sealant layer 16a, by using the above-mentioned adhesive constituent, a sealant layer can be formed on the metal foil layer without an adhesive layer. When the first sealant layer 16a contains components equivalent to the above-mentioned (A) component and (B) component in the same manner as the second sealant layer 16b, the first sealant layer 16a forms an island structure, and the first sealant layer 16a is a low-shrinkage sealant layer, the adhesion of the island interface can be improved, and it is easy to maintain the adhesion between the sealant layer and the metal foil layer, prevent the occurrence of voids associated with the foaming of the electrolyte, and have a tendency to further suppress the reduction of insulation after degassing heat sealing.
[0259] The adhesive constituents in the first sealant layer 16a are not particularly limited, and preferably contain a modified polypropylene resin (i) component as component (A) and a macroscopic phase separation thermoplastic elastomer (ii) component as component (B). In addition, the additive component preferably contains atactic polypropylene or atactic propylene-α-olefin copolymer (iii). Each component is described below.
[0260] (Modified polypropylene resin (i))
[0261] The modified polypropylene-based resin (i) is preferably a resin obtained by graft-modifying a polyolefin resin with an unsaturated carboxylic acid derivative component derived from any of an unsaturated carboxylic acid, an anhydride of an unsaturated carboxylic acid, and an ester of an unsaturated carboxylic acid.
[0262] Examples of the polypropylene-based resin include homopolypropylene and random polypropylene.
[0263] Examples of the compound used when graft-modifying these polyolefin resins include unsaturated carboxylic acid derivative components derived from any of unsaturated carboxylic acids, anhydrides of unsaturated carboxylic acids, and esters of unsaturated carboxylic acids.
[0264] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid.
[0265] Examples of the anhydride of unsaturated carboxylic acid include anhydrides of unsaturated carboxylic acids such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride.
[0266] Examples of the ester of unsaturated carboxylic acid include esters of unsaturated carboxylic acids such as methyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, dimethyl maleate, monomethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconic acid, dimethyl tetrahydrophthalic anhydride, and dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate.
[0267] The modified polypropylene resin (i) can be manufactured by graft polymerization (graft modification) of 0.2 to 100 parts by mass of the unsaturated carboxylic acid derivative component in the presence of a free radical initiator relative to 100 parts by mass of the polypropylene resin serving as the matrix. The reaction temperature of the graft modification is preferably 50 to 250° C., more preferably 60 to 200° C. In addition, the reaction time is appropriately set according to the manufacturing method. For example, when melt graft polymerization is performed using a twin-screw extruder, the residence time of the extruder is specifically preferably 2 to 30 minutes, more preferably 5 to 10 minutes. In addition, the graft modification can be implemented under any condition of normal pressure or pressurization.
[0268] Examples of the radical initiator used for graft modification include organic peroxides such as alkyl peroxides, aryl peroxides, acyl peroxides, ketone peroxides, peroxyketals, peroxycarbonates, peroxyesters, and hydrogen peroxide.
[0269] These organic peroxides can be appropriately selected and used according to the conditions of the above-mentioned reaction temperature or reaction time. For example, in the case of melt graft polymerization using a twin-screw extruder, alkyl peroxides, peroxyketals, and peroxyesters are preferred, and specifically, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di-tert-butyl peroxy-hexyne-3, diisopropylphenyl peroxide, etc. are preferred.
[0270] As the modified polypropylene resin (i), it is preferred that it is modified with maleic anhydride, such as "ADMER" manufactured by Mitsui Chemicals, "Modic" manufactured by Mitsubishi Chemical Corporation. Since such modified polypropylene resin (i) has excellent reactivity with various metals or polymers having various functional groups, the reactivity can be utilized to impart adhesion to the first sealant layer 16a, thereby improving electrolyte resistance.
[0271] (Macroscopic phase separation thermoplastic elastomer (ii))
[0272] The macro-phase-separated thermoplastic elastomer (ii) forms a macro-phase-separated structure with respect to the modified polypropylene-based resin (i) in which the dispersed phase size is in the range of more than 200 nm and 50 μm or less.
[0273] The first sealant layer 16a can release the residual stress generated when laminating the modified polypropylene resin (i) and the like which can be the main component of the first sealant layer 16a by containing the macro phase separation thermoplastic elastomer (ii), and can impart viscoelastic adhesion to the first sealant layer 16a. Therefore, the adhesion of the first sealant layer 16a is further improved, and an outer packaging material 20 with better electrolyte resistance can be obtained. By containing the macro phase separation thermoplastic elastomer (ii) in the first sealant layer 16a, the sealant layer 16 can be imparted with impact resistance, and the sealing strength and insulation can be improved.
[0274] The macroscopic phase separation thermoplastic elastomer (ii) exists in the modified polypropylene resin (i) in the form of an island, but when the dispersed phase size is below 200nm, it is difficult to impart viscoelastic adhesion. On the other hand, when the dispersed phase size exceeds 50μm, since the modified polypropylene resin (i) and the macroscopic phase separation thermoplastic elastomer (ii) are essentially incompatible, the physical strength of the first sealant layer 16a is easily reduced while the lamination suitability (processability) is significantly reduced. Therefore, the dispersed phase size is preferably 500nm to 10μm.
[0275] Examples of such macro-phase-separated thermoplastic elastomers (ii) include polyethylene-based thermoplastic elastomers obtained by copolymerizing ethylene with an α-olefin selected from 1-butene, 1-pentene, 1-hexene, 1-octene and 4-methyl-1-pentene.
[0276] As the macro-phase separation thermoplastic elastomer (ii), commercially available products can be used, and suitable examples include "TAFMER" manufactured by Mitsui Chemicals, Inc., "Zelas" manufactured by Mitsubishi Chemical Corporation, and "Catalloy" manufactured by Montell Corporation.
[0277] In the first sealant layer 16a, the content of the macro-phase separation thermoplastic elastomer (ii) relative to the modified polypropylene resin (i) is preferably 1 to 40 parts by mass, more preferably 5 to 30 parts by mass relative to 100 parts by mass of the modified polypropylene resin (i). Here, when the content of the macro-phase separation thermoplastic elastomer (ii) is less than 1 part by mass, it is impossible to expect an improvement in the adhesion of the first sealant layer. When the content of the macro-phase separation thermoplastic elastomer (ii) exceeds 40 parts by mass, since the compatibility of the modified polypropylene resin (i) and the macro-phase separation thermoplastic elastomer (ii) is low, the processability is easily reduced. In addition, since the macro-phase separation thermoplastic elastomer (ii) is not a resin showing adhesion, the adhesion of the first sealant layer 16a to other layers such as the second sealant layer 16b or the anti-corrosion treatment layer 14 becomes easy to reduce.
[0278] (Atactic polypropylene or atactic propylene-α-olefin copolymer (iii))
[0279] The first sealant layer 16a preferably contains atactic polypropylene or atactic propylene-α-olefin copolymer (hereinafter referred to as "(iii) component") as an additive component. Here, the (iii) component is a completely amorphous resin component. By containing the (iii) component in the first sealant layer 16a, the sealant layer 16 can be given flexibility. By making the sealant layer 16 flexible, the outer packaging material 10 can be given functions such as molding whitening inhibition, and an outer packaging material with further improved functionality can be provided.
[0280] Furthermore, the first sealant layer 16a may further contain, as an additive component, a propylene-α-olefin copolymer having an isotactic structure corresponding to the component (C) in addition to the component (iii) in order to impart flexibility.
[0281] In the first sealant layer 16a, the total mass of the components (i) and (ii) may be, for example, 60% to 95% by mass, or 70% to 90% by mass, based on the total mass of the first sealant layer 16a.
[0282] In the first sealant layer 16a, the mass of the component (iii) is preferably 5% by mass or more and 40% by mass or less based on the total mass of the components (i), (ii) and (iii). When the mass of the component (iii) is 5% by mass or more based on the total mass of the components (i), (ii) and (iii), there is a tendency to easily obtain the effect brought about by adding the above-mentioned additive. On the other hand, when the mass of the component (iii) is 40% by mass or less based on the total mass of the components (i), (ii) and (iii), there is a tendency that the adhesion of the first sealant layer 16a to other layers such as the second sealant layer 16b or the anti-corrosion treatment layer 14 is easily reduced. From these viewpoints, in the first sealant layer 16a, the total mass of the components (i) and (ii) is preferably 60 to 95% by mass based on the total mass of the components (i), (ii) and (iii).
[0283] In addition, as a method for analyzing the component (iii) as an additive component in the first sealant layer 16a, for example, it is possible to quantify the amount by evaluating stereoregularity using nuclear magnetic resonance spectroscopy (NMR).
[0284] In addition to the adhesive constituent components (i.e., modified polypropylene resin (i) and macro-phase separated thermoplastic elastomer (ii)) and additive components (i.e., component (iii)), the first sealant layer 16a may also contain various additives as needed, such as flame retardants, slip agents, anti-blocking agents, antioxidants, light stabilizers, adhesion-imparting agents, etc.
[0285] The thickness of the first sealant layer 16 a is not particularly limited, but is preferably the same as or less than the thickness of the second sealant layer 16 b from the viewpoint of stress relaxation and water / electrolyte permeation.
[0286] In addition, in the outer packaging material 20 for storage device, from the viewpoint of thin film, the thickness of the sealant layer 16 (the total thickness of the first sealant layer 16a and the second sealant layer 16b) can be 10 to 80 μm, 10 to 60 μm, 10 to 45 μm, or less than 30 μm. Even if the outer packaging material for storage device of the present embodiment is such a thin film, the decrease in insulation after heat sealing, molding and degassing heat sealing can be suppressed.
[0287] Figure 6 The sealant layer 16 is shown as being formed of two layers, but the sealant layer 16 may also be formed of two layers. Figure 7 The outer packaging material 30 for a power storage device shown in the figure is formed of three layers. Figure 7In the outer packaging material 30 for a power storage device shown, the sealant layer 16 is composed of a first sealant layer 16a, a second sealant layer 16b and a third sealant layer 16c. Here, the first sealant layer 16a is the outermost layer of the sealant layer (the layer on the metal foil side), the third sealant layer 16c is the middle layer of the sealant layer, and the second sealant layer 16b is the innermost layer of the sealant layer. At least one layer selected from these three layers is preferably a low-shrinkage sealant layer.
[0288] Examples and preferred aspects of the material constituting the first sealant layer 16 a of the power storage device packaging material 30 are the same as those of the first sealant layer 16 a of the power storage device packaging material 20 .
[0289] Examples and preferred aspects of the materials constituting the second sealant layer 16 b and the third sealant layer 16 c of the power storage device packaging material 30 are the same as those of the second sealant layer 16 b of the power storage device packaging material 20 .
[0290] In the outer packaging material 30 for the storage device, the thickness of the first sealant layer 16a can be, for example, 2 to 30 μm, 5 to 20 μm, or 8 to 10 μm, the thickness of the second sealant layer 16b can be, for example, 5 to 80 μm, 13 to 40 μm, or 15 to 20 μm, and the thickness of the third sealant layer 16c can be, for example, 2 to 30 μm, 5 to 20 μm, or 8 to 10 μm.
[0291] In the outer packaging material 30 for storage device, from the viewpoint of thin film, the thickness of the sealant layer 16 (the total thickness of the first sealant layer 16a, the second sealant layer 16b and the third sealant layer 16c) can be 30 μm or less. Even if the outer packaging material for storage device of this embodiment is such a thin film, it is possible to suppress the reduction of insulation after heat sealing, molding and degassing heat sealing.
[0292] When the sealant layer is composed of multiple layers, such as the outer packaging materials 20 and 30 for power storage devices, it is preferred that the first sealant layer 16a closest to the metal foil layer 13 is a low-shrinkage sealant layer. By making the first sealant layer 16a a low-shrinkage sealant layer, the sealing strength of the sea-island interface can be improved, and the formation of voids accompanying the foaming of the electrolyte can be suppressed, so there is a tendency to further improve the insulation after degassing heat sealing. The foaming of the electrolyte during degassing heat sealing mostly occurs in the portion of the sealant layer 16 close to the metal foil layer 13. By making the layer closest to the metal foil layer 13 a low-shrinkage sealant layer, there is a tendency to more effectively suppress the reduction of insulation.
[0293] In addition, the second sealant layer 16b or the third sealant layer 16c may also be a low-shrinkage sealant layer. By using the second sealant layer 16b or the third sealant layer 16c as a low-shrinkage sealant layer, the adhesion strength of the sea-island interface formed by the (A) and (B) components can be increased, and the formation of voids accompanying the foaming of the electrolyte can be suppressed, thereby further improving the insulation.
[0294] [Manufacturing method of outer packaging material]
[0295] Next, Figure 1 An example of a method for producing the outer packaging material 10 shown in FIG.
[0296] The manufacturing method of the outer packaging material 10 of the present embodiment is roughly composed of the following steps: a step of laminating an anti-corrosion treatment layer 14 on a metal foil layer 13; a step of bonding a base material layer 11 to the metal foil layer 13; a step of further laminating a sealant layer 16 via a second adhesive layer 17 to produce a laminate; and a step of performing an aging treatment on the obtained laminate as needed.
[0297] (Step of Laminating the Anticorrosion Treatment Layer 14 on the Metal Foil Layer 13)
[0298] This step is a step of forming the anticorrosion treatment layer 14 on the metal foil layer 13. As described above, the method includes degreasing, hot water deterioration, anodizing, chemical conversion, or coating the metal foil layer 13 with a coating agent having anticorrosion properties.
[0299] In addition, when the anti-corrosion treatment layer 14 is multi-layered, for example, the coating liquid (coating agent) constituting the anti-corrosion treatment layer on the lower side (the side of the metal foil layer 13) is applied on the metal foil layer 13 and sintered to form a first layer, and then the coating liquid (coating agent) constituting the anti-corrosion treatment layer on the upper side is applied on the first layer and sintered to form a second layer.
[0300] For degreasing treatment, spraying or dipping can be used; for hot water deterioration treatment or anodizing treatment, dipping can be used; for chemical conversion treatment, dipping, spraying, coating, etc. can be appropriately selected according to the type of chemical conversion treatment.
[0301] As a coating method of the coating agent having anticorrosion performance, various methods such as gravure coating, reverse coating, roll coating, and bar coating can be used.
[0302] As described above, the various treatments may be applied to both sides or one side of the metal foil. When the treatment is applied to one side, the treatment side is preferably applied to the side where the second adhesive layer 17 is laminated. If necessary, the surface of the base layer 11 may also be subjected to the above treatments.
[0303] In addition, the coating amount of the coating agent for forming the first layer and the second layer is preferably 0.005 to 0.200 g / m 2 , more preferably 0.010 to 0.100 g / m 2 .
[0304] When drying and curing is required, the drying can be carried out at a masterbatch temperature in the range of 60 to 300° C., depending on the drying conditions of the anticorrosion treatment layer 14 used.
[0305] (Step of Laminating the Base Material Layer 11 and the Metal Foil Layer 13)
[0306] This step is a step of laminating the metal foil layer 13 provided with the anticorrosion treatment layer 14 to the base material layer 11 via the first adhesive layer 12. As a laminating method, dry lamination, non-solvent lamination, wet lamination or the like is used to laminate the two using the material constituting the first adhesive layer 12. The first adhesive layer 12 is applied in a dry coating amount of 1 to 10 g / m 2 The range is preferably 3 to 7 g / m 2 range to set.
[0307] (Step of Laminating the Second Adhesive Layer 17 and the Sealant Layer 16)
[0308] This step is a step of laminating the sealant layer 16 to the anticorrosion treated layer 14 side of the metal foil layer 13 via the second adhesive layer 17. Examples of the laminating method include a wet process and dry lamination.
[0309] In the wet process, a solution or dispersion of the adhesive constituting the second adhesive layer 17 is applied to the anticorrosion treatment layer 14, and the solvent is dispersed at a predetermined temperature (a temperature above the melting point of the acid-modified polyolefin resin when the adhesive contains the acid-modified polyolefin resin), and a drying film is formed, or a sintering treatment is performed as needed after the drying film is formed. Then, the sealant layer 16 is laminated to manufacture the outer packaging material 10. As the coating method, various coating methods exemplified above can be cited.
[0310] The sealant layer 16 can be manufactured, for example, using a melt extrusion molding machine. In particular, for the melt extrusion molding machine used to manufacture the outer packaging material 10 of the second aspect of the present embodiment, the processing speed can be set to 80 m / min or more from the perspective of productivity. The sealant layer 16 obtained under such conditions tends to have a structure in which the B component is stretched in the MD direction.
[0311] (Aging treatment process)
[0312] This step is a step of aging (aging) the laminate. By aging the laminate, the adhesion between the metal foil layer 13 / the anti-corrosion treatment layer 14 / the second adhesive layer 17 / the sealant layer 16 can be promoted. The aging treatment can be performed in the range of room temperature to 100°C. The aging time is, for example, 1 to 10 days. Figure 5 The outer packaging material 10 (sealant layer 16) heated at 190°C for 30 seconds as described above may be one that has undergone the above-mentioned aging treatment.
[0313] In this way, it is possible to produce Figure 1 The outer packaging material 10 of this embodiment is shown.
[0314] Next, Figure 6 An example of a method for producing the outer packaging material 20 shown in FIG.
[0315] The manufacturing method of the outer packaging material 20 of the present embodiment generally comprises the following steps: a step of laminating the anti-corrosion treatment layer 14 on the metal foil layer 13; a step of laminating the base material layer 11 and the metal foil layer 13; a step of further laminating the first sealant layer 16a and the second sealant layer 16b to produce a laminate; and a step of heat-treating the obtained laminate as required. In addition, the steps up to the step of laminating the base material layer 11 and the metal foil layer 13 can be performed in the same manner as the manufacturing method of the outer packaging material 10 described above.
[0316] (Step of Laminating the First Sealant Layer 16a and the Second Sealant Layer 16b)
[0317] This process is a process for forming the first sealant layer 16a and the second sealant layer 16b on the anticorrosion treatment layer 14 formed by the previous process. As a method thereof, a method of sandwich laminating the first sealant layer 16a and the second sealant layer 16b using an extrusion laminator can be cited. Furthermore, lamination can also be performed by utilizing a tandem lamination method or a coextrusion method in which the first sealant layer 16a and the second sealant layer 16b are extruded. In the formation of the first sealant layer 16a and the second sealant layer 16b, for example, each component is matched in a manner that satisfies the composition of the first sealant layer 16a and the second sealant layer 16b.
[0318] Through this process, we obtain Figure 6 The laminate shown is a laminate in which the layers are laminated in the order of base material layer 11 / first adhesive layer 12 / metal foil layer 13 / anticorrosion treated layer 14 / first sealant layer 16a / second sealant layer 16b.
[0319] In addition, the first sealant layer 16a can be laminated directly using an extrusion laminator by dry-mixing the materials in a manner to form the above-mentioned material combination composition, or the first sealant layer 16a that has been granulated and melt-mixed in advance using a melt-mixing device such as a single-screw extruder, a twin-screw extruder, or a Brabender mixer can be laminated using an extrusion laminator.
[0320] The second sealant layer 16b can be laminated directly by using an extrusion laminator according to the composition used as the sealant layer formation to form the above-mentioned material combination composition, or the granulated material after melt mixing can be laminated by using an extrusion laminator to extrude the first sealant layer 16a and the second sealant layer 16b in series lamination and coextrusion method. In addition, the composition used for the sealant layer formation can also be used to make a sealant monofilm as a cast film in advance, and the film can be laminated together with an adhesive resin by a sandwich lamination method, or an adhesive can be laminated by using a dry lamination method. In particular, the formation speed (processing speed) of the sealant layers 16a and 16b when manufacturing the outer packaging material 20 of the second aspect of the present embodiment can be, for example, more than 80m / minute from the viewpoint of productivity. The sealant layers 16a and 16b obtained under such conditions are easy to have a structure in which the (B) component is stretched in the MD direction.
[0321] (Heat treatment process)
[0322] This process is a process of heat treating the laminate. By heat treating the laminate, the adhesion between the metal foil layer 13 / corrosion protection layer 14 / first sealant layer 16a / second sealant layer 16b can be improved, and better electrolyte resistance or hydrofluoric acid resistance can be imparted. As a method of heat treatment, it is preferred to treat at a temperature at least above the melting point of the first sealant layer 16a. As heat treatment, oven heating, clamping with heating rollers (thermal lamination), and winding on heating rollers can be cited, but are not limited to these. The heat treatment time can be appropriately adjusted from the perspectives of performance (adhesion strength (lamination strength) between the metal foil layer 13 / corrosion protection layer 14 / first sealant layer 16a / second sealant layer 16b) and productivity according to the heat treatment method, temperature conditions, etc. For example, when heat treatment is performed by clamping with heating rollers or winding on heating rollers, the heat treatment time can be more than 0.5 seconds from the perspective of the above-mentioned performance, and can be less than 1.0 seconds from the perspective of productivity. In addition, Figure 5 The outer packaging material 20 (sealant layer 16) shown and described as being heated at 190°C for 30 seconds may be one that has undergone the above-mentioned aging treatment or heat treatment.
[0323] In this way, it is possible to produce Figure 6 The outer packaging material 20 of this embodiment is shown.
[0324] Next, Figure 7 An example of a method for producing the outer packaging material 30 shown in FIG.
[0325] The manufacturing method of the outer packaging material 30 of the present embodiment is roughly composed of the following steps: a step of stacking the anti-corrosion treatment layer 14 on the metal foil layer 13; a step of bonding the base material layer 11 and the metal foil layer 13; a step of further stacking the first sealant layer 16a, the third sealant layer 16c and the second sealant layer 16b to produce a laminate; and a step of heat treating the obtained laminate as needed.
[0326] (Step of Laminating the First Sealant Layer 16a, the Third Sealant Layer 16c, and the Second Sealant Layer 16b)
[0327] This operation is a process for forming the first sealant layer 16a, the third sealant layer 16c and the second sealant layer 16b on the anticorrosion treatment layer 14. As its method, a tandem lamination method and a coextrusion method in which the first sealant layer 16a, the third sealant layer 16c and the second sealant layer 16b are extruded using an extrusion laminating machine can be cited. At this time, the material mixed by dry mixing can be directly stacked using an extrusion laminating machine according to the mode in which the constituent components used for forming the sealant layer become the above-mentioned material matching composition, or the granulated material after melt mixing implemented in advance by a single screw extruder, a twin screw extruder, a Brabender mixer, etc. can be stacked using an extrusion laminating machine to extrude the first sealant layer 16a, the third sealant layer 16c and the second sealant layer 16b in a tandem lamination method and a coextrusion method.
[0328] The third sealant layer 16c and the second sealant layer 16b can also be made into films by coextrusion, and these films are laminated together with the constituent components used to form the first sealant layer 16a by sandwich lamination. In particular, the formation speed (processing speed) of the sealant layers 16a, 16b, and 16c when manufacturing the outer packaging material 30 of the second aspect of the present embodiment can be, for example, 80m / minute or more from the perspective of productivity. The sealant layers 16a, 16b, and 16c obtained under such conditions are prone to have a structure in which the (B) component is stretched in the MD direction. The manufacturing method of the outer packaging material 30 of the present embodiment can also be equipped with the above-mentioned heat treatment step in the manufacturing method of the outer packaging material 20. The technique and conditions of the heat treatment can be the same as the above-mentioned technique and conditions in the manufacturing method of the outer packaging material 20.
[0329] In this way, it is possible to produce Figure 7 The outer packaging material 30 of this embodiment is shown.
[0330] The preferred embodiment of the outer packaging material for a storage device of the present invention is described in detail above, but the present invention is not limited to this specific embodiment, and various deformations and changes can be made within the scope of the gist of the present invention described in the claims. For example, when manufacturing an outer packaging material for a storage device without a first adhesive layer 12, as described above, the base material layer 11 can be formed by coating or applying a resin material that can form the base material layer 11 on the metal foil layer 13. In addition, the second aspect of the above-mentioned embodiment describes that for the low-shrinkage sealant layer, the region where the (B) component exists shrinks slightly due to heating, but it is also possible that the low-shrinkage sealant layer does not shrink due to heating.
[0331] The outer packaging material for a power storage device of the present invention can be preferably used as an outer packaging material for power storage devices such as secondary batteries such as lithium ion batteries, nickel-metal hydride batteries, and lead storage batteries, and electrochemical capacitors such as electric double layer capacitors. In particular, the outer packaging material for a power storage device of the present invention is preferably used as an outer packaging material for lithium ion batteries.
[0332] Example
[0333] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to the following Examples.
[0334] (1) Examples and Comparative Examples of the First Aspect
[0335] [Materials used]
[0336] Materials used in Examples 1-1 to 1-32 and Comparative Examples 1-1 and 1-2 are shown below.
[0337] <Base layer (thickness: 15 μm)>
[0338] A nylon (Ny) membrane (manufactured by Toyobo Co., Ltd.) was used.
[0339] <First adhesive layer (thickness: 4 μm)>
[0340] A polyurethane adhesive (manufactured by Toyo Ink Co., Ltd.) was used in which a polyester polyol-based main agent and a toluene diisocyanate adduct-based curing agent were blended.
[0341] <First anti-corrosion treatment layer (substrate layer side) and second anti-corrosion treatment layer (sealant layer side)>
[0342] (CL-1): "Sodium polyphosphate stabilized cerium oxide sol" adjusted to a solid content concentration of 10% by mass using distilled water as a solvent was used. The sodium polyphosphate stabilized cerium oxide sol was obtained by mixing 10 parts by mass of a sodium salt of phosphoric acid with 100 parts by mass of cerium oxide.
[0343] (CL-2): A composition composed of 90% by mass of "polyallylamine (manufactured by Nittobo Co., Ltd.)" adjusted to a solid content concentration of 5% by mass using distilled water as a solvent and 10% by mass of "polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Co., Ltd.)" was used.
[0344] (CL-3): A water-soluble phenolic resin (manufactured by Sumitomo Bakelite Co., Ltd.) was used as a solvent and adjusted to a solid content concentration of 1% by mass using a 1% by mass phosphoric acid aqueous solution. Chromium fluoride (CrF3) was added so that the amount of Cr present in the final dried film would be 10 mg / m 2 A chemical conversion treatment agent obtained by adjusting the concentration in a certain manner.
[0345] <Metal foil layer (thickness: 35 μm)>
[0346] A soft aluminum foil ("8079 material", manufactured by Toyo Aluminum Co., Ltd.) subjected to annealing and degreasing treatment was used.
[0347] <Second adhesive layer (thickness: 3 μm)>
[0348] As the adhesive for forming the second adhesive layer, the following adhesives a and b were prepared.
[0349] Adhesive a: An adhesive obtained by blending 10 parts by mass (solid content ratio) of a polyisocyanate compound having an isocyanurate structure with respect to 100 parts by mass of an acid-modified polyolefin resin dissolved in toluene.
[0350] Adhesive b: A polyurethane adhesive prepared by mixing polyester polyol composed of hydrogenated dimer fatty acid and diol and polyisocyanate so that the molar ratio (NCO / OH) becomes 2.
[0351] <Sealing layer>
[0352] [Matrix resin composition]
[0353] As the matrix resin composition for forming a sealant layer, RC1 to RC9 were prepared at the mass ratios described in Tables 1 and 2. In addition, the details of the terms used in Tables 1 and 2 are as follows.
[0354] ((A) ingredient)
[0355] Acid-modified PP: Acid-modified polypropylene.
[0356] Random PP: propylene-ethylene random copolymer.
[0357] ((B) ingredient)
[0358] Ethylene-α-olefin copolymer: an ethylene-propylene copolymer elastomer that is incompatible with the acid-modified PP (component (A)).
[0359] Ethylene-butene-1 random copolymer: an ethylene-butene-1 random copolymer elastomer that is incompatible with the random PP (component (A)).
[0360] Reactor-type TPO: A dispersion in which ethylene rubber is finely dispersed in polypropylene.
[0361] Dynamically cross-linked PP elastomer (TPV) (using peroxide): a dispersion in which a cross-linked elastomer is finely dispersed in polypropylene, wherein the cross-linked elastomer is grafted and the grafted portion constitutes an interface with the polypropylene.
[0362] Block copolymer 1: A block copolymer composed of crystalline ethylene units and ethylene-butylene units and having no compatibility with random PP (component (A)).
[0363] Block copolymer 2: A block copolymer composed of propylene units and ethylene units and having no compatibility with random PP (component (A)).
[0364] Graft copolymer: A graft copolymer composed of a polyolefin main chain and a polystyrene side chain, which is incompatible with random PP (component (A)).
[0365] ((C) ingredient)
[0366] Atactic copolymer: an atactic propylene-α-olefin copolymer compatible with the acid-modified PP (component (A)).
[0367] Propylene-butene-1 random copolymer: a propylene-butene-1 random copolymer elastomer having compatibility with random PP (component (A)).
[0368] In addition, reactor-type TPO and dynamically cross-linked PP-based elastomers are materials in which component (B) is dispersed in component (A). In Table 1, for convenience, for example, reactor-type TPO is classified as component (B) and recorded, but the mass ratio (10.0) of reactor-type TPO shown in Table 1 represents the amount of the component equivalent to component (B) in reactor-type TPO. The amount of the component equivalent to component (A) in reactor-type TPO is included in the mass ratio (70.0) of random PP. Similarly, the mass ratio (10.0) of the dynamically cross-linked PP-based elastomer shown in Table 1 also represents the amount of the component equivalent to component (B) in the dynamically cross-linked PP-based elastomer, and the amount of the component equivalent to component (A) in the dynamically cross-linked PP-based elastomer is included in the mass ratio (70.0) of random PP.
[0369] Table 1
[0370]
[0371] Table 2
[0372]
[0373] [Example 1-1]
[0374] First, the first and second anti-corrosion treatment layers were provided on the metal foil layer in the following steps. That is, (CL-1) was applied on both sides of the metal foil layer by micro-gravure coating so that the dry coating amount reached 70 mg / m 2 In the drying unit, a sintering treatment was performed at 200° C. Then, (CL-2) was coated on the obtained layer by micro-gravure coating so that the dry coating amount reached 20 mg / m 2 , thereby forming a composite layer composed of (CL-1) and (CL-2) as the first and second anti-corrosion treatment layers. The composite layer exhibits anti-corrosion performance by combining (CL-1) and (CL-2).
[0375] Next, a dry lamination technique is used to adhere the first anti-corrosion treatment layer side of the metal foil layer provided with the first and second anti-corrosion treatment layers to the substrate layer using a polyurethane adhesive (first adhesive layer). It is installed in the unwinding section of the extrusion laminator, and the material of the sealant layer is co-extruded onto the second anti-corrosion treatment layer under the processing conditions of 270°C and 100m / min, so that the layer on one side of the metal foil (hereinafter also referred to as the "AL side layer") (thickness of 8.3μm) and the innermost layer (thickness of 16.7μm) are stacked in sequence as the sealant layer. In addition, the AL side layer and the innermost layer are mixtures of various materials prepared in advance using a twin-screw extruder and subjected to water cooling and granulation processes for the above-mentioned extrusion lamination. Resin RC1 is used in the formation of the AL side layer. Resin RC3 is used in the formation of the innermost layer (equivalent to the sealant layer 16b).
[0376] The thus obtained stack is heat treated in such a manner that the maximum reaching temperature of the stack reaches 190°C, thereby manufacturing the outer packaging material of Example 1-1 (a stack of substrate layer / first adhesive layer / first anti-corrosion treatment layer / metal foil layer / second anti-corrosion treatment layer / AL side layer (sealant layer 16a) / innermost layer (sealant layer 16b)).
[0377] [Example 1-2]
[0378] The outer packaging material of Example 1-2 was produced in the same manner as in Example 1-1 except that the material used in forming the innermost layer (sealant layer 16 b ) was changed to resin RC4.
[0379] [Examples 1-3]
[0380] The outer packaging material of Example 1-3 was produced in the same manner as in Example 1-1 except that the material used in forming the innermost layer (sealant layer 16 b ) was changed to resin RC5.
[0381] [Examples 1-4]
[0382] The outer packaging material of Example 1-4 was produced in the same manner as in Example 1-2 except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC8.
[0383] [Examples 1-5]
[0384] The outer packaging material of Example 1-5 was produced in the same manner as in Example 1-2 except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC6.
[0385] [Examples 1-6]
[0386] The outer packaging material of Example 1-6 was produced in the same manner as in Example 1-3 except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC8.
[0387] [Examples 1-7]
[0388] The outer packaging material of Example 1-7 is manufactured in the same manner as Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) is changed to resin RC6, and the material used in forming the innermost layer (sealant layer 16b) is changed to resin RC9.
[0389] [Examples 1-8]
[0390] The outer packaging material of Example 1-8 is manufactured in the same manner as Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) is changed to resin RC7, and the material used in forming the innermost layer (sealant layer 16b) is changed to resin RC10.
[0391] [Examples 1-9]
[0392] The outer packaging material of Example 1-9 is manufactured in the same manner as Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) is changed to resin RC8, and the material used in forming the innermost layer (sealant layer 16b) is changed to resin RC11.
[0393] [Examples 1-10]
[0394] The outer packaging material of Example 1-10 was produced in the same manner as in Example 1-1 except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC6.
[0395] [Examples 1-11]
[0396] The outer packaging material of Example 1-11 was produced in the same manner as in Example 1-1 except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC8.
[0397] [Examples 1-12]
[0398] The outer packaging material of Example 1-12 was produced in the same manner as in Example 1-1 except that the material used in forming the innermost layer (sealant layer 16b) was changed to resin RC9.
[0399] [Examples 1-13]
[0400] The outer packaging material of Example 1-13 was produced in the same manner as in Example 1-1 except that the material used in forming the innermost layer (sealant layer 16 b ) was changed to resin RC11.
[0401] [Examples 1-14]
[0402] The outer packaging material of Example 1-14 was produced in the same manner as in Example 1-7 except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC2.
[0403] [Examples 1-15]
[0404] First, the first and second anti-corrosion treatment layers were provided on the metal foil layer in the following steps. That is, (CL-3) was applied on both sides of the metal foil layer by micro-gravure coating so that the dry coating amount reached 30 mg / m 2 In the drying unit, a sintering treatment was performed at 200° C. Then, (CL-2) was coated on the obtained layer by micro-gravure coating so that the dry coating amount reached 20 mg / m 2 , thereby forming a composite layer composed of (CL-3) and (CL-2) as the first and second anti-corrosion treatment layers. The composite layer exhibits anti-corrosion performance by combining (CL-3) and (CL-2). Except for using the metal foil layer provided with the first and second anti-corrosion treatment layers, the outer packaging material of Example 1-15 was manufactured in the same manner as Example 1-7.
[0405] [Examples 1-16]
[0406] The first and second anti-corrosion treatment layers are provided on the metal foil layer in the same manner as in Example 1-1. The first anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers is adhered to the substrate layer using a polyurethane adhesive (first adhesive layer) by dry lamination. Next, the second anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers is adhered to the sealant layer 16 (innermost layer) (thickness 25 μm) by dry lamination using adhesive a (second adhesive layer) to manufacture the outer packaging material of Example 1-16. A mixture with resin RC9 is used in the formation of the innermost layer (sealant layer 16).
[0407] [Example 1-17]
[0408] The first and second anti-corrosion treatment layers are provided on the metal foil layer in the same manner as in Example 1-1. The first anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers is adhered to the substrate layer using a polyurethane adhesive (first adhesive layer) by dry lamination. Next, the second anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers is adhered to the sealant layer 16 (innermost layer) (thickness 25 μm) by dry lamination using adhesive b (second adhesive layer) to manufacture the outer packaging material of Example 1-17. A mixture with resin RC9 is used in the formation of the innermost layer (sealant layer 16).
[0409] [Examples 1-18]
[0410] The outer packaging material of Example 1-18 is manufactured in the same manner as Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) is changed to resin RC6, and the material used in forming the innermost layer (sealant layer 16b) is changed to resin RC12.
[0411] [Example 1-19]
[0412] The outer packaging material of Example 1-19 is manufactured in the same manner as Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) is changed to resin RC8, and the material used in forming the innermost layer (sealant layer 16b) is changed to resin RC13.
[0413] [Examples 1-20]
[0414] The outer packaging material of Example 1-20 is manufactured in the same manner as Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) is changed to resin RC8, and the material used in forming the innermost layer (sealant layer 16b) is changed to resin RC14.
[0415] [Example 1-21]
[0416] The outer packaging material of Example 1-21 was manufactured in the same manner as in Example 1-7 except that the thickness of the AL side layer (sealant layer 16a) was changed to 3.3 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 6.7 μm.
[0417] [Examples 1-22]
[0418] The outer packaging material of Example 1-22 was manufactured in the same manner as in Example 1-9 except that the thickness of the AL side layer (sealant layer 16a) was changed to 3.3 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 6.7 μm.
[0419] [Example 1-23]
[0420] The outer packaging material of Example 1-23 was produced in the same manner as in Example 1-5 except that the thickness of the AL side layer (sealant layer 16a) was changed to 15 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 30 μm.
[0421] [Example 1-24]
[0422] The outer packaging material of Example 1-24 was manufactured in the same manner as in Example 1-6 except that the thickness of the AL side layer (sealant layer 16a) was changed to 15 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 30 μm.
[0423] [Example 1-25]
[0424] The outer packaging material of Example 1-25 was manufactured in the same manner as in Example 1-9 except that the thickness of the AL side layer (sealant layer 16a) was changed to 15 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 30 μm.
[0425] [Example 1-26]
[0426] The outer packaging material of Example 1-26 was produced in the same manner as in Example 1-5 except that the thickness of the AL side layer (sealant layer 16a) was changed to 20 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 40 μm.
[0427] [Example 1-27]
[0428] The outer packaging material of Example 1-27 was produced in the same manner as in Example 1-6 except that the thickness of the AL side layer (sealant layer 16a) was changed to 20 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 40 μm.
[0429] [Example 1-28]
[0430] The outer packaging material of Example 1-28 was manufactured in the same manner as in Example 1-9 except that the thickness of the AL side layer (sealant layer 16a) was changed to 20 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 40 μm.
[0431] [Example 1-29]
[0432] The outer packaging material of Example 1-29 was manufactured in the same manner as in Example 1-5 except that the thickness of the AL side layer (sealant layer 16a) was changed to 26.7 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 53.3 μm.
[0433] [Example 1-30]
[0434] The outer packaging material of Example 1-30 was manufactured in the same manner as in Example 1-6 except that the thickness of the AL side layer (sealant layer 16a) was changed to 26.7 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 53.3 μm.
[0435] [Example 1-31]
[0436] The outer packaging material of Example 1-31 was manufactured in the same manner as in Example 1-9 except that the thickness of the AL side layer (sealant layer 16a) was changed to 26.7 μm and the thickness of the innermost layer (sealant layer 16b) was changed to 53.3 μm.
[0437] [Example 1-32]
[0438] The outer packaging material of Example 1-32 is manufactured in the same manner as Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) is changed to resin RC15, and the material used in forming the innermost layer (sealant layer 16b) is changed to resin RC13.
[0439] [Comparative Example 1-1]
[0440] The outer packaging material of Comparative Example 1-1 was manufactured in the same manner as in Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC16, and the material used in forming the innermost layer (sealant layer 16b) was changed to resin RC18.
[0441] [Comparative Example 1-2]
[0442] The outer packaging material of Comparative Example 1-2 was manufactured in the same manner as in Example 1-1, except that the material used in forming the AL side layer (sealant layer 16a) was changed to resin RC17, and the material used in forming the innermost layer (sealant layer 16b) was changed to resin RC19.
[0443] Tables 3 and 4 show the main conditions of Examples 1-1 to 1-32 and Comparative Examples 1-1 to 1-2.
[0444] Table 3
[0445]
[0446] Table 4
[0447]
[0448] <Evaluation>
[0449] The following evaluation tests were performed on the outer packaging materials obtained in Examples and Comparative Examples.
[0450] (Seal Strength)
[0451] Cut the outer packaging material into 60mm×120mm samples, fold them in half with the sealant layer facing inward, and heat seal one side with a 10mm wide sealing strip at 190℃ and 0.5MPa for 3 seconds to form a bonded part. After storing at room temperature for 24 hours, cut the first heat-sealed side into 15mm wide (refer to Figure 8), the sealing strength (T-peel strength) from one end of the adhesive portion to the other end in the width direction was continuously measured using a testing machine (manufactured by INSTRON). The test was conducted in accordance with JIS K6854 at 23°C, 50% RH atmosphere, and at a peeling speed of 50 mm / min. The relationship between the displacement from one end of the adhesive portion and the sealing strength is shown in the graph (see Figure 3 ), the initial maximum value of the load after the start of peeling is taken as the maximum sealing strength S M (N / 15mm). In addition, in the above curve graph, when there is a stable region of sealing strength relative to displacement (mm) (a region where the unevenness of sealing strength below ±3N / 15mm continues for more than 5mm), the average sealing strength S in the stable region is calculated. S , calculate the average sealing strength S S With maximum sealing strength S M Ratio S S / S M In addition, in the above curve graph, when the above stable region does not exist, the sealing strength per 1 mm between the displacement from the maximum sealing strength to the displacement at the other end of the heat seal portion is measured (refer to Figure 4 ) and calculate the average sealing strength S by averaging them. A . Find the calculated average sealing strength S A With maximum sealing strength S M Ratio S A / S M .
[0452] (Electrolyte Lamination Strength)
[0453] The electrolyte solution to which LiPF6 is added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) in a manner to reach 1M is filled in a Teflon (registered trademark) container, and a sample of the outer packaging material cut into 15mm×100mm is placed therein, and the sample is sealed and stored at 85°C for 24 hours. After co-washing, the lamination strength (T-peel strength) between the metal foil layer / sealant layer is measured using a testing machine (manufactured by INSTRON). The test is carried out according to JIS K6854, at 23°C, 50% RH ambient gas, and a peeling speed of 50mm / min. Based on the results, evaluation is performed according to the following standards.
[0454] A: Lamination strength exceeds 7N / 15mm
[0455] B: Lamination strength is 6N / 15mm or more and 7N / 15mm or less
[0456] C: Lamination strength is 5N / 15mm or more and less than 6N / 15mm
[0457] D: Lamination strength is less than 5N / 15mm
[0458] (Electrolyte heat seal strength)
[0459] The outer packaging material was cut into a sample of 60 mm × 120 mm, and folded in half with the sealant layer facing the inside. One side was heat-sealed for 3 seconds at 190°C and 0.5 MPa with a 10 mm wide sealing strip to form a heat-sealed portion. After that, the remaining two sides were also heat-sealed. 2 ml of an electrolyte solution in which LiPF6 was added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) to reach 1 M was injected into the bag-shaped outer packaging material. After the small bag was stored at 60°C for 24 hours, the first heat-sealed side was cut into 15 mm wide (refer to Fig. 9 ), starting from one end of the heat-sealed portion (the end in contact with the electrolyte), the seal strength (T-peel strength) was continuously measured using a testing machine (manufactured by INSTRON). The test was conducted in accordance with JIS K6854 at 23°C, 50% RH, and a peeling speed of 50 mm / min. Based on the results of the maximum seal strength and ratio obtained in the same manner as the "seal strength" item, evaluation was performed according to the following standards.
[0460] S: Maximum sealing strength is 50N / 15mm or more
[0461] A: Maximum sealing strength is 45N / 15mm or more and less than 50N / 15mm
[0462] B: Maximum sealing strength is 35N / 15mm or more and less than 45N / 15mm
[0463] C: Maximum sealing strength is 25N / 15mm or more and less than 35N / 15mm
[0464] D: Maximum sealing strength is less than 25N / 15mm
[0465] (Degassing heat seal strength (Degassing heat seal strength))
[0466] Cut the outer packaging material into 75mm×150mm samples and fold them in half to 37.5mm×150mm with the sealant layer facing inside (refer to Fig.10(a)), heat seal the 150mm side and one 37.5mm side to make a bag. After that, inject 5ml of electrolyte in which LiPF6 is added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) to reach 1M into the small bag, heat seal the other 37.5mm side, and seal it with the sealing part DS1 to obtain a small bag. Next, after the small bag is stored at 60°C for 24 hours, the central part of the small bag is heat sealed with a 10mm wide sealing strip at 190°C and 0.3MPa for 2 seconds in the state of swallowing the electrolyte (degassing heat sealing part DS2, refer to Fig.10 (b)). In order to stabilize the sealed portion, after being stored at room temperature for 24 hours, the area including the degassing heat seal portion DS2 was cut into a 15 mm width (refer to Fig.10 (c) The seal strength (T-type peel strength) was measured from one end of the degassing heat seal portion (the end in contact with the electrolyte) using a testing machine (manufactured by INSTRON). The test was conducted in accordance with JIS K6854 at 23°C, 50% RH, and a peeling speed of 50 mm / min. Based on the results of the maximum seal strength and ratio obtained in the same manner as in the "Seal Strength" item, the evaluation was performed according to the following criteria.
[0467] S: Maximum sealing strength is 45N / 15mm or more
[0468] A: Maximum sealing strength is 40N / 15mm or more and less than 45N / 15mm
[0469] B: Maximum sealing strength is 30N / 15mm or more and less than 40N / 15mm
[0470] C: Maximum sealing strength is 20N / 15mm or more and less than 30N / 15mm
[0471] D: Maximum sealing strength is less than 20N / 15mm
[0472] (Insulation after degassing heat sealing (degassing insulation))
[0473] The outer packaging material was cut into a sample 40 of 120 mm × 200 mm and installed in a cold rolling metal mold in such a way that the sealant layer was in contact with the convex part of the molding machine. A deep drawing of 2.0 mm was performed at a molding speed of 15 mm / sec. After forming a deep drawing part 41, it was folded in half into a 120 mm × 100 mm (refer to Fig.11 (a)). Next, the upper edge 44 of 100 mm is heat-sealed with the tab 42 and the tab sealant 43 sandwiched therebetween (see Fig.11 (b)), heat seal the side edge 45 of 120 mm to make a bag (refer to Fig.11(c)). Then, in order to make the electrodes contact, a part of the outer layer of the sample 40 is scraped off to form an exposed portion 46 of the metal foil layer (see Fig.11 (d)). Next, 5 ml of an electrolyte solution containing 1 M LiPF6 was added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) in a small bag, and the lower edge 47 of the 100 mm side was sealed by heat sealing (refer to Fig.11 (e)). After that, the small bag was placed flat at 60°C for 24 hours, and the portion 48 closer to the inner side than the heat-sealed lower edge 47 was degassed and heat-sealed for 2 seconds at 190°C and 0.3 MPa (surface pressure) while the electrolyte was swallowed (refer to Fig.11 (f)). Next, the electrodes 49a and 49b were connected to the tab 42 and the exposed portion 46 of the metal foil layer, respectively, and 25V was applied using a withstand voltage-insulation resistance tester (manufactured by KIKUSUI, "TOS9201") to measure the resistance value at this time (refer to Fig.11 (g)). For samples with a resistance value less than 15MΩ, 25V is applied continuously for 2 hours to determine the insulation reduction area. By applying for a long time, the reaction products of the metal foil and the electrolyte will precipitate from the insulation reduction area, so the reduction area can be determined. The metal mold used has a molding area of 80mm×70mm (square tube type) and a punch corner radius (RCP) of 1.0mm. Based on the results, evaluation is performed according to the following standards.
[0474] A: Resistance value exceeds 200MΩ
[0475] B: Resistance value is 100MΩ or more and 200MΩ or less
[0476] C: Resistance value is 15MΩ or more and less than 100MΩ
[0477] D: Resistance value is less than 15MΩ
[0478] (Overall Quality)
[0479] The results of the above-mentioned evaluations are shown in Tables 5 and 6. In Tables 5 and 6 below, those without D evaluation in each evaluation result can be said to be excellent in overall quality.
[0480] Table 5
[0481]
[0482] Table 6
[0483]
[0484] In all the outer packaging materials obtained in Examples 1-1 to 1-32 and Comparative Examples 1-1 to 1-2, there is a stable area in the curve diagram of the seal strength evaluation. From the results shown in Tables 5 and 6, it can be seen that the outer packaging materials of Examples 1-1 to 1-32 are confirmed to have excellent insulation after degassing and heat sealing. It is further confirmed that the outer packaging materials of Examples 1-1 to 1-32 also have sufficient performance in terms of electrolyte lamination strength, electrolyte heat sealing strength, and degassing heat sealing strength. In contrast, it is confirmed that the sealing strength and insulation of the outer packaging materials of Comparative Examples 1-1 to 1-2 are poor.
[0485] When comparing Examples 1-1 to 1-3, it can be confirmed that by using a reactor-type TPO in which an elastomer is finely dispersed or a dynamically cross-linked PP-based elastomer grafted with an elastomer as the innermost layer's incompatible component (B), the adhesion of the sea-island interface is improved, and the sealing strength and insulation are improved.
[0486] When comparing Examples 1-21 to 1-31, it can be confirmed that when the sealant layer is thickened, the maximum sealing strength S M and ratio S S / S M Both of them were improved, and more excellent sealing strength and insulation were obtained. On the other hand, it was confirmed that even if the sealant layer was thinned, the sealing strength and insulation that could not be a problem as an outer packaging material were obtained.
[0487] (2) Examples and Comparative Examples of the Second Aspect
[0488] [Materials used]
[0489] Next, materials used in Examples 2-1 to 2-14 and Comparative Example 2-1 are shown below.
[0490] <Base layer (thickness: 15 μm)>
[0491] A nylon (Ny) membrane (manufactured by Toyobo Co., Ltd.) was used.
[0492] <First adhesive layer (thickness: 4 μm)>
[0493] A polyurethane adhesive (manufactured by Toyo Ink Co., Ltd.) obtained by blending a polyester polyol-based main agent with a toluene diisocyanate adduct-based curing agent was used.
[0494] <First anti-corrosion treatment layer (substrate layer side) and second anti-corrosion treatment layer (sealant layer side)>
[0495] (CL-1): "Sodium polyphosphate stabilized cerium oxide sol" adjusted to a solid content concentration of 10% by mass using distilled water as a solvent was used. The sodium polyphosphate stabilized cerium oxide sol was obtained by mixing 10 parts by mass of a sodium salt of phosphoric acid with 100 parts by mass of cerium oxide.
[0496] (CL-2): A composition composed of 90% by mass of "polyallylamine (manufactured by Nittobo Co., Ltd.)" adjusted to a solid content concentration of 5% by mass using distilled water as a solvent and 10% by mass of "polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Co., Ltd.)" was used.
[0497] (CL-3): A water-soluble phenolic resin (manufactured by Sumitomo Bakelite Co., Ltd.) was used as a solvent and adjusted to a solid content concentration of 1% by mass using a 1% by mass phosphoric acid aqueous solution. Chromium fluoride (CrF3) was added so that the amount of Cr present in the final dried film would be 10 mg / m 2 A chemical conversion treatment agent obtained by adjusting the concentration in a certain manner.
[0498] <Metal foil layer (thickness: 35 μm)>
[0499] A soft aluminum foil ("8079 material", manufactured by Toyo Aluminum Co., Ltd.) subjected to annealing and degreasing treatment was used.
[0500] <Second adhesive layer (thickness: 3 μm)>
[0501] As the adhesive for forming the second adhesive layer, the following adhesives a and b were prepared.
[0502] Adhesive a: An adhesive obtained by blending 10 parts by mass (solid content ratio) of a polyisocyanate compound having an isocyanurate structure with respect to 100 parts by mass of an acid-modified polyolefin resin dissolved in toluene.
[0503] Adhesive b: A polyurethane adhesive prepared by mixing polyester polyol composed of hydrogenated dimer fatty acid and diol and polyisocyanate so that the molar ratio (NCO / OH) becomes 2.
[0504] <Sealing layer>
[0505] The following materials were prepared as components (A) to (C) constituting the sealant layer-forming matrix resin composition.
[0506] ((A) ingredient)
[0507] Acid-modified PP: Acid-modified polypropylene.
[0508] Random PP: propylene-ethylene random copolymer.
[0509] ((B) ingredient)
[0510] Ethylene-α-olefin copolymer: an ethylene-propylene copolymer elastomer that is incompatible with acid-modified PP and random PP (component (A)).
[0511] Ethylene-butene-1 random copolymer: an ethylene-butene-1 random copolymer elastomer that is incompatible with the acid-modified PP and the random PP (component (A)).
[0512] ((B1) ingredient)
[0513] Block copolymer 1: A block copolymer composed of crystalline ethylene units and ethylene-butylene units and having no compatibility with acid-modified PP and random PP (component (A)).
[0514] Block copolymer 2: A block copolymer composed of propylene units and ethylene units and having no compatibility with the acid-modified PP and random PP (component (A)).
[0515] Graft copolymer: A graft copolymer composed of a polyolefin main chain and a polystyrene side chain, which is incompatible with acid-modified PP and random PP (component (A)).
[0516] ((C) ingredient)
[0517] Atactic copolymer: an atactic propylene-α-olefin copolymer compatible with the acid-modified PP (component (A)).
[0518] Propylene-butene-1 random copolymer: a propylene-butene-1 random copolymer elastomer having compatibility with random PP (component (A)).
[0519] [Production of outer packaging materials]
[0520] (Example 2-1)
[0521] First, the first and second anti-corrosion treatment layers were provided on the metal foil layer in the following steps. That is, (CL-1) was applied on both sides of the metal foil layer by micro-gravure coating so that the dry coating amount reached 70 mg / m 2 In the drying unit, a sintering treatment was performed at 200° C. Then, (CL-2) was coated on the obtained layer by micro-gravure coating so that the dry coating amount reached 20 mg / m 2 , thereby forming a composite layer composed of (CL-1) and (CL-2) as the first and second anti-corrosion treatment layers. The composite layer exhibits anti-corrosion performance by combining (CL-1) and (CL-2).
[0522] Next, the first anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers was adhered to the substrate layer using a polyurethane adhesive (first adhesive layer) by dry lamination. It was installed in the unwinding section of the extrusion laminator, and the material of the sealant layer was co-extruded onto the second anti-corrosion treatment layer under the processing conditions of 270°C and 100m / min, so that the metal foil side layer (hereinafter also referred to as "AL side layer") (thickness of 8.3μm) and the innermost layer (thickness of 16.7μm) were stacked in sequence as the sealant layer. In addition, the AL side layer and the innermost layer were prepared by using a twin-screw extruder to make a mixture of various materials and then water-cooled and granulated for the above-mentioned extrusion lamination. A mixture of acid-modified PP ((A) component, 55.0 mass%), ethylene-α-olefin copolymer ((B) component, 20.0 mass%) and atactic copolymer ((C) component, 25.0 mass%) was used in the formation of the AL side layer. The innermost layer is formed by using a mixture of random PP ((A) component, 63.6 mass%), ethylene-butene-1 random copolymer ((B) component, 9.1 mass%), block copolymer 2 ((B1) component, 9.1 mass%), and propylene-butene-1 random copolymer ((C) component, 18.2 mass%). In addition, the composition of each layer is also shown in the following Table 7. The numerical values in the sealant layer column in Table 7 represent the content or thickness of each component in each layer or the whole sealant layer.
[0523] The thus obtained stack is wound around a roller heated to 190°C for conveyance, and the stack is heat treated at 190°C for about 0.5 seconds to produce the outer packaging material of Example 2-1 (a stack of substrate layer / first adhesive layer / first anti-corrosion treatment layer / metal foil layer / second anti-corrosion treatment layer / AL side layer (sealant layer 16a) / innermost layer (sealant layer 16b)).
[0524] (Example 2-2)
[0525] The outer packaging material of Example 2-2 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 50.0 mass%), ethylene-α-olefin copolymer ((B) component, 18.2 mass%), block copolymer 2 ((B1) component, 9.1 mass%), and atactic copolymer ((C) component, 22.7 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 70.0 mass%), ethylene-butene-1 random copolymer ((B) component, 10.0 mass%), and propylene-butene-1 random copolymer ((C) component, 20.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0526] (Example 2-3)
[0527] The outer packaging material of Example 2-3 was produced in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 50.0 mass%), ethylene-α-olefin copolymer ((B) component, 18.2 mass%), block copolymer 2 ((B1) component, 9.1 mass%) and atactic copolymer ((C) component, 22.7 mass%) was used in the formation of the AL side layer (sealant layer 16a). In addition, the composition of each layer is also shown in Table 7 below.
[0528] (Example 2-4)
[0529] The outer packaging material of Example 2-4 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 52.4 mass%), ethylene-α-olefin copolymer ((B) component, 19.0 mass%), block copolymer 2 ((B1) component, 4.8 mass%) and atactic copolymer ((C) component, 23.8 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 66.7 mass%), ethylene-butene-1 random copolymer ((B) component, 9.5 mass%), block copolymer 2 ((B1) component, 4.8 mass%) and propylene-butene-1 random copolymer ((C) component, 19.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0530] (Example 2-5)
[0531] The outer packaging material of Example 2-5 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 54.4 mass%), ethylene-α-olefin copolymer ((B) component, 19.8 mass%), block copolymer 2 ((B1) component, 1.0 mass%), and atactic copolymer ((C) component, 24.8 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 69.3 mass%), ethylene-butene-1 random copolymer ((B) component, 9.9 mass%), block copolymer 2 ((B1) component, 1.0 mass%), and propylene-butene-1 random copolymer ((C) component, 19.8 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0532] (Example 2-6)
[0533] The outer packaging material of Example 2-6 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 55.0 mass%), block copolymer 2 ((B1) component, 20.0 mass%), and random stereostructure copolymer ((C) component, 25.0 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 70.0 mass%), block copolymer 2 ((B1) component, 10.0 mass%), and propylene-butene-1 random copolymer ((C) component, 20.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0534] (Example 2-7)
[0535] The outer packaging material of Example 2-7 was manufactured in the same manner as in Example 2-2 except that a mixture of random PP ((A) component, 70.0 mass%), block copolymer 2 ((B1) component, 10.0 mass%) and propylene-butene-1 random copolymer ((C) component, 20.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0536] (Example 2-8)
[0537] First, the first and second anti-corrosion treatment layers were provided on the metal foil layer in the following steps. That is, (CL-3) was applied on both sides of the metal foil layer by micro-gravure coating so that the dry coating amount reached 30 mg / m 2 In the drying unit, a sintering treatment was performed at 200° C. Then, (CL-2) was coated on the obtained layer by micro-gravure coating so that the dry coating amount reached 20 mg / m 2 , thereby forming a composite layer composed of (CL-3) and (CL-2) as the first and second anti-corrosion treatment layers. The composite layer exhibits anti-corrosion performance by compounding the two (CL-3) and (CL-2). Using the metal foil layer provided with the first and second anti-corrosion treatment layers, the outer packaging material of Example 2-8 was manufactured in the same manner as in Example 2-7. In addition, the composition of each layer is also shown in Table 7 below.
[0538] (Example 2-9)
[0539] The first and second anti-corrosion treatment layers were provided on the metal foil layer in the same manner as in Example 2-1. The first anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers was adhered to the substrate layer using a polyurethane adhesive (first adhesive layer) by dry lamination. Next, the second anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers was adhered to the sealant layer 16 (innermost layer) (thickness 25 μm) by dry lamination using adhesive a (second adhesive layer) to manufacture the outer packaging material of Example 2-9. A mixture of random PP ((A) component, 70.0 mass%), block copolymer 2 ((B1) component, 10.0 mass%) and propylene-butene-1 random copolymer ((C) component, 20.0 mass%) was used in the formation of the innermost layer (sealant layer 16). In addition, the composition of each layer is also shown in Table 7 below.
[0540] (Example 2-10)
[0541] The first and second anti-corrosion treatment layers were provided on the metal foil layer in the same manner as in Example 2-1. The first anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers was adhered to the substrate layer using a polyurethane adhesive (first adhesive layer) by dry lamination. Next, the second anti-corrosion treatment layer of the metal foil layer provided with the first and second anti-corrosion treatment layers was adhered to the sealant layer 16 (innermost layer) (thickness 25 μm) by dry lamination using adhesive b (second adhesive layer) to manufacture the outer packaging material of Example 2-10. A mixture of random PP ((A) component, 70.0 mass%), block copolymer 2 ((B1) component, 10.0 mass%) and propylene-butene-1 random copolymer ((C) component, 20.0 mass%) was used in the formation of the innermost layer (sealant layer 16). In addition, the composition of each layer is also shown in Table 7 below.
[0542] (Example 2-11)
[0543] The outer packaging material of Example 2-11 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 72.7 mass%), ethylene-α-olefin copolymer ((B) component, 18.2 mass%) and block copolymer 2 ((B1) component, 9.1 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 90.0 mass%) and block copolymer 2 ((B1) component, 10.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0544] (Example 2-12)
[0545] The outer packaging material of Example 2-12 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 50.0 mass%), ethylene-α-olefin copolymer ((B) component, 18.2 mass%), block copolymer 1 ((B1) component, 9.1 mass%) and atactic copolymer ((C) component, 22.7 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 63.6 mass%), ethylene-butene-1 random copolymer ((B) component, 9.1 mass%), block copolymer 2 ((B1) component, 9.1 mass%) and propylene-butene-1 random copolymer ((C) component, 18.2 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0546] (Example 2-13)
[0547] The outer packaging material of Example 2-13 was manufactured in the same manner as in Example 2-12, except that a mixture of random PP ((A) component, 70.0 mass%), block copolymer 2 ((B1) component, 10.0 mass%) and propylene-butene-1 random copolymer ((C) component, 20.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0548] (Example 2-14)
[0549] The outer packaging material of Example 2-14 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 50.0 mass%), ethylene-α-olefin copolymer ((B) component, 18.2 mass%), graft copolymer ((B1) component, 9.1 mass%), and atactic copolymer ((C) component, 22.7 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 70.0 mass%), graft copolymer ((B1) component, 10.0 mass%), and propylene-butene-1 random copolymer ((C) component, 20.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0550] (Comparative Example 2-1)
[0551] The outer packaging material of Comparative Example 2-1 was manufactured in the same manner as in Example 2-1, except that a mixture of acid-modified PP ((A) component, 52.0 mass%), ethylene-α-olefin copolymer ((B) component, 45.0 mass%) and atactic copolymer ((C) component, 3.0 mass%) was used in the formation of the AL side layer (sealant layer 16a); and a mixture of random PP ((A) component, 52.0 mass%), ethylene-butene-1 random copolymer ((B) component, 45.0 mass%) and propylene-butene-1 random copolymer ((C) component, 3.0 mass%) was used in the formation of the innermost layer (sealant layer 16b). In addition, the composition of each layer is also shown in Table 7 below.
[0552] Table 7
[0553]
[0554] <Evaluation>
[0555] The following evaluation tests were performed on the outer packaging materials obtained in Examples 2-1 to 2-14 and Comparative Example 2-1.
[0556] (Shrinkage ratio and aspect ratio of the region where component (B) exists)
[0557] A portion of the outer packaging material was cut and heated in an oven at 190°C for 30 seconds to prepare samples before and after heating, and sealed for cross-sectional observation. A scanning electron microscope (SEM) was used to observe the range of 50 μm in the MD direction and 25 μm in the VD direction in the cross-section of the sealant layer along the VD direction and MD direction of the above sample, and the length L in the MD direction of any five or more regions where the (B) component in the sample before heating exists was measured. MD and the length Lh in the MD direction of any five or more regions where the component (B) exists in the heated sample MD , find the average length LA MD and LAh MD . Then, from the obtained LA MD and LAh MD Calculate the shrinkage ratio (LAh) of the region where component (B) exists before and after heating MD / LA MD ).
[0558] In addition, the cross-section of the heated sample along the VD direction and the MD direction of the sealant layer was observed by SEM in the range of 50 μm in the MD direction and 25 μm in the VD direction, and the length Lh of any five or more regions where the component (B) existed in the MD direction was measured. MD And the length Lh in the VD direction VD , find the average length LAh MDand LAh VD . Then, from the obtained LAh MD and LAh VD The aspect ratio (LAh) of the region where component (B) exists is calculated. MD / LAh VD ).
[0559] (Seal Strength)
[0560] Cut the outer packaging material into a sample of 60mm×120mm, fold it in half, and heat seal one side with a 10mm wide sealing strip at 190℃ and 0.5MPa for 3 seconds. After the heat-sealed sample is stored at room temperature for 24 hours, cut the first heat-sealed side into 15mm wide (refer to Figure 8 ), the sealing strength (T-peel strength) was continuously measured using a testing machine (manufactured by INSTRON). The test was conducted in accordance with JIS K6854 at 23°C, 50% RH, and a peeling speed of 50 mm / min. The sealing strength was evaluated according to the following criteria based on the results of the maximum value of the initial sealing strength (rupture strength) after the peeling started.
[0561] S: Bursting strength is 60N / 15mm or more
[0562] A: The bursting strength is 50N / 15mm or more and less than 60N / 15mm
[0563] B: Bursting strength is 40N / 15mm or more and less than 50N / 15mm
[0564] C: Bursting strength is 35N / 15mm or more and less than 40N / 15mm
[0565] D: Breaking strength less than 35N / 15mm
[0566] (Electrolyte Lamination Strength)
[0567] The electrolyte solution to which LiPF6 is added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) in a manner to reach 1M is filled in a Teflon (registered trademark) container, and a sample of the outer packaging material cut into 15mm×100mm is placed therein, and the sample is sealed and stored at 85°C for 24 hours. After co-washing, the lamination strength (T-peel strength) between the metal foil layer / sealant layer is measured using a testing machine (manufactured by INSTRON). The test is carried out according to JIS K6854, at 23°C, 50% RH ambient gas, and a peeling speed of 50mm / min. Based on the results, evaluation is performed according to the following standards.
[0568] A: Lamination strength exceeds 7N / 15mm
[0569] B: Lamination strength is 6N / 15mm or more and 7N / 15mm or less
[0570] C: Lamination strength is 5N / 15mm or more and less than 6N / 15mm
[0571] D: Lamination strength is less than 5N / 15mm
[0572] (Electrolyte heat seal strength)
[0573] The outer packaging material was cut into a sample of 60 mm × 120 mm, and folded in half with the sealant layer facing the inside. One side was heat-sealed for 3 seconds at 190°C and 0.5 MPa with a 10 mm wide sealing strip to form a heat-sealed portion. After that, the remaining two sides were also heat-sealed. 2 ml of an electrolyte solution in which LiPF6 was added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) to reach 1 M was injected into the bag-shaped outer packaging material. After the small bag was stored at 60°C for 24 hours, the first heat-sealed side was cut into 15 mm wide (refer to Fig. 9 ), starting from one end of the heat-sealed portion (the end in contact with the electrolyte), the seal strength (T-peel strength) was continuously measured using a testing machine (manufactured by INSTRON). The test was conducted in accordance with JIS K6854 at 23°C, 50% RH, and a peeling speed of 50 mm / min. The rupture strength obtained in the same manner as the "seal strength" item was evaluated according to the following standards.
[0574] S: Bursting strength is 50N / 15mm or more
[0575] A: The bursting strength is 45N / 15mm or more and less than 50N / 15mm
[0576] B: Bursting strength is 35N / 15mm or more and less than 45N / 15mm
[0577] C: Bursting strength is 25N / 15mm or more and less than 35N / 15mm
[0578] D: Breaking strength less than 25N / 15mm
[0579] (Degassing heat seal strength (Degassing heat seal strength))
[0580] Cut the outer packaging material into 75mm×150mm samples and fold them in half to 37.5mm×150mm with the sealant layer facing inside (refer to Fig.10(a)), heat seal the 150mm side and one 37.5mm side to make a bag. After that, inject 5ml of an electrolyte solution in which LiPF6 is added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) to reach 1M into the small bag, heat seal the other 37.5mm side, and seal it with the sealing part DS1 to obtain a small bag. Next, after the small bag is stored at 60°C for 24 hours, the central part of the small bag is heat sealed at 190°C and 0.3MPa for 2 seconds with a 10mm wide sealing strip in the state containing the electrolyte (degassing heat seal part DS2, refer to Fig.10 (b)). In order to stabilize the sealed portion, after being stored at room temperature for 24 hours, the area including the degassing heat seal portion DS2 was cut into a 15 mm width (refer to Fig.10 (c) The seal strength (T-type peel strength) was measured from one end of the degassing heat seal portion (the end in contact with the electrolyte) using a testing machine (manufactured by INSTRON). The test was conducted in accordance with JIS K6854 at a peeling speed of 50 mm / min at 23°C and 50% RH. The burst strength obtained in the same manner as in the "seal strength" item was evaluated according to the following criteria.
[0581] S: Bursting strength is 45N / 15mm or more
[0582] A: The bursting strength is 40N / 15mm or more and less than 45N / 15mm
[0583] B: Bursting strength is 30N / 15mm or more and less than 40N / 15mm
[0584] C: Bursting strength is 20N / 15mm or more and less than 30N / 15mm
[0585] D: Breaking strength less than 20N / 15mm
[0586] (Insulation after degassing heat sealing (degassing insulation))
[0587] The outer packaging material was cut into a sample 40 of 120 mm × 200 mm and installed in a cold rolling metal mold in such a way that the sealant layer was in contact with the convex part of the molding machine. A deep drawing of 2.0 mm was performed at a molding speed of 15 mm / sec. After forming a deep drawing part 41, it was folded in half into a 120 mm × 100 mm (refer to Fig.11 (a)). Next, the upper edge 44 of 100 mm is heat-sealed with the tab 42 and the tab sealant 43 sandwiched therebetween (see Fig.11 (b)), heat seal the side edge 45 of 120 mm to make a bag (refer to Fig.11(c)). Then, in order to make the electrodes contact, a part of the outer layer of the sample 40 is scraped off to form an exposed portion 46 of the metal foil layer (see Fig.11 (d)). Next, 5 ml of an electrolyte solution containing 1 M LiPF6 was added to a mixed solution of ethylene carbonate / diethyl carbonate / dimethyl carbonate = 1 / 1 / 1 (mass ratio) in a small bag, and the lower edge 47 of 100 mm was sealed by heat sealing (refer to Fig.11 (e)). After that, the small bag was placed flat at 60°C for 24 hours, and the portion 48 further inside the heat-sealed lower edge portion 47 was degassed and heat-sealed for 2 seconds at 190°C and 0.3 MPa (surface pressure) while the electrolyte was swallowed (refer to Fig.11 (f)). Next, the electrodes 49a and 49b were connected to the tab 42 and the exposed portion 46 of the metal foil layer, respectively, and 25V was applied using a withstand voltage-insulation resistance tester (manufactured by KIKUSUI, "TOS9201") to measure the resistance value at this time (refer to Fig.11 (g)). For samples with a resistance value less than 15MΩ, continue to apply 25V for 2 hours to determine the insulation reduction area. By applying for a long time, the reaction products of the metal foil and the electrolyte will precipitate from the insulation reduction area, so the reduction area can be determined. The metal mold used has a molding area of 80mm×70mm (square tube type) and a punch corner radius (RCP) of 1.0mm. Based on the results, evaluation is performed according to the following standards.
[0588] A: Resistance value is above 200MΩ
[0589] B: Resistance value is above 100MΩ and less than 200MΩ
[0590] C: Resistance value is 15MΩ or more and less than 100MΩ
[0591] D: Resistance value is less than 15MΩ
[0592] The results of the shrinkage ratio and aspect ratio of the component (B), sealing strength, electrolyte lamination strength, electrolyte sealing strength, degassing heat seal strength, and degassing insulation evaluated as above are shown in the following Table 8 together with the contents of the component (B) and the component (C) based on the entire sealant layer. In the following Table 8, those without D evaluation in each evaluation result can be said to have excellent overall quality.
[0593] Table 8
[0594]
[0595] Fig.12These are SEM images of the cross-section along the VD direction and MD direction of the sealant layer of the outer packaging material for the storage device obtained in Example 2-7, (a) is the image before heating at 190°C for 30 seconds, and (b) is the image after heating at 190°C for 30 seconds. Fig.12 The layers confirmed in (a) are, from the top, the metal foil layer 13, the AL side layer before heating (sealant layer 16a), and the innermost layer before heating (sealant layer 16b). Fig.12 (a) In the AL side layer and the innermost layer, the gray regions 162a and 162b where the component (A) exists and the white regions 164a and 164b where the component (B) exists can be confirmed. Fig.12 (a) It can be further confirmed that the regions 164a and 164b where the component (B) exists are stretched in the MD direction. Fig.12 The layers confirmed in (b) are, from the top, the metal foil layer 13, the heated AL side layer (heated sealant layer 16ha), and the heated innermost layer (heated sealant layer 16hb). Fig.12 In (b) showing the cross section after heating, it can be confirmed that the gray areas 162ha and 162hb of the (A) component and the white areas 164ha and 164hb of the (B) component are present in the AL side layer 16ha and the innermost layer 16hb, respectively. Fig.12 (a) with Fig.12 In (b), it can be confirmed that the (B) component existing regions 164ha and 164hb after heating appear to be slightly shrunk in the MD direction compared to before heating. However, the shrinkage ratio is 0.63, which can be said to be small.
[0596] In addition, from the results shown in Table 8, it can be seen that the outer packaging materials for power storage devices obtained in Examples 2-1 to 2-14 have a low shrinkage sealant layer with a shrinkage rate of 0.20 or more, so the insulation after degassing and heat sealing is excellent. It is further confirmed that the outer packaging materials of Examples 2-1 to 2-14 have sufficient performance in terms of electrolyte lamination strength, electrolyte heat sealing strength, and degassing heat sealing strength. In contrast, it is confirmed that the sealing strength and insulation of the outer packaging material of Comparative Example 2-1 are poor.
[0597] Explanation of symbols
[0598] 10, 20, 30 outer packaging material for power storage device, 11 base material layer, 12 first adhesive layer, 13 metal foil layer, 14 anti-corrosion treatment layer, 16 sealant layer, 16a first sealant layer, 16b second sealant layer, 16c third sealant layer, 17 second adhesive layer, 162 area where polypropylene resin exists, 164 area where incompatible components exist, 164h area where incompatible components exist after heating, DS1 sealing part, DS2 degassing heat sealing part.
Claims
1. An outer packaging material for a power storage device, comprising at least a base layer, a metal foil layer having an anti-corrosion treatment layer on one or both surfaces, and a sealant layer in this order, wherein: The sealant layer contains a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin. The content of the incompatible component (B) is 1 to 40% by mass based on the total amount of the sealant layer, and the incompatible component (B) contains a compound (B1) having a compatible portion and an incompatible portion compatible with the polypropylene resin (A), and the compound (B1) contains a graft copolymer, or a block copolymer having a block composed of crystalline ethylene units and a block composed of ethylene-butylene units, a block copolymer having a block composed of ethylene and a block composed of ethylene-octene 1, or a block copolymer having a block composed of propylene units and a block composed of ethylene units, For the bonded portion formed by heat-sealing and bonding the outer packaging materials overlapped with the sealant layers facing each other under the conditions of temperature 190° C., pressure 0.5 MPa, and 3 seconds, in a graph showing the relationship between the displacement from one end and the seal strength when the seal strength is measured continuously from one end to the other end, the maximum seal strength S M 45N / 15mm or more and meets the following conditions (1) or (2): (1) After obtaining the maximum sealing strength S M After the displacement of , there is a stable region of sealing strength, and the sealing strength S in this stable region S With the maximum sealing strength S M Ratio S S / S M is 0.5 or more, (2) There is no stable region, and the maximum sealing strength S is obtained. M The average sealing strength S between the displacement of the first end and the displacement of the other end A With the maximum sealing strength S M Ratio S A / S M It is 0.5 or more.
2. The outer packaging material for a power storage device according to claim 1, wherein In the graph, the ratio S S / S M Or the ratio S A / S M It is above 0.
6.
3. The outer packaging material for a power storage device according to claim 1, wherein The sealant layer is composed of a plurality of layers, at least one of which is a layer containing the polypropylene resin (A) and the incompatible component (B) that is incompatible with the polypropylene resin, and the incompatible component (B) contains the compound (B1).
4. The outer packaging material for a power storage device according to any one of claims 1 to 3, wherein The incompatible component (B) contains an ethylene-α-olefin copolymer.
5. The outer packaging material for a power storage device according to any one of claims 1 to 3, wherein The sealant layer further contains a compatible elastomer (C) that is compatible with the polypropylene resin (A). The compatibilizing elastomer (C) contains a propylene-α-olefin copolymer.
6. An outer packaging material for a power storage device, comprising at least a base layer, a metal foil layer having an anti-corrosion treatment layer on one or both surfaces, and a sealant layer in this order, wherein: The sealant layer contains a polypropylene resin (A) and an incompatible component (B) that is incompatible with the polypropylene resin, and has a region where the polypropylene resin (A) exists and a plurality of regions where the incompatible component (B) exists surrounded by the polypropylene resin (A), and the incompatible component (B) contains a compound (B1) having a compatible portion and an incompatible portion that are compatible with the polypropylene resin (A), the content of the compound (B1) is 1 to 40% by mass based on the total amount of the sealant layer, and the compound (B1) contains a graft copolymer, or a block copolymer having a block composed of crystalline ethylene units and a block composed of ethylene-butene units, a block copolymer having a block composed of ethylene and a block composed of ethylene-octene 1, or a block copolymer having a block composed of propylene units and a block composed of ethylene units, The sealant layer comprises a low shrinkage sealant layer, wherein the low shrinkage sealant layer is an average length LAh in the MD direction of the region where the incompatible component (B) exists in the cross section along the thickness direction and the MD direction of the sealant layer after the outer packaging material for the storage device is heated at 190°C for 30 seconds. MD The average length LA of the region where the incompatible component (B) exists in the cross section along the thickness direction and the MD direction in the MD direction MD The ratio of LAh MD / LA MD The layer is 0.20 or more.
7. The outer packaging material for a power storage device according to claim 6, wherein The average length LAh in the MD direction of the region where the incompatible component (B) exists in the cross section along the thickness direction and the MD direction of the sealant layer after the outer packaging material for a storage battery device is heated at 190° C. for 30 seconds MD The average length LAh in the thickness direction VD The ratio of LAh MD / LAh VD Above 2.
50.
8. The outer packaging material for a power storage device according to claim 6 or 7, wherein The sealant layer is composed of multiple layers, at least one of which is the low-shrinkage sealant layer.
9. The outer packaging material for a power storage device according to claim 6 or 7, wherein The sealant layer is composed of multiple layers, and the layer closest to the metal foil layer is the low-shrinkage sealant layer.
10. The outer packaging material for a power storage device according to claim 6 or 7, wherein The sealant layer further contains a compatible elastomer (C) that is compatible with the polypropylene resin (A). The compatibilizing elastomer (C) contains a propylene-α-olefin copolymer.
11. The outer packaging material for a power storage device according to claim 6 or 7, wherein: The sealant layer further contains a compatible elastomer (C) that is compatible with the polypropylene resin (A). The sealant layer is composed of multiple layers, in which the polypropylene resin (A) contains acid-modified polypropylene in the layer closest to the metal foil layer, and the compatible elastomer (C) contains atactic polypropylene or atactic propylene-α-olefin copolymer.
12. The outer packaging material for a power storage device according to any one of claims 1 to 3 and 6 to 7, wherein The thickness of the sealant layer is 10-45 μm.
13. The outer packaging material for an electrical storage device according to any one of claims 1 to 3 and 6 to 7, in, An adhesive layer is further provided between the metal foil layer and the sealant layer. The adhesive layer contains an acid-modified polyolefin and at least one curing agent selected from a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxyl group, a compound having an oxazoline group, and a carbodiimide compound.
Citation Information
Patent Citations
Material for wrapping lithium ion battery
JP2002245983A