Hard coating film

The hard coating film, with a specific resin composition and properties, addresses the challenge of repeated folding and scratch resistance in flexible display devices, ensuring durability and performance.

CN119095923APending Publication Date: 2024-12-06DEXERIALS AMERICA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280095453.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-03
Filing Date
2022-11-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Conventional hard coating materials for flexible display devices lack the ability to withstand repeated folding without cracking or separating from the screen, and they also suffer from reduced scratch resistance when made flexible.

Method used

A hard coating film comprising a base material and a hard coating layer made of a resin composition containing a multifunctional (meth)acrylic monomer with a functionality greater than or equal to 4 and aliphatic polyurethane acrylate, with specific glass transition temperature and loss tangent properties, and optionally including metal oxide nanoparticles, to enhance flexibility and scratch resistance.

Benefits of technology

The hard coating film can withstand at least 100,000 folds without cracking or separating and maintains excellent scratch resistance, even in high-temperature environments, while retaining optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095923A_ABST
    Figure CN119095923A_ABST
Patent Text Reader

Abstract

The hard coating film (10) includes a base material (11) and a hard coating layer (12) composed of a cured product of a resin composition containing a resin (A) and a resin (B), the hard coating layer (12) being laminated on the base material (11). The resin (A) is a polyfunctional (meth) acrylic monomer having a weighted average functionality of 4 or more. The resin (B) is an aliphatic urethane acrylate. The hard coat layer (12) has a glass transition temperature (Tg) of 50 DEG C or more and 100 DEG C or less. When the loss tangent (tan [delta]) of the hard coating layer (12) is measured by a dynamic viscoelasticity measurement method in which a dynamic load at a frequency of 1-Hz is applied, the loss tangent (tan [delta]) at a glass transition temperature (Tg) is 0.07-0.15.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a hard coating film. Background Art

[0002] Display devices such as liquid crystal display (LCD), plasma display (PDP) or organic EL display (OLED) are widely used in smart phones, mobile phones, mobile personal computers, car navigation devices, etc. Generally speaking, the outermost surface of the screen of the display device is provided with a protective film to prevent the screen from being scratched. The protective film includes a base material and a hard coating layer laminated on the base material. Conventional hard coating layers are made of materials each having a high crosslinking density.

[0003] Currently, foldable flexible display devices with flexible screens are being developed. Such flexible display devices need to be folded repeatedly in one or more directions for multiple times, such as hundreds of thousands of times. Therefore, the protective film covering the screen of the flexible display device also needs to be flexible to withstand the above multiple and repeated folding.

[0004] However, the material with high crosslink density used for conventional hard coating has hardness but high shrinkage, resulting in lack of flexibility. Therefore, when the flexible display device is covered with a protective film with a conventional hard coating and the flexible display device is repeatedly folded many times (such as hundreds of thousands of times), the hard coating and the protective film will easily separate from the screen. In addition, when the material of the hard coating has a high crosslink density, the hard coating will be fragile, or even if the hard coating itself is thin, the hard coating will easily crack.

[0005] Thus, for example, Patent Document 1 discloses a hard coating layer having a thickness of 5 μm as a flexible hard coating layer which can be bent around a mandrel having a diameter of 2 mm without cracking.

[0006] Reference List

[0007] Patent Literature

[0008] Patent document 1: US2009 / 0004478 A1 Summary of the invention

[0009] Technical issues

[0010] However, Patent Document 1 does not disclose the repeated folding of the hard coating layer many times (eg, hundreds of thousands of times), the material of the hard coating layer required for such repeated folding, the properties of the hard coating layer, and the like.

[0011] In addition, if the hard coating layer is made of a soft material that allows multiple folding, the scratch resistance of the hard coating layer will be reduced, and therefore, the hard coating layer will be easily scratched. Therefore, the hard coating layer to be used as a protective film for a flexible display device not only needs to have a performance that can withstand the above-mentioned multiple and repeated folding, but also needs to have scratch resistance to prevent scratches.

[0012] Therefore, the present invention has been made in view of the above-mentioned problems, and an object thereof is to provide a hard coating film having both the performance of being able to withstand multiple and repeated folding and the scratch resistance.

[0013] Solution to the problem

[0014] In order to solve the above problems, according to one aspect of the present invention, a hard coating film is provided, the hard coating film comprising:

[0015] Base materials; and

[0016] A hard coating layer comprising a cured product of a resin composition containing a resin (A) and a resin (B), the hard coating layer being laminated on the base material, wherein

[0017] Resin (A) is a multifunctional (meth) acrylic monomer having a weighted average functionality greater than or equal to 4,

[0018] Resin (B) is aliphatic polyurethane acrylate,

[0019] The hard coating has a glass transition temperature Tg greater than or equal to 50° C. and less than or equal to 100° C., and

[0020] The loss tangent tanδ at the glass transition temperature Tg is greater than or equal to 0.07 and less than or equal to 0.15,

[0021] The loss tangent tan δ of the hard coating layer is measured by a dynamic viscoelasticity measurement method applying a 1-Hz frequency dynamic load.

[0022] The resin composition may further contain metal oxide nanoparticles having an average particle size of less than or equal to 100 nm.

[0023] In certain embodiments, the content of the metal oxide nanoparticles contained in the resin composition may be greater than or equal to 2 mass % and less than or equal to 5 mass % of the total solid content of the resin composition of the hard coating layer.

[0024] The metal oxide in the metal oxide nanoparticles may be either or both of silicon dioxide and aluminum oxide.

[0025] The Mohs hardness of the metal oxide nanoparticles may be greater than 6.

[0026] The water contact angle of the surface of the hard coating after wear can be greater than 100°, wherein the wear is performed using a wear tester by using steel wool #0000, and the surface of the hard coating is worn with steel wool under the conditions of a load of 1000g, a speed of 50mm / sec, a reciprocating distance of 40mm and 2500 reciprocations.

[0027] In certain embodiments, the water contact angle of the surface of the hard coating before abrasion may be greater than 110°.

[0028] In certain embodiments, the water contact angle of the surface of the hard coating after abrasion may decrease by less than 13% relative to the water contact angle of the surface of the hard coating before abrasion.

[0029] In certain embodiments, the content of the resin (A) contained in the resin composition may be greater than twice and less than nine times the content of the resin (B).

[0030] In certain embodiments, the content of resin (A) contained in the resin composition may be greater than or equal to 20 mass % and less than or equal to 40 mass %, and the content of resin (B) contained in the resin composition may be greater than or equal to 2 mass % and less than or equal to 15 mass %.

[0031] The hard coat film may be configured to be folded at least one hundred thousand times by bending inwardly or outwardly without causing any cracking, separation between layers, or loss of optical properties.

[0032] The base material may be a thermoplastic base material having a thickness greater than or equal to 10 μm and less than or equal to 200 μm.

[0033] The resin composition may contain a fluorine compound, and the fluorine compound may segregate to the first region located on the surface side of the hard coating layer.

[0034] In addition, the segregated fluorine compound can provide an antifouling effect.

[0035] In certain embodiments, the fluorine compound may segregate to the surface of the hardcoat.

[0036] In certain embodiments, the hard coat film can be configured to be folded at least one hundred thousand times by bending inward or outward without any loss of optical performance, wherein the optical performance is one or more selected from the group consisting of total transmittance (%), transmittance haze, gloss, and change in chromaticity b* (intensity of hue from blue to yellow).

[0037] In certain embodiments, there may be a second region on the base material side of the hard coating where the fluorine compound does not segregate.

[0038] Advantageous Effects of the Invention

[0039] According to one embodiment of the present invention, a hard coating film having both the performance of being able to withstand multiple and repeated folding and having scratch resistance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1is a cross-sectional view showing a hard coating film according to one embodiment of the present invention.

[0041] Figure 2 is a cross-sectional view showing a hard coating film according to another embodiment of the present invention.

[0042] Figure 3 is a cross-sectional view showing a hard coating film according to another embodiment of the present invention.

[0043] Figure 4 is a schematic diagram showing a hard coating film manufacturing apparatus according to the embodiment. DETAILED DESCRIPTION

[0044] Embodiments of the present invention will be described in detail below with reference to the accompanying drawings. The dimensions, materials, specific values, etc. described in such embodiments are only for the convenience of understanding the present invention, and unless otherwise specified, the present invention is not limited thereto. Note that in this specification and the accompanying drawings, elements having substantially the same function and configuration are assigned the same reference numerals, and their repeated descriptions will be omitted. In addition, illustrations of elements that are not directly related to the present invention may be omitted.

[0045] Note that in the drawings to be referred to in the following description, the sizes of some components may be exaggerated for ease of description. Therefore, the relative sizes of the components shown in the drawings do not necessarily convey the actual precise proportional relationship between the components.

[0046] [1. Overall configuration of hard coat film]

[0047] First, refer to Figure 1 The overall configuration of a hard coating film 10 according to one embodiment of the present invention is described. Figure 1 2 is a cross-sectional view showing a hard coating film 10 according to the present embodiment.

[0048] The hard coating film 10 according to the present embodiment is provided on the outermost surface of the flexible display device as a protective film, for example, to prevent scratches. Figure 1 As shown in FIG. 1 , the hard coating film 10 according to the present embodiment includes a base material 11 and a hard coating layer 12. The hard coating layer 12 is laminated on the base material 11. Each layer will be described below.

[0049] [Basic material 11]

[0050] The base material 11 is made of, for example, a transparent material that can transmit light in the visible light range of 350 to 830 nm in wavelength.

[0051] The base material 11 may be, for example, an inorganic material such as a glass film, or an organic material such as a plastic film.

[0052] The material of the plastic film can be, for example, one or more selected from polyester resin, acetate resin, polyether sulfone resin, polycarbonate resin, polyamide resin, polyimide resin, polyolefin resin, poly(meth)acrylate resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin, polyarylate resin and polyphenylene sulfide resin, preferably one or more selected from polyester resin, acetate resin, polycarbonate resin, polyimide resin and polyolefin resin.

[0053] Considering aspects such as processing capability, flexibility, cost and performance, the thickness of the base material 11 is preferably greater than or equal to 10 μm and less than or equal to 200 μm, for example, more preferably greater than or equal to 20 μm and less than or equal to 100 μm, and even more preferably greater than or equal to 40 μm and less than or equal to 60 μm.

[0054] When the thickness of the base material 11 is greater than or equal to 10 μm, at least one of the following advantages will be achieved. Since the rigidity of the base material 11 itself can be ensured, the hard coating film 10 is less likely to wrinkle even when stress is applied to the hard coating film 10. In addition, even if the hard coating layer 12 is continuously formed on the base material 11, since the hard coating film 10 is less likely to wrinkle, manufacturing problems involving the hard coating film 10 can be reduced. In addition, the reduction in curling of the hard coating film 10 eliminates the need to laminate another coating layer on the rear surface of the base material 11. Note that the rear surface of the base material 11 refers to the surface opposite to the surface on which the hard coating layer 12 is laminated.

[0055] When a roller is used when manufacturing the hard coating film 10, the thickness of the base material 11 is preferably less than or equal to 200 μm. When the thickness of the base material 11 is less than or equal to 200 μm, the hard coating film 10 during manufacturing and the hard coating film 10 after manufacturing will be easy to roll into a roll, thereby efficiently manufacturing the hard coating film 10. In addition, the base material 11 is ideally a thermoplastic base material.

[0056] For purposes such as improving adhesion, the base material 11 may be surface treated in advance. The surface treatment may include one or more treatments, such as corona treatment, plasma treatment, UV treatment, excimer treatment, and primer treatment. In order to improve adhesion, a surface treatment including the use of a silane coupling agent is particularly desirable. In addition, before forming the hard coating layer 12 on the base material 11, it is also preferred to remove dust and clean the surface of the base material 11 with a net cleaner or the like as needed.

[0057] [Hard coating 12]

[0058] The hard coating layer 12 is provided on the base material 11. The hard coating layer 12 may be, for example, a cured product of a resin composition. In certain embodiments, the resin composition contains a resin (A), a resin (B), an active energy ray polymerization initiator, and a solvent.

[0059] Resin (A) and resin (B) can be energy ray curable resins, such as ultraviolet curable resins, electron beam curable resins or infrared curable resins. Note that ultraviolet curable resins are preferably used as resin (A) and resin (B). This is because the need for post-treatment after curing is eliminated. For appropriate curing treatment, curing in a nitrogen atmosphere is ideal.

[0060] Resin (A) may be a multifunctional (meth) acrylic monomer having a weighted average functionality greater than or equal to 4. The weighted average functionality of resin (A) is preferably greater than 4.2 and less than 5.1. In the present embodiment, resin (A) contains, for example, a difunctional acrylic monomer and a hexafunctional acrylic monomer. Examples of difunctional acrylic monomers may include the product "SR833S" (difunctional tricyclodecane dimethanol diacrylate) and the product "SR306" (tripropylene glycol diacrylate), both of which are available from SARTOMER. Examples of hexafunctional acrylic monomers may include the product "DPHA" (dipentaerythritol hexaacrylate) available from DAICEL-ALLNEX LTD., and the like. Here, at least one of a trifunctional acrylic monomer, a tetrafunctional acrylic monomer, or a pentafunctional acrylic monomer may be used instead of or together with the difunctional acrylic monomer. Examples of trifunctional monomers may include "SR351" (trimethylolpropane triacrylate) or "SR454" (ethoxylated trimethylolpropane triacrylate), both available from SARTOMER. Examples of tetrafunctional monomers may include "SR295" (pentaerythritol tetraacrylate), "SR355" (di-trimethylolpropane tetraacrylate) or "SR494" (ethoxylated pentaerythritol tetraacrylate), both available from SARTOMER. Examples of pentafunctional monomers may include "SR399" (dipentaerythritol pentaacrylate) available from SARTOMER.

[0061] In certain embodiments, resin (B) is aliphatic urethane acrylate. Resin (B) is, for example, trifunctional aliphatic urethane acrylate, trifunctional aliphatic polyester urethane acrylate, etc. Commercially available specific examples of resin (B) can include product "CN989" (trifunctional aliphatic urethane acrylate) and product "CN929" (trifunctional aliphatic polyester urethane acrylate), both of which are available from SARTOMER, etc.

[0062] By making the hard coating layer 12 into a cured product of a resin composition containing a resin (A) which is a multifunctional (meth) acrylic monomer having a weighted average functionality greater than or equal to 4 as described above and a resin (B) which is an aliphatic polyurethane acrylate, the glass transition temperature Tg of the hard coating layer 12 can be greater than or equal to 50°C and less than or equal to 100°C. In addition, by similarly manufacturing the hard coating layer 12, the loss tangent tanδ of the hard coating layer 12 at the glass transition temperature Tg can be greater than or equal to 0.07 and less than or equal to 0.15. The loss tangent tanδ of the hard coating layer 12 at the above-mentioned glass transition temperature Tg is a value calculated by a dynamic viscoelasticity measurement method applying a 1-Hz frequency dynamic load. In addition, the loss tangent tanδ is the ratio between the storage modulus (E′) and the loss modulus (E") (tanδ=E" / E'). The storage modulus (E') is the component of the increase in internal energy when strain occurs in the object under study. The storage modulus (E') indicates the elastic properties of the object under study. The loss modulus (E") is the energy component lost when strain occurs in the object. The lost energy is the energy diffused to the outside of the object in the form of heat. The loss modulus (E") indicates the viscosity property of the object.

[0063] When the glass transition temperature Tg is less than 50°C, the hard coating layer 12 becomes soft in a high temperature environment such as a car interior or the like, and the scratch resistance of the hard coating layer 12 is significantly reduced. On the other hand, when the glass transition temperature Tg exceeds 100°C, the flexibility of the hard coating layer 12 cannot be ensured, which makes it difficult to repeatedly fold the hard coating layer 12 many times.

[0064] Therefore, the glass transition temperature Tg of the hard coating layer 12 is preferably set to be greater than or equal to 50° C. and less than or equal to 100° C. Accordingly, the scratch resistance of the hard coating layer 12 can be improved even in a high temperature environment such as in a car, and the hard coating layer 12 can be repeatedly folded more than or equal to one hundred thousand times.

[0065] When the loss tangent tanδ of the hard coating layer 12 at the glass transition temperature Tg is less than 0.07, the hardness of the hard coating layer 12 will become too high and the flexibility of the hard coating layer 12 will be reduced. On the other hand, when the loss tangent tanδ of the hard coating layer 12 at the glass transition temperature Tg is greater than 0.15, the hardness of the hard coating layer 12 will become too low and the scratch resistance of the hard coating layer 12 will be reduced.

[0066] Therefore, the loss tangent tanδ of the hard coating layer 12 at the glass transition temperature Tg is preferably set to be greater than or equal to 0.07 and less than or equal to 0.15. Accordingly, the scratch resistance of the hard coating layer 12 can be improved, and the hard coating layer 12 can also be repeatedly folded more than or equal to 100,000 times.

[0067] The content (mass %) of the resin (A) contained in the resin composition is preferably greater than twice the content (mass %) of the resin (B) and less than nine times the content (mass %) of the resin (B), more preferably greater than or equal to four times the content (mass %) of the resin (B) and less than nine times the content (mass %) of the resin (B), and still more preferably greater than or equal to four times the content (mass %) of the resin (B) and less than or equal to five times the content (mass %) of the resin (B). The content of the resin (A) contained in the resin composition is preferably greater than or equal to 20% by mass and less than or equal to 40% by mass, more preferably greater than or equal to 26% by mass and less than or equal to 33% by mass. The content of the resin (B) contained in the resin composition is preferably greater than or equal to 2% by mass and less than or equal to 15% by mass, more preferably greater than or equal to 4.5% by mass and less than or equal to 11.5% by mass.

[0068] In certain embodiments, the active energy ray polymerization initiator is a Norrish I type photoinitiator or a Norrish II type photoinitiator. Specific commercial examples of active energy ray polymerization initiators can include products "OMNIRAD 184 (IRGACURE 184)" (1-hydroxycyclohexyl-phenyl ketone), "OMNIRAD 500 (IRGACURE 500)" (a mixture of benzophenone and 1-hydroxycyclohexyl-phenyl ketone), and "OMNIRAD TPO" (2,4,6-trimethylbenzoyl-diphenylphosphine oxide), all of which are available from IGM RESINS (formerly BASF).

[0069] Solvent is not particularly limited, as long as the coating performance of resin combination is met, and preferably considers safety to select solvent.In certain embodiments, solvent contains one or more selected from following: for example alcohol solvent such as ethanol, n-propyl alcohol, isopropanol, n-butyl alcohol, isobutyl alcohol and diacetone alcohol, ketone solvent such as acetone, methyl ethyl ketone (hereinafter referred to as MEK), methyl isobutyl ketone and cyclohexanone, ester solvent such as methyl acetate, butyl acetate, propylene glycol monomethyl ether acetate (hereinafter referred to as PGMEA), ether solvent such as propylene glycol monomethyl ether (hereinafter referred to as PGME), ether and diisopropyl ether etc.Solvent preferably contains any one of MEK, PGME and PGMEA.Particularly preferably use any one or both in PGME and PGMEA, so as to improve the coating performance of resin combination.

[0070] For example, the thickness of the hard coating layer 12 is preferably greater than or equal to 3 μm, more preferably greater than or equal to 5 μm. When the thickness of the hard coating layer 12 is greater than or equal to 3 μm, sufficient hardness will be obtained so that the hard coating layer 12 is less likely to be scratched during the manufacturing process. In addition, the thickness of the hard coating layer 12 is preferably less than or equal to 15 μm, more preferably less than or equal to 10 μm. When the thickness of the hard coating layer 12 is less than or equal to 15 μm, microcracks that may occur when the hard coating film 10 is bent during manufacturing are less likely to be generated in the hard coating layer 12, resulting in good productivity of the hard coating film 10.

[0071] The metal oxide nanoparticles may be contained in a dispersed manner in the resin composition of the hard coat layer 12. When the resin composition contains the metal oxide nanoparticles, the hardness of the hard coat layer 12 may be increased.

[0072] For example, the average particle size of the metal oxide nanoparticles is preferably less than or equal to 100 nm, more preferably less than or equal to 50 nm. Note that in the present embodiment, the average particle size refers to a value measured by the BET method.

[0073] When the average particle size of the metal oxide nanoparticles is greater than 100nm, the transmittance of the hard coat 12 in the visible light range may be reduced. Therefore, by setting the average particle size of the metal oxide nanoparticles to be less than or equal to 100nm, the transmittance of the hard coat 12 in the visible light range can be maintained. By setting the average particle size of the metal oxide nanoparticles to be less than or equal to 50nm, these advantages can be further exerted. When the base material 11 is an opaque base material, since the hard coat 12 may not have a high transmittance, the average particle size of the metal oxide nanoparticles may be greater than 100nm.

[0074] The content of the metal oxide nanoparticles (excluding monomers) in the resin composition is preferably greater than or equal to 2 mass % of the total solid content of the resin composition of the hard coating layer 12 and less than or equal to 5 mass % of the total solid content of the resin composition of the hard coating layer 12. When the content of the metal oxide nanoparticles is greater than 5 mass %, the hard coating layer 12 tends to become brittle. Therefore, by setting the content of the metal oxide nanoparticles according to the present embodiment within the above range, the flexibility of the hard coating layer 12 can be maintained. The solid content of the resin composition refers to the total content excluding the solvent, and the liquid monomer content is also included in the solid content.

[0075] In certain embodiments, the metal oxide constituting the metal oxide nanoparticles is either or both of SiO2 (silicon dioxide) and Al2O3 (aluminum oxide). This can prevent the light transmittance of the hard coating layer 12 from being reduced in the visible light range.

[0076] The Mohs hardness of the metal oxide nanoparticles is preferably greater than 6. This can increase the hardness of the hard coating layer 12 without reducing the flexibility of the hard coating layer 12 .

[0077] [Antifouling layer 13]

[0078] In certain embodiments of the present invention, the antifouling layer 13 may be provided as a part of the hard coating layer 12 . Figure 2 1 is a cross-sectional view showing a hard coating film 10 according to a specific embodiment. Figure 2 As shown in , the fluorine compound contained in the hard coating layer 12 segregates to the first region 12a located on the surface side of the hard coating layer 12 to form an antifouling layer 13. In the second region 12b located on the base material 11 side of the hard coating layer 12, the fluorine compound is not segregated. In other words, the amount of fluorine compound in the second region 12b is less than the amount of fluorine compound in the first region 12a. The second region 12b may contain fluorine compounds. The fluorine compound may be dispersed (discrete) in the second region 12b. The thickness Ta of the first region 12a is, for example, at most 10% of the total thickness T of the hard coating layer 12. The second region 12b is an area other than the first region 12a in the hard coating layer 12. As used herein, the term "segregation" means that during the curing of the resin composition, the distribution of the fluorine compound in the resin composition becomes larger on the surface side of the hard coating layer 12 than on the base material 11 side. The antifouling layer 13 will prevent the hard coating layer 12 from being contaminated. The antifouling layer 13 may or may not form a clear layer, depending on the segregation state of the fluorine compound.

[0079] The antifouling layer 13 contains a fluorine compound. The fluorine compound preferably has a (methyl) acryloyl group. In addition, from the perspective of environmental regulations, the fluorine compound is preferably a perfluoropolyether derivative rather than a fluoroalkyl derivative. The fluorine compound can be a hybrid material of an organic material and an inorganic material. The example of the hybrid material can include fluorinated silsesquioxane. In the present embodiment, because the antifouling layer 13 contains a fluorine compound, the antifouling performance and chemical resistance of the hard coating film 10 can be improved. Chemical resistance is resistance to, for example, acids, alkalis, solvents and oils.

[0080] Examples of the fluorine compound contained in the antifouling layer 13 may include product "KY-1203" available from SHIN-ETSU CHEMICAL CO., LTD., product "OPTOOL DAC-HP" available from DAIKIN INDUSTRIES, LTD., product "FLUOROLINK AD1700" available from SOLVAY SPECIALTY POLYMERS, product "CN4000" available from SARTOMER, and the like.

[0081] [2. Properties of the hard coating layer 12]

[0082] Next, the properties of the hard coat layer 12 according to the present embodiment will be described. The hard coat layer 12 according to the present embodiment has, for example, at least one of the following properties (I) to (IV).

[0083] (I) Glass transition temperature Tg and loss tangent tanδ

[0084] The hard coating layer 12 has a glass transition temperature Tg of 50° C. or more and 100° C. or less, preferably 60° C. or more and 90° C. or less. The loss tangent tan δ is 0.07 or more and 0.15 or less, preferably 0.09 or more and 0.13 or less.

[0085] Accordingly, even in a high temperature environment such as inside a vehicle or the like, the scratch resistance and abrasion resistance of the hard coating layer 12 can be improved, and the hard coating layer 12 can be repeatedly folded a plurality of times greater than or equal to one hundred thousand times.

[0086] The glass transition temperature Tg and the loss tangent tan δ can be measured using, for example, a dynamic mechanical analyzer DMA7100 available from HITACHI HIGH-TECHSCIENCE CORPORATION.

[0087] The measurement conditions of the dynamic viscoelasticity measurement method when calculating the glass transition temperature Tg and the loss tangent tan δ are as follows.

[0088] Frequency of induced sine wave vibration: 1Hz

[0089] Sample size: 20mm long x 4.4mm wide x 0.10mm thick

[0090] Test method: Raise the temperature from 20°C to 200°C at a rate of 10°C / min

[0091] (II) Number of folds

[0092] The hard coating film 10 is configured to be folded at least 100,000 times by bending inward or outward without causing any cracking, interlayer separation or loss of optical properties. In this article, the optical properties mentioned include changes in total transmittance (%), transmission haze, glossiness or chromaticity b* (intensity of hue from blue to yellow). Even when the flexible display device covered by the hard coating film 10 is repeatedly folded hundreds of thousands of times, the above configuration can prevent the hard coating film 10 from separating from the flexible display device.

[0093] The number of folding times (number of bending times) can be measured using, for example, a folding tester available from YUASA SYSTEM CO., LTD. (mandrel diameter: 3 mm, bending radius: 1.5 mm).

[0094] (III) Water contact angle (WCA)

[0095] The water contact angle is an angle formed by the surface of a water droplet and the surface of the hard coating layer 12 when the water droplet contacts the surface of the hard coating layer 12. The water contact angle was measured before and after the abrasion test was performed.

[0096] The wear test was conducted using a wear tester by using steel wool #0000, and the surface of the hard coating layer 12 was worn with the steel wool under the conditions of a load of 1000 g, a speed of 50 mm / sec, a reciprocating distance of 40 mm, and 2500 reciprocations.

[0097] Before the wear test (before wear), the water contact angle θ1 of the surface of the hard coating 12 is preferably greater than 110° and less than 120°. After the wear test (after wear), the water contact angle θ2 of the surface of the hard coating 12 is preferably greater than 100° and less than the water contact angle θ1.

[0098] The reduction in the water contact angle of the surface of the hard coating 12 before and after wear is preferably less than 13%, more preferably less than or equal to 7.6%. Having a small reduction in the water contact angle means that even if the hard coating 12 is subjected to a wear test, the hard coating 12 is hardly scraped off, that is, the wear resistance is excellent. In this context, the reduction in the water contact angle can be obtained by the following formula:

[0099] (Water contact angle before wear test - water contact angle after wear test) / water contact angle before wear test×100.

[0100] The water contact angle can be measured, for example, using an automatic contact angle meter DM-501Hi available from KYOWA INTERFACE SCIENCE CO., LTD.

[0101] (IV) Visible scratches

[0102] After the hard coating layer 12 according to the present embodiment was subjected to the above-mentioned abrasion test, no visible scratches were found in the hard coating layer 12. In other words, it is understood that in the hard coating film 10 according to the present embodiment, the hard coating layer 12 is less likely to be scratched and has excellent scratch resistance.

[0103] [3. Apparatus for producing the hard coating film 10]

[0104] Figure 4 Schematic diagram showing a film manufacturing apparatus 100 according to this embodiment. Figure 4 As shown in FIG. 1 , the film manufacturing apparatus 100 includes a delivery roller 110, a winding roller 112, guide rollers 114a to 114d, a coating device 120, a drying device 130, and a curing device 140. Figure 4 In , the solid arrow indicates the direction of roller rotation. Figure 4, the dotted arrow indicates the direction in which the base material 11 is conveyed.

[0105] The base material 11 in the form of a strip is wound into a roll shape around a delivery roller 110. The delivery roller 110 is arranged so that the base material 11 can be continuously delivered by means of a guide roller 114a or the like.

[0106] The take-up roller 112 is arranged so that the hard coating film 10 in the form of a strip manufactured by the film manufacturing apparatus 100 can be taken up.

[0107] The guide rollers 114a to 114d are arranged on the conveying path in the film manufacturing apparatus 100 so that the base material 11 in the form of a strip and the hard coating film 10 in the form of a strip can be conveyed. The material of the guide rollers 114a to 114b is selected as appropriate according to the required roller characteristics. The material of the guide rollers 114a to 114b is metal such as stainless steel, rubber, silicone resin, etc.

[0108] The coating device 120 is disposed between the guide rollers 114a and 114b. The coating device 120 laminates (eg, applies) the resin composition on the base material 11. The coating device 120 is, for example, a gravure coater, a wire bar coater, a die coater, or the like.

[0109] The drying device 130 is disposed between the guide roller 114b and the guide roller 114c. The drying device 130 heats the base material 11 to which the resin composition has been applied, thereby drying the resin composition. The drying device 130 evaporates the solvent contained in the resin composition. This allows the solvent to be removed from the resin composition.

[0110] The curing device 140 is disposed between the guide roller 114c and the guide roller 114d. The curing device 140 includes guide rollers 144, 146 and a light source 148 for irradiating the resin composition with energy rays. Examples of energy rays include electron beams, ultraviolet rays, visible rays, gamma rays, etc. The guide rollers 144 and 146 are in contact with the rear surface of the base material 11 to which the resin composition has been applied, thereby delivering the base material 11 toward the guide roller 114d.

[0111] Next, a method for manufacturing a hard coating film 10 using the film manufacturing apparatus 100 will be described. First, a base material 11 is delivered from a delivery roller 110. The delivered base material 11 passes under a coating device 120 through a guide roller 114a. The coating device 120 applies a resin composition to the base material 11 passing under the coating device 120. The base material 11 to which the resin composition has been applied is conveyed to a drying device 130 through a guide roller 114b. The drying device 130 dries the resin composition applied to the base material 11.

[0112] The base material 11 on which the dried resin composition is laminated is conveyed to the curing device 140 by the guide roller 114c, and the resin composition is irradiated with energy rays from the light source 148. The resin composition is thereby cured, and a hard coating film 10 having the hard coating layer 12 laminated on the base material 11 is manufactured.

[0113] The hard coating film 10 thus manufactured is wound around the winding roll 112 via the guide rolls 146 and 114 d .

[0114] Note that the resin composition preferably contains a fluorine compound. Accordingly, when the solvent is evaporated by the drying device 130, the fluorine compound will be made to float above the resin composition as the solvent dries and rises, so that the antifouling layer 13 can be formed.

[0115] Note that the antifouling layer 13 can be obtained by laminating a layer containing a fluorine compound separately after forming the hard coating layer 12 . Figure 3 1 is a cross-sectional view showing a hard coating film 10 according to a specific embodiment. Figure 3 As shown in , the antifouling layer 13 may be a layer separate from the hard coating layer 12. In this case, the antifouling layer 13 is formed on the hard coating layer 12. In the case of forming the antifouling layer 13 in a separate step, a method such as coating, vapor deposition, or sputtering may be used. In the case of using a coating method, an apparatus similar to the film manufacturing apparatus 100 may be used. Therefore, the antifouling layer 13 may be a part of the hard coating layer 12 or a layer different from the hard coating layer 12.

[0116] [Example]

[0117] Hereinafter, examples of the present invention and comparative examples will be specifically described, the examples to be described below are merely illustrative, and the hard coating film according to the present invention is not limited to the following examples.

[0118] Examples 1 to 13 and Comparative Examples 1 to 8 were produced as hard coating layers and antifouling layers. When producing hard coating layers and antifouling layers, resin compositions each containing a resin (A), a resin (B), an active energy ray polymerization initiator, a solvent and a fluorine compound were prepared. The formulas of the resin compositions of Examples 1 to 5 are shown in Table 1 below. The formulas of the resin compositions of Examples 6 to 10 are shown in Table 2 below. The formulas of the resin compositions of Examples 11 to 13 are shown in Table 3 below. The formulas of the resin compositions of Comparative Examples 1 to 5 are shown in Table 4 below. The formulas of the resin compositions of Comparative Examples 6 to 8 are shown in Table 5 below. Note that the units of the blending ratios in Tables 1 to 5 are in mass %.

[0119] The glass transition temperature Tg, the loss tangent tanδ (tan Delta, peak value) at the glass transition temperature Tg, the number of folding times, the water contact angle (WCA) before and after the abrasion test, and visible scratches of the hard coating films according to Examples 1 to 13 and Comparative Examples 1 to 8 were measured.

[0120] The glass transition temperature Tg and the loss tangent tan δ at the glass transition temperature Tg were measured using a dynamic mechanical analyzer DMA7100 available from HITACHI HIGH-TECH SCIENCE CORPORATION. The measurement conditions of the dynamic viscoelasticity measurement method when calculating the loss tangent tan δ are similar to those in the above-described embodiment.

[0121] The number of folding times was measured using a folding test device (mandrel diameter: 3 mm, bending radius: 1.5 mm) available from YUASA SYSTEM CO., LTD. In Tables 1 to 5, the evaluation of the folding test results is indicated on a scale of 1 to 3. In Tables 1 to 5, a rating of "3" indicates an excellent rating that does not change even after two hundred thousand (200K) foldings. In Tables 1 to 5, a rating of "2" indicates an acceptable rating that does not change even after one hundred thousand (100K) foldings. In Tables 1 to 5, a rating of "1" indicates a poor rating that changes occurred before 100K foldings.

[0122] The water contact angle was measured with 2.0 μL of pure water dropped on the surface of the hard coating film according to each experimental example before and after abrasion using steel wool with an abrasion tester. The surface of the hard coating film was abraded under the conditions of a load of 1000 g, a speed of 50 mm / sec, a reciprocating distance of 40 mm, and 2500 reciprocations. In addition, the average value of the water contact angle measured ten times at the center of the worn portion was calculated. The water contact angles shown in Tables 1 to 5 below are average values. For example, the automatic contact angle meter DM-501Hi available from KYOWAINTERFACE SCIENCE CO., LTD. is used to measure the water contact angle.

[0123] After the above-described abrasion test was performed, it was visually checked whether scratches occurred in the surface of the hard coating film according to each Experimental Example.

[0124] [Table 1]

[0125]

[0126] *Folding performance rating:

[0127] 3 = Excellent (no change after 200K folds)

[0128] 2 = Acceptable (no change after 100K folds)

[0129] 1 = Bad (changed before 100K folds)

[0130] [Example 1]

[0131] As shown in Table 1, the resin composition of Example 1 contains 5.64 mass % of "SR833S" available from SARTOMER and 22.56 mass % of "DPHA" available from DAICEL-ALLNEX LTD. as resin (A), 9.4 mass % of "CN989" available from SARTOMER as resin (B), 5.64 mass % of "OMNIRAD 500" available from IGM RESINS and 1.41 mass % of "OMNIRAD TPO" available from IGM RESINS as active energy ray polymerization initiators, 46.984 mass % of "PGME" available from SIGMA-ALDRICH as a solvent, 7.52 mass % of "AL2260" available from NANOPHASE TECHNOLOGIES CORPORATION as metal oxide nanoparticles and 0.846 mass % of "KY-1203" available from SHIN-ETSU CHEMICAL. CO., LTD. as a fluorine compound.

[0132] Herein, "AL2260" contains 30% by mass of alumina particles and 70% by mass of a difunctional monomer (TPGDA). Therefore, the content of the difunctional monomer is reflected in the "weighted average functionality", and the content ratio between the resin (A) and the resin (B) of Examples 1 to 13 and Comparative Examples 1 to 8 (hereinafter referred to as "A / B") is shown in Tables 1 to 5.

[0133] In Example 1, the weighted average functionality of resin (A) was 4.70, and A / B was 3.56.

[0134] In Example 1, the glass transition temperature Tg was 60.4° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1046.

[0135] In the folding test of Example 1, there was no change even after 200K foldings of the hard coat film (rating "3"). In Example 1, the water contact angle before the abrasion test was 114.7°, and the water contact angle after the abrasion test was 106°. No visible scratches were found.

[0136] [Example 2]

[0137] As shown in Table 1, the resin composition of Example 2 contains 7.52 mass % of "SR833S" and 22.56 mass % of "DPHA" as resin (A) and 7.52 mass % of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 2 are similar to those of Example 1.

[0138] In Example 2, the weighted average functionality of resin (A) was 4.55, and A / B was 4.70.

[0139] In Example 2, the glass transition temperature Tg was 54.4° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1126.

[0140] In the folding test of Example 2, there was no change even after 200K foldings of the hard coating film. In Example 2, the water contact angle before the abrasion test was 115.2°, and the water contact angle after the abrasion test was 100.8°. No visible scratches were found.

[0141] [Example 3]

[0142] As shown in Table 1, the resin composition of Example 3 contains 7.52 mass % of "SR833S" and 18.8 mass % of "DPHA" as resin (A) and 11.28 mass % of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 3 are similar to those of Example 1.

[0143] In Example 3, the weighted average functionality of resin (A) was 4.38, and A / B was 2.80.

[0144] In Example 3, the glass transition temperature Tg is 68.5° C. The loss tangent tan δ at the glass transition temperature Tg is 0.1246.

[0145] In the folding test of Example 3, there was no change even after the hard coat film was folded 200K times. In Example 3, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 105.1°. No visible scratches were found.

[0146] As shown in Table 1, the resin composition of Example 4 contains 9.4% by mass of "SR833S" and 20.68% by mass of "DPHA" as resin (A) and 7.52% by mass of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 4 are similar to those of Example 1.

[0147] In Example 4, the weighted average functionality of resin (A) was 4.34, and A / B was 4.70.

[0148] In Example 4, the glass transition temperature Tg was 68.5° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1274.

[0149] In the folding test of Example 4, there was no change even after the hard coat film was folded 200K times. In Example 4, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 106.7°. No visible scratches were found.

[0150] [Example 5]

[0151] As shown in Table 1, the resin composition of Example 5 contains 5.64 mass % of "SR833S" and 24.44 mass % of "DPHA" as resin (A) and 7.52 mass % of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 5 are similar to those of Example 1.

[0152] In Example 5, the weighted average functionality of resin (A) was 4.77, and A / B was 4.70.

[0153] In Example 5, the glass transition temperature Tg was 76.8° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1017.

[0154] In the folding test of Example 5, there was no change even after the hard coat film was folded 200K times. In Example 5, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 106.5°. No visible scratches were found.

[0155] [Table 2]

[0156]

[0157] *Folding performance rating:

[0158] 3 = Excellent (no change after 200K folds)

[0159] 2 = Acceptable (no change after 100K folds)

[0160] 1 = Bad (changed before 100K folds)

[0161] [Example 6]

[0162] As shown in Table 2, the resin composition of Example 6 contains 9.4% by mass of "SR833S" and 18.8% by mass of "DPHA" as resin (A) and 9.4% by mass of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 6 are similar to those of Example 1.

[0163] In Example 6, the weighted average functionality of resin (A) was 4.25, and A / B was 3.56.

[0164] In Example 6, the glass transition temperature Tg was 73.4° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1125.

[0165] In the folding test of Example 6, there was no change even after the hard coat film was folded 200K times. In Example 6, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 107.3°. No visible scratches were found.

[0166] [Example 7]

[0167] As shown in Table 2, the resin composition of Example 7 contains 5.64 mass % of "SR833S" and 20.68 mass % of "DPHA" as resin (A) and 11.28 mass % of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 7 are similar to those of Example 1.

[0168] In Example 7, the weighted average functionality of resin (A) was 4.62, and A / B was 2.80.

[0169] In Example 7, the glass transition temperature Tg was 50.6° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1152.

[0170] In the folding test of Example 7, there was no change even after the hard coat film was folded 200K times. In Example 7, the water contact angle before the abrasion test was 113.2°, and the water contact angle after the abrasion test was 102.3°. No visible scratches were found.

[0171] [Example 8]

[0172] As shown in Table 2, the resin composition of Example 8 contains 4.7% by mass of "SR833S" and 25.38% by mass of "DPHA" as resin (A) and 7.52% by mass of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 8 are similar to those of Example 1.

[0173] In Example 8, the weighted average functionality of resin (A) was 4.87, and A / B was 4.70.

[0174] In Example 8, the glass transition temperature Tg was 58.3° C. The loss tangent tan δ at the glass transition temperature Tg was 0.0912.

[0175] In the folding test of Example 8, there was no change even after the hard coat film was folded 200K times. In Example 8, the water contact angle before the abrasion test was 114.5°, and the water contact angle after the abrasion test was 105.6°. No visible scratches were found.

[0176] [Example 9]

[0177] As shown in Table 2, the resin composition of Example 9 contains 3.76 mass % of "SR833S" and 26.32 mass % of "DPHA" as resin (A) and 7.52 mass % of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 9 are similar to those of Example 1.

[0178] In Example 9, the weighted average functionality of resin (A) was 4.98, and A / B was 4.70.

[0179] In Example 9, the glass transition temperature Tg was 91.7° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1003.

[0180] In the folding test of Example 9, there was no change even after the hard coat film was folded 200K times. In Example 9, the water contact angle before the abrasion test was 115.8°, and the water contact angle after the abrasion test was 107.1°. No visible scratches were found.

[0181] [Example 10]

[0182] As shown in Table 2, the resin composition of Example 10 contains 2.82 mass % of "SR833S" and 27.26 mass % of "DPHA" as resin (A) and 7.52 mass % of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 10 are similar to those of Example 1.

[0183] In Example 10, the weighted average functionality of resin (A) was 5.09, and A / B was 4.70.

[0184] In Example 10, the glass transition temperature Tg was 85.3° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1007.

[0185] In the folding test of Example 10, there was no change even after 200K foldings of the hard coat film. In Example 10, the water contact angle before the abrasion test was 116.1°, and the water contact angle after the abrasion test was 109.6°. No visible scratches were found.

[0186] [Table 3]

[0187]

[0188] *Folding performance rating:

[0189] 3 = Excellent (no change after 200K folds)

[0190] 2 = Acceptable (no change after 100K folds)

[0191] 1 = Bad (changed before 100K folds)

[0192] [Example 11]

[0193] As shown in Table 3, the resin composition of Example 11 contains 5.64 mass % of "SR833S" and 27.26 mass % of "DPHA" as resin (A) and 4.7 mass % of "CN989" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Example 11 are similar to those of Example 1.

[0194] In Example 11, the weighted average functionality of resin (A) was 4.86, and A / B was 8.12.

[0195] In Example 11, the glass transition temperature Tg was 58.3° C. The loss tangent tan δ at the glass transition temperature Tg was 0.0912.

[0196] In the folding test of Example 11, there was no change even after 200K foldings of the hard coating film. In Example 11, the water contact angle before the abrasion test was 116.7°, and the water contact angle after the abrasion test was 110.2°. No visible scratches were found.

[0197] [Example 12]

[0198] As shown in Table 3, the resin composition of Example 12 contains 8.064 mass % of "SR833S" and 24.192 mass % of "DPHA" as resin (A), 8.064 mass % of "CN929" available from SARTOMER as resin (B), 1.613 mass % of "OMNIRAD 184" available from IGM RESINS as an active energy ray polymerization initiator, 49.693 mass % of "PGME" as a solvent, 8.064 mass % of "AL2260" as metal oxide nanoparticles and 0.31 mass % of "KY-1203" as a fluorine compound.

[0199] In Example 12, the weighted average functionality of resin (A) was 4.55, and A / B was 4.70.

[0200] In Example 12, the glass transition temperature Tg was 69.4° C. The loss tangent tan δ at the glass transition temperature Tg was 0.09.

[0201] In the folding test of Example 12, there was no change even after 250K or more folding of the hard coating film. In Example 12, the water contact angle before the abrasion test was 115.3°, and the water contact angle after the abrasion test was 107.7°. No visible scratches were found.

[0202] [Example 13]

[0203] As shown in Table 3, the resin composition of Example 13 contains 8.014 mass % of "SR833S" and 22.04 mass % of "DPHA" as resin (A), 10.02 mass % of "CN989" as resin (B), 1.603 mass % of "OMNIRAD184" as an active energy ray polymerization initiator, 50 mass % of "PGME" as a solvent, 8.014 mass % of "AL2260" as metal oxide nanoparticles and 0.31 mass % of "KY-1203" as a fluorine compound.

[0204] In Example 13, the weighted average functionality of resin (A) was 4.47, and A / B was 3.56.

[0205] In Example 13, the glass transition temperature Tg was 80° C. The loss tangent tan δ at the glass transition temperature Tg was 0.099.

[0206] In the folding test of Example 13, there was no change even after 250K or more foldings of the hard coating film. In Example 13, the water contact angle before the abrasion test was 114.9°, and the water contact angle after the abrasion test was 105.9°. No visible scratches were found.

[0207] As described above, in Examples 1 to 13, the weighted average functionality of the resin (A) is greater than or equal to 4. Therefore, the glass transition temperature Tg of Examples 1 to 13 is in the range of greater than or equal to 50°C and less than or equal to 100°C, and the loss tangent tanδ at the glass transition temperature Tg is in the range of greater than or equal to 0.07 and less than or equal to 0.15. Therefore, it is speculated that the number of folding times of Examples 1 to 13 is greater than or equal to 200K. It is also speculated that in Examples 1 to 13, the water contact angle before the wear test is greater than 110°, and the water contact angle after the wear test is greater than 100°. It is also speculated that in Examples 1 to 13, the reduction in the water contact angle after the wear test relative to the water contact angle before the wear test is less than 13%. It is also seen that no visible scratches are found in Examples 1 to 13. In other words, it is confirmed that Examples 1 to 13 have the performance of being able to withstand multiple and repeated foldings, and improved scratch resistance and wear resistance are achieved even in a high temperature environment such as in a car or the like.

[0208] [Table 4]

[0209]

[0210]

[0211] *Folding performance rating:

[0212] 3 = Excellent (no change after 200K folds)

[0213] 2 = Acceptable (no change after 100K folds)

[0214] 1 = Bad (changed before 100K folds)

[0215] [Comparative Example 1]

[0216] As shown in Table 4, the resin composition of Comparative Example 1 contained 7.515 mass % of "SR833S", 5.01 mass % of "SR306 (TPGDA)" available from SARTOMER and 9.018 mass % of "DPHA" as resin (A), 16.032 mass % of "CN929" as resin (B), 2.004 mass % of "OMNIRAD 184" as an active energy ray polymerization initiator, 50.09 mass % of "PGME" as a solvent, 10.02 mass % of "AL2460" available from NANOPHASE TECHNOLOGIES CORPORATION as metal oxide nanoparticles, and 0.31 mass % of "KY-1203" as a fluorine compound.

[0217] In Comparative Example 1, the weighted average functionality of the resin (A) was 2.77, and A / B was 1.78.

[0218] In Comparative Example 1, the glass transition temperature Tg was 59.5° C. The loss tangent tan δ at the glass transition temperature Tg was 0.1516.

[0219] In the folding test of Comparative Example 1, there was no change even after 250K or more foldings of the film. The water contact angle before the abrasion test was 115°, and the water contact angle after the abrasion test was 106°. On the other hand, visible scratches were found.

[0220] As described above, in Comparative Example 1, the weighted average functionality of the resin (A) contained in the resin composition is 2.77. Therefore, the loss tangent tanδ at the glass transition temperature Tg of Comparative Example 1 is as high as 0.1516, which means that the flexibility of the film is slightly reduced. Therefore, it is presumed that this is the reason why visible scratches are observed in Comparative Example 1.

[0221] [Comparative Example 2]

[0222] As shown in Table 4, the resin composition of Comparative Example 2 contains 16.65% by mass of "SR444" available from SARTOMER as resin (A), 30.91% by mass of "PU610" available from M1WONSPECIALTY CHEMICAL as resin (B), 2.37% by mass of "OMNIRAD 184" as an active energy ray polymerization initiator, 49.76% by mass of "PGME" as a solvent, and 0.31% by mass of "KY-1203" as a fluorine compound. Note that the resin composition of Comparative Example 2 does not contain metal oxide nanoparticles. In addition, "SR 444" is a monomer mainly composed of a trifunctional group and containing a tetrafunctional group.

[0223] In Comparative Example 2, the weighted average functionality of the resin (A) was 3.00, and A / B was 0.54.

[0224] In Comparative Example 2, the glass transition temperature Tg was 100° C. The loss tangent tan δ at the glass transition temperature Tg was 0.055.

[0225] In the folding test of Comparative Example 2, the sample was cracked during the process of folding the film 100 times. In Comparative Example 2, the water contact angle before the wear test was 110°, and the water contact angle after the wear test was 95°. No visible scratches were found.

[0226] As described above, in Comparative Example 2, the weighted average functionality of the resin (A) contained in the resin composition is 3.00. Therefore, the loss tangent tanδ of Comparative Example 2 at the glass transition temperature Tg is as low as 0.055, and the hardness of the film is too high. It is speculated that this is the reason why the number of foldings in Comparative Example 2 is less than or equal to 100. In general, it is believed that in Comparative Example 2, since the scratch resistance is improved due to the increase in crosslinking density, no scratches are found, but since the excessive increase in crosslinking density leads to a loss of flexibility, no good results are obtained in the folding test.

[0227] [Comparative Example 3]

[0228] As shown in Table 4, the resin composition of Comparative Example 3 contains 7.35 mass % of "SR444" and 24.51 mass % of "IBOA (SR506-A)" available from SARTOMER as resin (A), 9.81 mass % of "CN9047" available from SARTOMER as resin (B), 0.98 mass % of "OMNIRAD 184" as an active energy ray polymerization initiator, 49.75 mass % of "PGME" as a solvent, 7.35 mass % of "AL2260" as metal oxide nanoparticles, and 0.25 mass % of "KY-1203" as a fluorine compound. Herein, "IBOA (SR506-A)" is a monofunctional monomer.

[0229] In Comparative Example 3, the weighted average functionality of the resin (A) was 1.54, and A / B was 3.77.

[0230] In Comparative Example 3, the glass transition temperature Tg was 129.6° C. The loss tangent tan δ at the glass transition temperature Tg was 0.25.

[0231] In the folding test of Comparative Example 3, there was no change even after 200K foldings of the film. However, in Comparative Example 3, the water contact angle before the wear test was 113.4°, and the water contact angle after the wear test was 87.3°. Visible scratches were found.

[0232] As described above, in Comparative Example 3, the weighted average functionality of the resin (A) contained in the resin composition is 1.54. Therefore, the glass transition temperature Tg of Comparative Example 3 is as high as 129.6°C. The loss tangent tanδ of Comparative Example 3 at the glass transition temperature Tg is as high as 0.25. In other words, it is presumed that since Comparative Example 3 has a high tanδ and a low crosslinking density and is soft, it shows good results in the folding test, however, since the hardness is too low, visible scratches are found after the wear test.

[0233] [Comparative Example 4]

[0234] As shown in Table 4, the resin composition of Comparative Example 4 contains 7.35 mass % of "SR444" and 22.06 mass % of "IBOA (SR506-A)" as resin (A) and 12.26 mass % of "CN9047" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Comparative Example 4 are similar to those of Comparative Example 3.

[0235] In Comparative Example 4, the weighted average functionality of the resin (A) was 1.57, and A / B was 2.82.

[0236] In Comparative Example 4, the glass transition temperature Tg was 117.8° C. The loss tangent tan δ at the glass transition temperature Tg was 0.208.

[0237] In the folding test of Comparative Example 4, there was no change even after 200K foldings of the film. However, in Comparative Example 4, the water contact angle before the wear test was 113.7°, and the water contact angle after the wear test was 73.9°. Visible scratches were found.

[0238] As described above, in Comparative Example 4, the weighted average functionality of the resin (A) contained in the resin composition is 1.57. Therefore, the glass transition temperature Tg of Comparative Example 4 is as high as 117.8°C. The loss tangent tanδ of Comparative Example 4 at the glass transition temperature Tg is as high as 0.208. In other words, it is presumed that since Comparative Example 4 has a high tanδ and a low crosslinking density and is soft, it shows good results in the folding test, however, since the hardness is too low, visible scratches are found after the wear test.

[0239] [Comparative Example 5]

[0240] As shown in Table 4, the resin composition of Comparative Example 5 contains 7.35 mass % of "SR444" and 19.61 mass % of "IBOA (SR506-A)" as resin (A) and 14.71 mass % of "CN9047" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Comparative Example 5 are similar to those of Comparative Example 3.

[0241] In Comparative Example 5, the weighted average functionality of the resin (A) was 1.62, and A / B was 2.18.

[0242] In Comparative Example 5, the glass transition temperature Tg was 106.3° C. The loss tangent tan δ at the glass transition temperature Tg was 0.194.

[0243] In the folding test of Comparative Example 5, there was no change even after 200K foldings of the film. However, in Comparative Example 5, the water contact angle before the wear test was 114.1°, and the water contact angle after the wear test was 76.1°. Visible scratches were found.

[0244] As described above, in Comparative Example 5, the weighted average functionality of the resin (A) contained in the resin composition is 1.62. Therefore, the glass transition temperature Tg of Comparative Example 5 is as high as 106.3°C. The loss tangent tanδ of Comparative Example 5 at the glass transition temperature Tg is as high as 0.194. In other words, it is presumed that since Comparative Example 5 has a high tanδ and a low crosslinking density and is soft, it shows good results in the folding test, however, since the hardness is too low, visible scratches are found after the wear test.

[0245] [Table 5]

[0246]

[0247] *Folding performance rating:

[0248] 3 = Excellent (no change after 200K folds)

[0249] 2 = Acceptable (no change after 100K folds)

[0250] 1 = Bad (changed before 100K folds)

[0251] [Comparative Example 6]

[0252] As shown in Table 5, the resin composition of Comparative Example 6 contains 4.9 mass % of "SR444" and 24.51 mass % of "IBOA (SR506-A)" as resin (A) and 12.26 mass % of "CN9047" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Comparative Example 6 are similar to those of Comparative Example 3.

[0253] In Comparative Example 6, the weighted average functionality of the resin (A) was 1.43, and A / B was 2.82.

[0254] In Comparative Example 6, the glass transition temperature Tg was 111.9° C. The loss tangent tan δ at the glass transition temperature Tg was 0.2791.

[0255] In the folding test of Comparative Example 6, there was no change even after 200K foldings of the film. However, in Comparative Example 6, the water contact angle before the wear test was 113.5°, and the water contact angle after the wear test was 77.4°. Visible scratches were found.

[0256] As described above, in Comparative Example 6, the weighted average functionality of the resin (A) contained in the resin composition is 1.43. Therefore, the glass transition temperature Tg of Comparative Example 6 is as high as 111.9°C. The loss tangent tanδ of Comparative Example 6 at the glass transition temperature Tg is as high as 0.2791. In other words, it is presumed that since Comparative Example 6 has a high tanδ and a low crosslinking density and is soft, it shows good results in the folding test, however, since the hardness is too low, visible scratches are found after the wear test.

[0257] [Comparative Example 7]

[0258] As shown in Table 5, the resin composition of Comparative Example 7 contains 4.9 mass % of "SR444" and 22.06 mass % of "IBOA (SR506-A)" as resin (A) and 14.71 mass % of "CN9047" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Comparative Example 7 are similar to those of Comparative Example 3.

[0259] In Comparative Example 7, the weighted average functionality of the resin (A) was 1.47, and A / B was 2.18.

[0260] In Comparative Example 7, the glass transition temperature Tg was 102.7° C. The loss tangent tan δ at the glass transition temperature Tg was 0.2455.

[0261] In the folding test of Comparative Example 7, there was no change even after 200K foldings of the film. However, in Comparative Example 7, the water contact angle before the wear test was 113.5°, and the water contact angle after the wear test was 70.3°. Visible scratches were found.

[0262] As described above, in Comparative Example 7, the weighted average functionality of the resin (A) contained in the resin composition is 1.47. Therefore, the glass transition temperature Tg of Comparative Example 7 is as high as 102.7°C. The loss tangent tanδ of Comparative Example 7 at the glass transition temperature Tg is as high as 0.2455. In other words, it is presumed that since Comparative Example 7 has a high tanδ and a low crosslinking density and is soft, it shows good results in the folding test, however, since the hardness is too low, visible scratches are found after the wear test.

[0263] [Comparative Example 8]

[0264] As shown in Table 5, the resin composition of Comparative Example 8 contains 4.9 mass % of "SR444" and 19.61 mass % of "IBOA (SR506-A)" as resin (A) and 17.16 mass % of "CN9047" as resin (B). The active energy ray polymerization initiator, solvent, metal oxide nanoparticles and fluorine compound contained in the resin composition of Comparative Example 8 are similar to those of Comparative Example 3.

[0265] In Comparative Example 8, the weighted average functionality of the resin (A) was 1.50, and A / B was 1.73.

[0266] In Comparative Example 8, the glass transition temperature Tg was 93.2° C. The loss tangent tan δ at the glass transition temperature Tg was 0.2183.

[0267] In the folding test of Comparative Example 8, there was no change even after 200K foldings of the film. However, in Comparative Example 8, the water contact angle before the abrasion test was 107°, and the water contact angle after the abrasion test was 65°. Visible scratches were found.

[0268] As described above, in Comparative Example 8, the weighted average functionality of the resin (A) contained in the resin composition is 1.50. Therefore, the loss tangent tanδ at the glass transition temperature Tg of Comparative Example 8 is as high as 0.2183, and the hardness is too low. This is presumably the reason why the water contact angle of Comparative Example 8 after the wear test is as low as 65° and visible scratches are found.

[0269] As described above, according to the present embodiment, it is possible to provide the hard coating film 10 having both the performance of being able to withstand multiple and repeated folding and the resistance to scratches and abrasions.

[0270] The embodiments of the present invention have been described above with reference to the accompanying drawings. However, the invention disclosed herein is not limited thereto, and a person skilled in the art will understand various changes and modifications within the scope of the disclosure and claims.

[0271] The hard coating film 10 of the present invention can be used as a protective film in each device requiring such a film, such as a display screen, a screen, goggles, an eye mask, and a face mask of a display device. The hard coating film 10 disclosed above is particularly suitable for electronic devices such as (foldable) flexible displays, information terminals, etc. to be used in a curved manner, and all other similar items.

[0272] When the hard coating film 10 of the present disclosure is used for a display device, the hard coating film 10 may include a functional material layer and / or an adhesive layer for improving visibility. Examples of the functional material layer may include a diffusion layer, an anti-reflection layer, etc. Examples of the adhesive layer may include a photoelastic resin layer, etc.

[0273] Reference numerals list

[0274] 10 Hard coating film

[0275] 11 Basic Materials

[0276] 12 Hard coating

[0277] 12a First Area

[0278] 12b Second Area

[0279] 13 Antifouling layer

[0280] 100 Manufacturing Equipment

[0281] 110 Delivery Roller

[0282] 112 Take-up roller

[0283] 114a-d guide roller

[0284] 120 Coating device

[0285] 130 Drying device

[0286] 140 Curing device

[0287] 144 Guide Roller

[0288] 146 Guide Roller

[0289] 148 Light Source

Claims

1. A hard coating film, the hard coating film include: Basic materials; and A hard coating layer comprising a cured product of a resin composition containing a resin (A) and a resin (B), the hard coating layer being laminated on the base material, wherein The resin (A) is a multifunctional (meth) acrylic monomer having a weighted average functionality greater than or equal to 4, The resin (B) is aliphatic polyurethane acrylate, The hard coating has a glass transition temperature Tg greater than or equal to 50° C. and less than or equal to 100° C., and The loss tangent tanδ at the glass transition temperature Tg is greater than or equal to 0.07 and less than or equal to 0.15, The loss tangent tan δ of the hard coating layer is measured by a dynamic viscoelasticity measurement method applying a 1-Hz frequency dynamic load. 2 . The hard coating film according to claim 1 , wherein the resin composition further comprises metal oxide nanoparticles having an average particle size of less than or equal to 100 nm.

3. The hard coating film according to claim 2, wherein the content of the metal oxide nanoparticles contained in the resin composition is greater than or equal to 2 mass % and less than or equal to 5 mass % of the total solid content of the resin composition of the hard coating layer. 4 . The hard coating film according to claim 2 , wherein the metal oxide constituting the metal oxide nanoparticles is any one or both of silicon dioxide and aluminum oxide. The hard coating film according to claim 2 , wherein the metal oxide nanoparticles have a Mohs hardness greater than 6.

6. The hard coating film according to claim 1, wherein the water contact angle of the surface of the hard coating after abrasion is greater than 100°. The wear test was performed using a wear tester by using steel wool #0000, and the surface of the hard coating layer was worn by the steel wool under the conditions of a load of 1000 g, a speed of 50 mm / sec, a reciprocating distance of 40 mm, and 2500 reciprocations. 7 . The hard coating film according to claim 6 , wherein a water contact angle of the surface of the hard coating layer before abrasion is greater than 110°. 8 . The hard coating film according to claim 7 , wherein a decrease in a water contact angle of the surface of the hard coating layer after abrasion relative to a water contact angle of the surface of the hard coating layer before abrasion is less than 13%. 9 . The hard coating film according to claim 7 , wherein the content of the resin (A) contained in the resin composition is more than twice the content of the resin (B) and less than nine times the content of the resin (B).

10. The hard coating film according to claim 9, wherein the content of the resin (A) contained in the resin composition is greater than or equal to 20 mass % and less than or equal to 40 mass %, and the content of the resin (B) contained in the resin composition is greater than or equal to 2 mass % and less than or equal to 15 mass %.

11. The hard coating film of claim 1, wherein the hard coating film is configured to be folded at least one hundred thousand times by bending inwardly or outwardly without causing any cracking, interlayer separation, or loss of optical properties. 12 . The hard coating film according to claim 1 , wherein the base material is a thermoplastic base material having a thickness of greater than or equal to 10 μm and less than or equal to 200 μm. 13 . The hard coat film according to claim 1 , wherein the resin composition contains a fluorine compound, and the fluorine compound segregates to a first region located on a surface side of the hard coat layer. The hard coating film according to claim 13 , wherein the segregated fluorine compound provides an antifouling effect.

15. The hard coating film according to claim 13, wherein the fluorine compound is segregated to the surface of the hard coating layer.

16. The hard coating film according to claim 11, wherein the hard coating film is configured to be folded at least one hundred thousand times by bending inward or outward without any loss of optical performance, wherein the optical performance is one or more selected from the group consisting of total transmittance (%), transmission haze, gloss, and change in chromaticity b* (intensity of hue from blue to yellow). 17 . The hard coat film according to claim 13 , wherein the fluorine compound does not segregate in a second region located on the base material side of the hard coat layer.

Citation Information

Patent Citations

  • Flexible hardcoat compositions, articles, and methods

    US20090004478A1

  • Hardcoat layers on release liners

    CN101688093A

  • UV-curing acrylic resin compositions for thermoformable hardcoat applications

    CN109929292A

  • High hardness flexible hard coating film

    US20210079254A1