Electrochemical device separator, method of manufacturing the same, and electrochemical device including the same
By forming a porous coating containing polymer binder particles and inorganic particles in the lithium secondary battery, and using deformation technology in the film forming region, the problem of separation of the porous coating and the porous substrate is solved, and the lithium secondary battery is improved durability and performance stability.
Patent Information
- Application Number
- CN202480002303.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-15
- Filing Date
- 2024-01-16
- Publication Date
- 2024-12-06
AI Technical Summary
The porous coating of existing lithium secondary batteries is easily separated from the porous substrate during the manufacturing process, resulting in low durability and affecting the performance of the electrochemical device.
By forming a porous coating containing polymer binder particles and inorganic particles on the surface of the porous polymer substrate, the film-forming region is used to deform at the glass transition temperature of the polymer binder particles to form a 3% to 50% Film-forming areas to improve the adhesion strength of the porous coating to the porous substrate.
The durability and bonding strength of the porous coating are significantly improved, separation from the porous substrate is avoided, the stability of breathability and resistance is maintained, and the service life of the electrochemical device is extended.
Smart Images

Figure CN119096411A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a separator for an electrochemical device, a method of manufacturing the separator, and an electrochemical device including the same. Background Art
[0002] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions, and recently, lithium secondary batteries have been widely used, which may have high energy density and voltage, long cycle life, and may be used in a variety of fields.
[0003] The lithium secondary battery may include an electrode assembly formed by a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and the electrode assembly may be manufactured by being stored in a housing together with an electrolyte. The separator may include a porous coating layer comprising a polymer binder and inorganic particles on at least one surface of a porous substrate. The inorganic particles may be connected to other inorganic particles by a polymer binder to form an interstitial volume, and lithium ions may move by passing through the interstitial volume. In addition to fixing the inorganic particles, the polymer binder may also provide bonding strength to the porous coating layer, and the porous coating layer may be combined with each of the porous substrate and the electrode.
[0004] Conventionally, aqueous particulate polymer binders have been used to form a single-component coating on the surface of a porous substrate such as polyolefin to form a porous coating having excellent heat resistance and adhesive strength. However, the porous coating has a problem of being easily separated from the porous substrate during the manufacture of electrode assemblies and electrochemical devices due to low durability.
[0005] Therefore, a separator having a structure that prevents the porous coating layer from being easily separated from the porous substrate while maintaining the advantages of the porous coating layer including an aqueous particulate polymer binder and the physical properties of the separator and a method for manufacturing the same have been studied. Summary of the invention
[0006] Technical issues
[0007] The present disclosure aims to provide a method of manufacturing a separator for an electrochemical device having excellent bonding strength to a porous substrate and an electrode by improving the durability of a porous coating layer including a polymer binder and inorganic particles.
[0008] Technical Solution
[0009] One aspect of the present disclosure provides a separator for an electrochemical device, which includes a porous polymer substrate and a porous coating, wherein the porous coating includes a particle region formed by polymer binder particles and inorganic particles and a film-forming region containing deformed polymer binder particles, and is formed on at least any surface of the porous polymer substrate, wherein the film-forming region is in the range of 3 wt % to 50 wt % relative to the total weight of the polymer binder particles.
[0010] When the end of the diamond tip is disposed in a region between a surface of the porous coating contacting a porous polymer substrate and an opposite surface facing the surface, and the diamond tip is moved in a direction parallel to the porous polymer substrate at a speed of 100 mm / min, the first dynamic friction coefficient caused by friction loss can be in the range of 1 to 2.
[0011] When the end of the diamond tip is disposed in a region between a surface of the porous coating layer contacting a porous polymer substrate and an opposite surface facing the surface, and the diamond tip is moved in a direction parallel to the porous polymer substrate at a speed of 100 mm / min, the difference between the static friction coefficient caused by friction loss and the first dynamic friction coefficient can be 3 or less.
[0012] The adhesive strength between the porous polymer substrate and the porous coating layer may be in the range of 1.5 to 6 times the adhesive strength exhibited by the opposite surface of the porous coating layer facing the surface contacting the porous polymer substrate.
[0013] The polymer binder particles may include one or more selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethylhexyl acrylate, methyl methacrylate, styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber.
[0014] The film-forming region can be formed by exposing the polymer binder particles to the glass transition temperature T g To T g Formed at temperatures in the range of +40°C.
[0015] One aspect of the present disclosure provides an electrochemical device including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is a separator for an electrochemical device according to one aspect.
[0016] The electrochemical device may be a lithium secondary battery.
[0017] One aspect of the present disclosure provides a method for manufacturing a separator for an electrochemical device, the method comprising coating at least one surface of a porous polymer substrate with a coating slurry comprising polymer binder particles, inorganic particles and a dispersion medium, forming a coating layer comprising a particle region formed by the polymer binder particles and the inorganic particles, removing the dispersion medium by drying the coating layer, and forming a film-forming region by deforming 3 wt % to 50 wt % relative to the total weight of the polymer binder particles by drying the coating layer.
[0018] Removal of the dispersion medium may include preventing the surface of the coating from exceeding 50°C.
[0019] The formation of the film-forming region may include exposing the coating to a temperature of the glass transition temperature T g To T g Temperatures in the range of +40°C for 24 hours or less.
[0020] Beneficial Effects
[0021] According to the separator for an electrochemical device according to the present disclosure, by deforming a predetermined amount of polymer binder particles into the form of a film, the separation strength between the porous coating layer and the porous polymer substrate can be increased without deteriorating the air permeability and the resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a top view of a separator according to one embodiment of the present disclosure, which is a conceptual diagram showing the appearance of the porous coating layer 20 .
[0023] Figure 2 : is a cross-sectional view of a separator 1 according to one embodiment of the present disclosure, which is a conceptual diagram showing a state when a diamond tip T is inserted into a porous coating layer 20 to a depth D for measuring a friction coefficient according to one embodiment. DETAILED DESCRIPTION
[0024] Hereinafter, each configuration of the present disclosure will be described in more detail so that those skilled in the art to which the present disclosure belongs can easily implement the present disclosure, but this is merely an example, and the scope of the present disclosure is not limited by the following description.
[0025] As used herein, the term "comprising" is used to list materials, compositions, devices and methods useful in the present disclosure and is not limited to the listed examples.
[0026] The terms "about" and "substantially" as used herein are used to refer to ranges or approximations of numbers or degrees that take into account unique manufacturing and material tolerances, and are used to prevent an infringer from unfairly using the disclosure in which precise values or absolute values provided to aid understanding of the disclosure are mentioned.
[0027] The term "electrochemical device" used herein may refer to a primary battery, a secondary battery, a supercapacitor, and the like.
[0028] The term "film-forming region" as used herein refers to a region in which the polymer binder contained in the porous coating layer is exposed to a temperature above its intrinsic glass transition temperature T g The invention relates to a region that is deformed by a temperature and because it may not be able to maintain its original shape, or a region formed by physical or chemical connection with one or more adjacent polymer binders according to the deformation.
[0029] In the following, although the present disclosure has been described through specific examples and implementation schemes, the present disclosure is not limited thereto and may include a situation where any one or more configurations in the specific examples and implementation schemes are combined by a person skilled in the art to which the present disclosure belongs, and various modifications and changes may be made within the technical spirit of the present disclosure and the equivalent scope of the appended claims.
[0030] In the following, reference will be made to Figure 1 and Figure 2 A specific example of the present disclosure is described. Figure 1 is a top view of a separator according to a specific example of the present disclosure, which is a conceptual diagram showing the appearance of the porous coating layer 20, Figure 2 2 is a side view of the separator 1 , which is a conceptual diagram showing a process of measuring a friction coefficient by inserting a diamond tip T into the porous coating layer 20 .
[0031] A specific example of the present disclosure provides a separator 1 for an electrochemical device, comprising a porous polymer substrate 10 and a porous coating 20, the porous coating 20 comprising a particle region P composed of polymer binder particles 21 and inorganic particles 22 and a film-forming region F comprising deformed polymer binder particles, and is formed on at least any surface of the porous polymer substrate 10, and the film-forming region F is in the range of 3 wt % to 50 wt % relative to all polymer binder particles.
[0032] The porous polymer substrate 10 is a porous film in which a plurality of pores are formed, and can prevent short circuits by electrically insulating the positive electrode and the negative electrode. For example, when the electrochemical device is a lithium secondary battery, the porous polymer substrate 10 can be an ion conductive barrier that allows lithium ions to pass through while preventing electrical contact between the positive electrode and the negative electrode. At least some of the pores can form a three-dimensional network that communicates with the surface and the interior of the porous polymer substrate 10, and a fluid can pass through the porous polymer substrate 10 through the pores.
[0033] The porous polymer substrate 10 can use a material that is physically and chemically stable relative to the electrolyte as an organic solvent. For example, the porous polymer substrate 10 is made of a resin such as: polyolefins (e.g., polyethylene, polypropylene, and polybutylene), polyvinyl chloride, polyethylene terephthalate, polycycloolefins, polyethersulfones, polyamides, polyimides, polyimide amides, nylons, polytetrafluoroethylene, and copolymers or mixtures thereof, but is not limited thereto. Preferably, a polyolefin-based resin can be used. A polyolefin-based resin can be processed into a relatively small thickness and is easy to apply with a coating slurry, and is therefore suitable for manufacturing an electrochemical device with a higher energy density.
[0034] The porous polymer substrate 10 may have a single-layer structure or a multi-layer structure. The porous polymer substrate 10 may include two or more polymer resin layers having different melting points Tm, and provide a shutdown function when the battery is out of control at high temperature. For example, the porous polymer substrate 10 may include a polypropylene layer having a relatively high melting point and a polyethylene layer having a relatively low melting point. Preferably, the porous polymer substrate 10 may have a three-layer structure in which polypropylene, polyethylene, and polypropylene are stacked in sequence. When the temperature of the battery rises to a predetermined temperature or higher, the polyethylene layer melts and closes the pores to prevent thermal runaway of the battery.
[0035] The thickness of the porous polymer substrate 10 may be in the range of 1 μm or more and 100 μm or less. Specifically, the thickness of the porous polymer substrate 10 may be in the range of 10 μm or more and 90 μm or less, 20 μm or more and 80 μm or less, 30 μm or more and 70 μm or less, or 40 μm or more and 60 μm or less. Preferably, the thickness of the porous polymer substrate 10 may be in the range of 1 μm or more and 30 μm or less. More preferably, the thickness of the porous polymer substrate 10 may be in the range of 5 μm or more and 15 μm or less, or 8 μm or more and 13 μm or less. By adjusting the thickness of the porous polymer substrate 10 within the above range, the amount of active material contained in the electrochemical device can be increased by minimizing the volume of the electrochemical device while electrically insulating the positive and negative electrodes.
[0036] The porous polymer substrate 10 may include pores whose average diameter is in the range of 0.01 μm or more and 1 μm or less. Specifically, the size of the pores included in the porous polymer substrate 10 may be in the range of 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. Preferably, the size of the pores may be in the range of 0.02 μm or more and 0.06 μm or less. By adjusting the pore size of the porous polymer substrate 10 within the above range, the air permeability and ionic conductivity of the manufactured separator as a whole can be adjusted.
[0037] The air permeability of the porous polymer substrate 10 may be 10 seconds / 100cc or more and 100 seconds / 100cc or less. Specifically, the air permeability of the porous polymer substrate 10 is in the range of 10 seconds / 100cc or more and 90 seconds / 100cc or less, 20 seconds / 100cc or more and 80 seconds / 100cc or less, 30 seconds / 100cc or more and 70 seconds / 100cc or less, or 40 seconds / 100cc or more and 60 seconds / 100cc or less. Preferably, the air permeability of the porous polymer substrate 10 may be in the range of 50 seconds / 100cc or more and 70 seconds / 100cc or less. When the air permeability of the porous polymer substrate 10 is within the above range, the air permeability of the manufactured separator may be provided within a range suitable for ensuring the output and cycle characteristics of the electrochemical device.
[0038] Air permeability (seconds / 100cc) refers to the time (seconds) it takes for 100cc of air to pass through a porous polymer substrate 10 or separator 1 having a predetermined area at a constant pressure. Air permeability can be measured using a Gurley densitometer according to ASTM D 726-58, ASTM D726-94, or JIS-P8117. For example, Gurley's 4110N device can be used to measure the air permeability of 100cc of air at 0.304 kPa air or 1.215 kN / m 2 Water pressure passes through 1 square inch (or 6.54 cm 2 For example, the Asahi Seiko EG01-55-1MR instrument can be used to measure the time it takes for 100cc of air to pass through a 1 square inch sample at room temperature under a constant pressure of 4.8 inches of water.
[0039] The porosity of the porous polymer substrate 10 may be 10% by volume or more and 60% by volume or less. Specifically, the porosity of the porous polymer matrix 10 may be in the range of 15% by volume or more and 55% by volume or less, 20% by volume or more and 50% by volume or less, 25% by volume or more and 45% by volume or less, or 30% by volume or more and 40% by volume or less. Preferably, the porosity of the porous polymer substrate 10 may be in the range of 30% by volume or more and 50% by volume or less. When the porosity of the porous polymer substrate 10 is within the above range, the ionic conductivity of the manufactured separator 1 may be provided within a range suitable for ensuring the output and cycle characteristics of the electrochemical device.
[0040] Porosity refers to the volume ratio of pores to the total volume of the porous polymer substrate 10. Porosity can be measured by methods known in the art. For example, porosity can be measured by BET (Brunauer Emmett Teller) measurement using nitrogen adsorption, capillary flow porosimetry, or water or mercury penetration methods.
[0041] The porous coating layer 20 is formed on at least any one surface of the porous polymer substrate 10 and includes polymer binder particles 21 and inorganic particles 22. The porous coating layer 20 can be formed by coating at least one surface of the porous polymer substrate 10 with a coating slurry including the polymer binder particles 21, the inorganic particles 22, and a dispersion medium. The porous coating layer 20 is combined with the porous polymer substrate 10 by including a gap volume in which the inorganic particles 22 are connected by the polymer binder particles 21 to allow lithium ions to pass through, thereby preventing thermal shrinkage of the porous polymer substrate 10.
[0042] The coating slurry may include a dispersion medium to dissolve or disperse at least some of the polymer binder particles 21 and disperse the inorganic particles 22. By adjusting the type and content of the dispersion medium, the coating slurry can be used to uniformly disperse the polymer binder particles 21 and the inorganic particles 22. For example, the dispersion medium can be one selected from the following: water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile and a combination thereof. Preferably, the dispersion medium can be a mixture of water and isopropyl alcohol or water. A porous coating 20 in which the polymer binder particles 21 and the inorganic particles 22 are uniformly dispersed using the above-mentioned type of dispersion medium can be formed.
[0043] The coating slurry may further include additives such as dispersants, surfactants, defoamers, and flame retardants to improve dispersibility and flame retardancy, and to improve the uniformity of the formed porous coating 20. For example, the dispersant may include one or more selected from the following: polyacrylic acid, oil-soluble polyamines, oil-soluble amine compounds, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, and pyrogallic acid. By using the above-mentioned types of dispersants, the stability of the coating slurry can be improved and the uniformity of the porous coating 20 formed by the coating slurry can be ensured.
[0044] The additive may be included in an amount of 0 wt % or more and 5 wt % or less relative to the total weight of the coating slurry. Specifically, the content of the additive may be in the range of 0.01 wt % or more and 4 wt % or less, 0.1 wt % or more and 3 wt % or less, or 1 wt % or more and 2 wt % or less. Preferably, the content of the additive may be in the range of 1 wt % or more and 5 wt % or less. By adjusting the content of the additive within the above range, uniform dispersion and stability of the inorganic particles contained in the coating slurry may be achieved.
[0045] After forming the porous coating 20, the dispersion medium contained in the coating slurry can be removed by drying or heating. For example, the porous coating 20 may contain 5ppm or less of the dispersion medium. Preferably, the porous coating 20 may be formed by polymer binder particles 21 and inorganic particles 22. In the process of removing the dispersion medium, a plurality of pores may be formed inside and on the surface of the porous coating 20. The pores may include interstitial volumes formed between the inorganic particles 22, and have a structure that allows fluid to pass through due to the formation of a three-dimensional network.
[0046] The thickness of the porous coating layer 20 may be in the range of 1 μm or more and 15 μm or less. Specifically, the thickness of the porous coating layer 20 may be in the range of 2 μm or more and 14 μm or less, 3 μm or more and 13 μm or less, 4 μm or more and 12 μm or less, 5 μm or more and 11 μm or less, 6 μm or more and 10 μm or less, or 7 μm or more and 9 μm or less. Preferably, the thickness of the porous coating layer 20 may be in the range of 1 μm or more and 5 μm or less, more preferably, 1 μm or more and 3 μm or less. By adjusting the thickness of the porous coating layer 20 within the above range, the shrinkage of the porous polymer substrate 10 can be minimized, thereby achieving stable bonding with the porous polymer substrate 10.
[0047] The polymer binder particles 21 may bind the inorganic particles 22 contained in the porous coating layer 20 and provide adhesive strength to the porous coating layer 20. The polymer binder particles 21 may have a spherical or elliptical shape, but may also include other shapes besides an amorphous shape. When the polymer binder particles 21 are exposed to a temperature higher than the glass transition temperature T of the polymer binder particles 21, the porous coating layer 20 may be bonded to the inorganic particles 22. g When the temperature reaches , the polymer binder particles 21 may no longer maintain the shape of the particles and may be deformed to form the film-forming region F.
[0048] The film-forming region F may be an irregular region due to the polymer binder particles 21 that may not maintain the original shape and solidify in a collapsed state, and may be formed by bonding one or more polymer binder particles 21 to each other. The porous coating layer 20 may include the film-forming region F and the particle region P as a remaining region. As the dispersion medium is removed from the coating slurry, the particle region P may be formed by the polymer binder particles 21 and the inorganic particles 22. The film-forming region F may be formed by deforming the shape of one or more polymer binder particles 21 contained in the particle region P. Figure 1 and Figure 2 , the porous coating layer 20 may include one or more film-forming regions F. The remaining region of the porous coating layer 20 except the film-forming region F may be referred to as a particle region P. The film-forming region F may be bonded to one or more of the polymer binder particles 21, the inorganic particles 22, the porous polymer substrate 10, and the additional film-forming region F contained in the adjacent particle region P. The film-forming region F may have a smaller surface area than the polymer binder particles 21 having the same weight, but has a larger surface area in contact with the additional polymer binder particles 21, the additional film-forming region F, or the inorganic particles 22 contained in the porous coating layer 20. For example, while the spherical polymer binder particles 21 are bonded in contact with the spherical inorganic particles 22 with a relatively small surface area, the irregular film-forming region F may be bonded in contact with the spherical inorganic particles 22 with a relatively large surface area. The porous coating layer 20 including the film-forming region F may show a higher bonding strength to the porous polymer substrate 10. Furthermore, the porous coating layer 20 including the film-forming region F may show higher adhesive strength to a surface opposite to the surface in contact with the porous polymer substrate 10 (ie, an electrode).
[0049] The film-forming region F can be formed by additional drying or heating after the porous coating layer 20 is formed by applying the coating slurry on the porous polymer substrate 10 and drying. The film-forming region F can be dispersed in the thickness direction of the porous coating layer 20. For example, the film-forming region F can be dispersed between the surface of the porous coating layer 20 in contact with the porous polymer substrate 10 and the opposite surface facing the surface (i.e., the surface in contact with the electrode). The film-forming region F can be uniformly dispersed between the two surfaces of the porous coating layer 20 and may not be densely dispersed on either surface. This may mean that half or more of the film-forming region F is dispersed between the two surfaces of the porous coating layer 20 relative to the weight of the entire film-forming region. When half or more of the film-forming region F is dispersed on either or both surfaces of the porous coating layer relative to the weight of the entire film-forming region F, the pores formed on or inside the porous coating layer 20 may be closed. Preferably, the film-forming region F can be uniformly dispersed in the thickness direction of the porous coating layer 20.
[0050] Relative to a plane surface parallel to one surface of the porous polymer substrate 10, the maximum cross-sectional area of the film-forming region F is 1.1 to 3.5 times the maximum cross-sectional area of the polymer binder particles 21. Specifically, the maximum cross-sectional area of the film-forming region F may be in the range of 1.3 times or more and 3.3 times or less, 1.5 times or more and 3.1 times or less, 1.7 times or more and 2.9 times or less, 1.9 times or more and 2.7 times or less, or 2.1 times or more and 2.5 times or less compared to the maximum cross-sectional area of the polymer binder particles 21. Preferably, the maximum cross-sectional area of the film-forming region F may be in the range of 1.1 to 2.5 times the maximum cross-sectional area of the polymer binder particles 21. By adjusting the cross-sectional area ratio of the film-forming region F to the polymer binder particles 21 within the above range, the air permeability of the separator suitable for the electrochemical device can be ensured, and the bonding strength to the porous polymer substrate 10 can be ensured.
[0051] The film-forming region F may be in the range of 3 wt % or more and 50 wt % or less relative to the total weight of the polymer binder particles 21 contained in the porous coating layer 20. The weight of the film-forming region F may be in the range of 3 wt % or more and 50 wt % or less relative to the sum of the total weight of the polymer binder particles 21 contained in the particle region P and the weight of the film-forming region F. Specifically, the film-forming region F may be in the range of 5 wt % or more and 45 wt % or less, 10 wt % or more and 40 wt % or less, 15 wt % or more and 35 wt % or less, or 20 wt % or more and 30 wt % or less relative to the total weight of the polymer binder particles 21. Preferably, the film-forming region F may be in the range of 3 wt % or more and 10 wt % or less, or 30 wt % or more and 50 wt % or less relative to the total weight of the polymer binder particles 21. For example, when the polymer binder particles 21 are contained at 5 wt% or less relative to the total weight of the porous coating layer 20, the film-forming region F may be 3 wt% or more and 10 wt% or less relative to the total weight of the polymer binder particles 21. When the polymer binder particles 21 are contained at more than 5 wt% relative to the total weight of the porous coating layer 20, the film-forming region F may be in the range of 30 wt% or more and 50 wt% or less relative to the total weight of the polymer binder particles 21. When more than 50 wt% of the total weight of the polymer binder particles 21 contained in the porous coating layer 20 are film-formed, the air permeability and resistance of the separator 1 manufactured by closing the pores formed inside or on the surface of the porous coating layer 20 may increase, thereby deteriorating the performance of the electrochemical device. When less than 3 wt% of the total weight of the polymer binder particles 21 contained in the porous coating layer 20 are film-formed, the adhesive strength to the porous polymer substrate 10 cannot be sufficiently ensured, and thus the porous coating layer may be separated due to repeated use of the electrochemical device.
[0052] Whether the porous coating layer 20 is separated from the porous polymer substrate 10 due to repeated use of the electrochemical device can be determined by the friction coefficient caused by friction loss on the porous coating layer 20 and whether the porous coating layer 20 is separated due to friction. The friction coefficient can be measured by using a friction loss meter according to JIS K 7125, JIS P 8147, or JIS K 5600. For example, when repeated friction is applied by using a 5g / diamond tip as an accessory, the static friction coefficient at the time point of the initial movement of the tip and the dynamic friction coefficient at the first friction loss can be measured by using a 14FW type surface property tester of Heidon. Figure 2, the friction loss meter (not shown) may have a horizontal and flat test surface, and generate friction by placing and fixing the separator 1 on the test surface, and then moving and repeatedly moving (A or B) the diamond tip T at a predetermined speed in a direction parallel to the porous polymer substrate 10. The moving speed of the tip T may be in the range of 50 mm / min to 200 mm / min. For example, the friction coefficient may be measured by arranging the end of the diamond tip T in a region between the surface of the porous coating 20 contacting the porous polymer substrate 10 and the surface opposite to the surface, and moving the diamond tip T in a direction parallel to the porous polymer substrate 10 at a speed of 100 mm / min. The end of the tip T is not arranged to contact any surface of the porous coating 20. For example, the end of the diamond tip T may be arranged at a depth D less than the thickness of the porous coating 20. For example, when the thickness of the porous coating 20 is 3 μm, the end of the tip T may be repeatedly moved in a state of being spaced apart from the surface of the porous coating 20 in contact with the porous polymer substrate 10 by an interval of 1.0 μm to 1.5 μm. For example, when the thickness of the porous coating 20 is 2 μm, the end of the tip T may be set at a depth D of 1 μm. The diamond tip T may peel the porous coating 20 from the porous polymer substrate 10 while reciprocating in the A direction, the B direction, or the A direction and the B direction. Whether the peeling of the porous coating 20 occurs can be determined by visually checking the time point at which the porous coating 20 is peeled from the porous polymer substrate 10 by applying repeated friction to the separator 1, and the peeling strength of the porous coating 20 can be checked from the number of repeated frictions until the peeling time point.
[0053] In a separator for an electrochemical device according to a specific example, when the end of the diamond tip T is set in a region between the surface of the porous coating 20 contacting the porous polymer substrate 10 and the opposite surface facing the surface, and the diamond tip moves at a speed of 100 mm / min in a direction parallel to the porous polymer substrate 10, the first kinetic friction coefficient caused by friction loss can be in the range of 1 or more and 2 or less. Specifically, the first kinetic friction coefficient caused by friction loss on the porous coating 20 can be in the range of 1.1 or more and 1.9 or less, 1.2 or more and 1.8 or less, 1.3 or more and 1.7 or less, or 1.4 or more and 1.6 or less. Preferably, the first kinetic friction coefficient caused by friction loss on the porous coating 20 can be in the range of 1.2 or more and 1.5 or less. The first kinetic friction coefficient is a kinetic friction coefficient displayed when the tip starts to move and performs an initial reciprocating motion, and can be displayed in proportion to the content of the film-forming region F included in the porous coating 20. When the first kinetic friction coefficient exceeds 2, an excess or half or more of the content of the film-forming region F may be densely dispersed on any surface of the porous coating layer 20, and the transmittance and resistance of the separator 1 manufactured by closing the pores of the porous coating layer 20 may increase, thereby deteriorating the performance of the electrochemical device. When the first kinetic friction coefficient is less than 1, the adhesive strength to the porous polymer substrate 10 cannot be sufficiently ensured, and thus the porous coating layer 20 may be separated from the porous polymer substrate 10 due to repeated use of the electrochemical device.
[0054] In the separator 1 for an electrochemical device according to a specific example, when the end of the diamond tip T is set in the region between the surface of the porous coating layer 20 contacting the porous polymer substrate 10 and the opposite surface facing the surface, and the diamond tip T moves at a speed of 100 mm / min in a direction parallel to the porous polymer substrate 10, the difference between the static friction coefficient caused by friction loss and the first dynamic friction coefficient can be 3 or less. Specifically, the difference between the static friction coefficient caused by friction loss and the first dynamic friction coefficient on the porous coating layer 20 can be in the range of 2.9 or less, 2.8 or less, 2.6 or less, 2.4 or less, 2.2 or less, 2.0 or less, or 1.8 or less. Preferably, the difference between the static friction coefficient caused by friction loss and the first dynamic friction coefficient on the porous coating layer 20 can be in the range of 1.0 or more and 2.9 or less. When the film-forming regions F are densely dispersed on any surface of the porous coating layer 20, the difference between the static friction coefficient and the first dynamic friction coefficient shows a large difference, which means that the pores formed inside or on the surface of the porous coating layer 20 are more closed. When the difference exceeds 3, the air permeability and resistance of the separator 1 manufactured by closing the pores formed inside or on the surface of the porous coating layer 20 may increase, thereby deteriorating the performance of the electrochemical device.
[0055] In a separator 1 for an electrochemical device according to a specific example, when the end of the diamond tip T is set in a region between the surface of the porous coating layer 20 contacting the porous polymer substrate 10 and the opposite surface facing the surface, and friction loss is caused by moving the diamond tip in a direction parallel to the porous polymer substrate 10 at a speed of 100 mm / min 5 times or more and 35 times or less, the porous coating layer 20 can be separated. Specifically, after performing friction loss in the range of 6 times or more and 34 times or less, 7 times or more and 33 times or less, 8 times or more and 32 times or less, 9 times or more and 31 times or less, 10 times or more and 30 times or less, 11 times or more and 29 times or less, 12 times or more and 28 times or less, 13 times or more and 27 times or less, 14 times or more and 26 times or less, 15 times or more and 25 times or less, 16 times or more and 24 times or less, 17 times or more and 23 times or less, 18 times or more and 22 times or less, or 19 times or more and 21 times or less, the porous coating layer 20 can be peeled off from the porous polymer substrate 10. Peeling means that at least a portion of the porous coating layer 20 is separated from the porous polymer substrate 10. Preferably, the porous coating layer 20 can be peeled off from the porous polymer substrate 10 when the friction loss is repeated 18 times or more and 32 times or less. The separator 1 satisfying the above range may exhibit gas permeability and resistance suitable for application to an electrochemical device.
[0056] The air permeability of the separator 1 for electrochemical devices can be 20 seconds / 100cc or more and 90 seconds / 100cc or less. Specifically, the air permeability of the separator 1 can be 25 seconds / 100cc or more and 85 seconds / 100cc or less, 30 seconds / 100cc or more and 80 seconds / 100cc or less, 35 seconds / 100cc or more and 75 seconds / 100cc or less, 40 seconds / 100cc or more and 70 seconds / 100cc or less, 45 seconds / 100cc or more and 65 seconds / 100cc or less, or 50 seconds / 100cc or more and 55 seconds / 100cc or less. Preferably, the air permeability of the separator 1 can be in the range of 80 seconds / 100cc or more and 90 seconds / 100cc or less. When the air permeability of the separator 1 is within the above range, the output, stability and cycle characteristics of the electrochemical device can be ensured.
[0057] When a battery is manufactured by using the separator 1 for an electrochemical device, the resistance of the battery may be 0.5 ohms or more and 1.5 ohms or less. Specifically, the resistance of the battery may be in the range of 0.6 ohms or more and 1.4 ohms or less, 0.7 ohms or more and 1.3 ohms or less, 0.8 ohms or more and 1.2 ohms or less, or 0.9 ohms or more and 1.1 ohms or less. Preferably, the resistance of the battery may be in the range of 0.6 ohms or more and 0.8 ohms or less.
[0058] In the separator 1 for an electrochemical device according to a specific example, the adhesive strength between the porous coating and the surface of the porous coating contacting the porous polymer substrate 10, i.e., the peel strength, may be in the range of 100 gf / 15 mm or more and 200 gf / 15 mm or less. Specifically, the peel strength of the separator 1 may be in the range of 110 gf / 15 mm or more and 190 gf / 15 mm or less, 120 gf / 15 mm or more and 180 gf / 15 mm or less, 130 gf / 15 mm or more and 170 gf / 15 mm or less, or 140 gf / 15 mm or more and 160 gf / 15 mm or less. Preferably, the peel strength of the separator 1 may be in the range of 100 gf / 15 mm or more and 130 gf / 15 mm or less. When the peel strength is less than 100 gf / 15 mm, the porous coating is peeled off from the porous polymer substrate 10 during the cycle life of the electrochemical device, and when the peel strength is greater than 200 gf / 15 mm, the film-forming area F is densely dispersed on one surface of the porous coating 20, especially on the surface in contact with the porous polymer substrate 10, which manifests as an increase in permeability and resistance.
[0059] In the separator 1 for an electrochemical device according to a specific example, the bonding strength between the porous coating 20 and the surface of the porous coating 20 contacting the electrode, that is, the electrode-separator bonding strength may be in the range of 10gf / 25mm or more and 50gf / 25mm or less. Specifically, the electrode-separator bonding strength may be in the range of 15gf / 25mm or more and 45gf / 25mm or less, 20gf / 25mm or more and 40gf / 25mm or less, or 25gf / 25mm or more and 35gf / 25mm. Preferably, the electrode-separator bonding strength may be in the range of 35gf / 25mm or more and 50gf / 25mm or less. When the electrode-separator bonding strength is less than 10 gf / 25 mm, the electrode and the separator are separated after manufacturing the electrode assembly, and when the electrode-separator bonding strength exceeds 50 gf / 25 mm, the separator 1 in the electrode assembly cannot be uniformly wetted by the electrolyte, and lithium dendrites may precipitate on the surface of the separator 1.
[0060] The peel strength of separator 1 and the electrode-separator bonding strength can be measured by attaching a double-sided tape to separator 1, combining a glass slide, and then peeling the glass slide from the separator in a direction of 180° relative to the bonding direction. For example, the peel strength of the porous coating 20 can be measured by attaching a double-sided tape to the porous coating 20 of separator 1 and separating the glass slide at a speed of 300 minutes / mm using Instron's UTM (Universal Testing Machine). For example, the electrode-separator bonding strength can be measured by combining the electrode and separator 1, then attaching the double-sided tape to the separator, and separating the glass slide at a speed of 300 minutes / mm using UTM.
[0061] In a separator 1 for an electrochemical device according to a specific example, the bonding strength between the porous polymer substrate 10 and the porous coating 20 may be in the range of 1.5 to 6 times the bonding strength shown by the opposite surface of the porous coating 20 facing the surface contacting the porous polymer substrate 10. That is, the peel strength of the separator 1 may be in the range of 1.5 to 6 times the electrode-separator bonding strength. Specifically, the peel strength of the separator 1 may be in the range of 2 to 5.5 times, 2.5 to 5 times, 3 to 4.5 times, or 3.5 to 4 times the electrode-separator bonding strength. Preferably, the peel strength of the separator 1 may be in the range of 3 times or more and 6 times or less of the electrode-separator bonding strength. The durability of the electrode assembly manufactured by combining the separator 1 and the electrode can be ensured within the above range.
[0062] The glass transition temperature T of the polymer binder particles 21 g It may be 0°C or higher and 60°C or lower. Specifically, the glass transition temperature of the polymer binder particles 21 may be in the range of 5°C or higher and 55°C or lower, 10°C or higher and 50°C or lower, 15°C or higher and 45°C or lower, 20°C or higher and 40°C or lower, or 25°C or higher and 35°C or lower. Preferably, the glass transition temperature of the polymer binder particles 21 may be in the range of 20°C or higher and 40°C or lower. The polymer binder particles 21 having a glass transition temperature within the above range may maintain a particle shape during the drying process for removing the dispersion medium contained in the coating slurry, and then at least some of the polymer binder particles 21 may form a film-forming region F by drying or heating within the temperature range described below.
[0063] The weight average molecular weight Mw of the polymer binder particles 21 may be in the range of 1,000 or more and 10,000,000 or less. Specifically, the weight average molecular weight of the polymer binder particles 21 may be in the range of 1,000 or more and 10,000,000 or less, 10,000 or more and 9,000,000 or less, 100,000 or more and 8,000,000 or less, 200,000 or more and 7,000,000 or less, 300,000 or more and 6,000,000 or less, 500,000 or more and 5,000,000 or less, 1,000,000 or more and 4,000,000 or less, or 2,000,000 or more and 3,000,000 or less. The separator 1 having a durable porous coating layer may be manufactured by adjusting the weight average molecular weight of the polymer binder particles 21 within the above range to ensure mechanical characteristics of the porous coating layer 20 .
[0064] The weight average molecular weight can be measured by using gel permeation chromatography (GPC, PL GPC220, Agilent Technologies). For example, the weight average molecular weight can be measured by using TCB (trichlorobenzene) as a solvent in a PL Olexis (Polymer Laboratories) column (column temperature: 160°C) and using an Agilent high temperature RI detector under the conditions of a sample concentration of 1.0 mg / mL, a flow rate of 1.0 mL / min, and an injection volume of 200 μl (standard: polystyrene).
[0065] The porous coating layer 20 may include polymer binder particles 21 and inorganic particles 22 in a weight ratio of 5:95 to 80:20. Specifically, the weight ratio of the polymer binder particles 21 to the inorganic particles 22 in the porous coating layer 20 may be in the range of 10:90 to 80:20, 20:80 to 80:20, 30:70 to 70:30, 40:60 to 60:40, or 50:50. Preferably, the weight ratio of the polymer binder particles 21 to the inorganic particles 22 may be in the range of 60:40 to 80:20. By adjusting the composition of the porous coating layer 20 within the above range, the total polymer binder particles 21 in the above content range are formed into a film, thereby simultaneously ensuring the durability of the porous polymer substrate 10 and the bonding strength of the separator 1.
[0066] The polymer binder particles 21 may be a copolymer containing an acrylic polymer resin or a copolymer containing an acrylic monomer. The acrylic polymer resin may be one or more selected from the following: polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, and their copolymers. The copolymer containing an acrylic monomer may be one or more selected from styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber. Preferably, the polymer binder particles 21 may be styrene-butadiene rubber. The separator 1 having the durability and adhesive strength of the porous coating 20 can be obtained by sequentially forming the film-forming region F after selecting the above types of polymer binder particles 21 and removing the dispersion medium during the manufacture of the porous coating 20.
[0067] The inorganic particles 22 may be electrochemically stable particles. The inorganic particles 22 are not particularly limited as long as no oxidation and / or reduction reaction occurs within the operating voltage range of the electrochemical device (e.g., 0 V to 5 V based on Li / Li+). In particular, when using inorganic particles with a high dielectric constant as the inorganic particles 22, the ionic conductivity of the electrolyte can be increased by promoting the dissociation degree of electrolyte salts such as lithium salts in the liquid electrolyte. For the above reasons, the inorganic particles 22 include high dielectric constant inorganic particles with a dielectric constant of 5 or greater, preferably 10 or greater. Non-limiting examples of inorganic particles 22 with a dielectric constant of 5 or greater include BaTiO3, Pb(Zr,Ti)O3 (PZT), b 1-x La x Zr 1-y Ti y O3 (PLZT, 0 < x < 1, 0 < y < 1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnium oxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, Al(OH)3, SiC, AlOOH, TiO2, or a mixture thereof.
[0068] In addition, as the inorganic particles 22, inorganic particles having lithium ion transport ability can be used, that is, inorganic particles 22 containing lithium element and having the function of allowing lithium ions to move without storing lithium. Non-limiting examples of inorganic particles 22 having lithium ion transport ability include lithium phosphate (Li3PO4); lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3); lithium aluminum titanium phosphate (Li x Aly Ti z (PO4)3, where 0 < x < 2, 0 < y < 1, 0 < z < 3); (LiAlTiP) x O y series of glasses (0 < x < 4, 0 < y < 13) such as 14Li2O - 9Al2O3 - 38TiO2 - 39P2O5; lithium lanthanum titanate (Li x La y TiO3, where 0 < x < 2, 0 < y < 3); lithium germanium thiophosphate (Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), such as Li 3.25 Ge 0.25 P 0.75 S4; lithium nitride, such as Li3N (Li x N y , where 0 < x < 4, 0 < y < 2); SiS2 series of glasses (Li x Si y S z , where 0 < x < 3, 0 < y < 2, 0 < z < 4), such as, Li3PO4 - Li2S - SiS2; P2S5 series of glasses (Li x P y S z , where 0 < x < 3, 0 < y < 3, 0 < z < 7), such as LiI - Li2S - P2S5; or a mixture thereof.
[0069] In addition, the inorganic particles 22 are flame - retardant inorganic particles, and inorganic particles capable of providing flame - retardant properties to the separator or preventing a rapid increase in the internal temperature of the electrochemical device can be used. Non - limiting examples of the flame - retardant inorganic particles 22 include Sb2O3, Sb2O4, Sb2O5, SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, Zn2SnO4, ZnSnO3, ZnSn(OH)6, which include ZrO2, Y2O3, SiO2, Al2O3, AlOOH, Al(OH)3, SiC, TiO2, H3BO3, HBO2, and mixtures thereof.
[0070] The average particle size D50 of the inorganic particles 22 may be within a range of 50 nm or more and 5,000 nm or less. Specifically, the average particle size D50 of the inorganic particles 22 may be within a range of 100 nm or more and 4,500 nm or less, 200 nm or more and 4,000 nm or less, 300 nm or more and 3,000 nm or less, 400 nm or more and 2,000 nm or less, or 500 nm or more and 1,000 nm or less. When the average particle size of the inorganic particles 22 is less than 50 nm, an additional polymer binder is required for bonding between the inorganic particles 22 due to an increase in specific surface area, which is disadvantageous in terms of resistance. When the average particle size of the inorganic particles 22 exceeds 5,000 nm, the uniformity of the coating surface may be reduced, and the porous polymer substrate 10 or the electrode may be damaged during lamination.
[0071] The aspect ratio of the inorganic particles 22 may be in the range of 1 or more and 2 or less. Specifically, the aspect ratio of the inorganic particles 22 may be in the range of 1.1 or more and 1.9 or less, 1.2 or more and 1.8 or less, 1.3 or more and 1.7 or less, or 1.4 or more and 1.6 or less. By adjusting the aspect ratio of the inorganic particles 22 within the above range, it is easy to move the polymer binder particles 21 through the pores between the inorganic particles 22, and by forming the film-forming regions F after the polymer binder particles 21 move, a porous coating layer 20 in which the film-forming regions F are uniformly dispersed is formed.
[0072] The BET specific surface area of the inorganic particles 22 can be 5 m 2 / g or more and 25m 2 / g or less. Specifically, the BET specific surface area of the inorganic particles 22 may be within the range of 6m 2 / g or more and 24m 2 / g or less, 7m 2 / g or more and 23m 2 / g or less, 8m 2 / g or more and 22m 2 / g or less, 9m 2 / g or more and 21m 2 / g or less, 10m 2 / g or more and 20m 2 / g or less, 11m 2 / g or more and 19m 2 / g or less, 12m 2 / g or more and 18m 2 / g or less, 13m 2 / g or more and 17m 2 / g or less, or 14m 2 / g or more and 26m 2 By adjusting the BET specific surface area of the inorganic particles 22 within the above range, the movement of the polymer binder particles 21 through the pores between the inorganic particles 22 can be adjusted.
[0073] A specific example of the present disclosure provides a method for manufacturing a separator 1 for an electrochemical device, the method comprising: forming a coating layer including a particle region P formed of polymer binder particles 21 and inorganic particles 22 by coating at least one surface of a porous polymer substrate 10 with a coating slurry including polymer binder particles 21, inorganic particles 22, and a dispersion medium, removing the dispersion medium by drying the coating layer, and forming a film-forming region F by drying the coating layer and varying the amount by 3 wt % to 50 wt % relative to the total weight of the polymer binder particles 21. The contents overlapping with the above contents in the separator for an electrochemical device are replaced with the description of the previous specific example.
[0074] The formation of the coating layer includes coating at least one surface of the porous polymer substrate 10 with a coating slurry containing polymer binder particles 21, inorganic particles 22 and a dispersion medium. For example, the coating layer can be formed by a method such as a rod coater, a wire rod coater, a roller coater, a spray coater, a spin coater, an inkjet coater, a screen coater, a reverse coater, a gravure coater, a blade coater, a slot die coater, a hot melt coater, a comma coater and a direct metering coater, but is not limited thereto. Preferably, the formation of the coating layer can include coating both surfaces of the porous polymer substrate 10 with the coating slurry by using a rod coater or a slot die coater.
[0075] The formation of the coating layer may further include subjecting at least one surface of the porous polymer substrate 10 to a corona discharge treatment. After subjecting the porous polymer substrate 10 to the corona discharge treatment, the method may include coating the porous polymer substrate 10 with the coating slurry. Subjecting at least one surface of the porous polymer substrate 10 to a corona discharge treatment may prevent the bonding strength between the surface of the porous polymer substrate 10 and the surface of the coating layer from decreasing at high temperatures, and prevent the bonding strength between the surface of the porous polymer substrate 10 and the surface of the coating layer from decreasing due to the electrolyte.
[0076] The corona discharge treatment can treat at least one surface of the porous polymer substrate 10 in the air at a voltage of 0.1 kV or more and 10 kV or less. Specifically, the corona discharge treatment can be carried out at a voltage of 0.2 kV or more and 9 kV or less, 0.3 kV or more and 8 kV or less, 0.4 kV or more and 7 kV or less, 0.5 kV or more and 6 kV or less, 0.6 kV or more and 5 kV or less, 0.7 kV or more and 4 kV or less, 0.8 kV or more and 3 kV or less, 0.9 kV or more and 2 kV or less, or 1.0 kV or more and 2 kV or less. Preferably, the corona discharge treatment can be carried out in the air at a voltage of 1.8 kV. By adjusting the applied voltage of the corona discharge treatment within the above range, an appropriate number of functional groups can be formed on the surface of the porous polymer substrate 10, and damage to the surface of the porous polymer substrate 10 can be prevented.
[0077] The removal of the dispersion medium may include evaporating the dispersion medium contained in the coating by drying or heating the coating, and may be referred to as a first heating operation. The first heating operation may be performed at a temperature at which only the dispersion medium contained in the coating may evaporate without deforming the polymer binder particles 21 contained in the coating. For example, the first heating operation may be heating the coating at a predetermined temperature, and the temperature of the coating surface does not exceed 50°C. For example, the coating subjected to the first heating operation may be formed by a particle region P, which is formed by polymer binder particles 21 and inorganic particles 22. When the coating is heated under the above conditions, thermal energy is first used to heat the dispersion medium to change the phase, and may not be used to deform the polymer binder particles 21. The film-forming region P may be formed by removing the dispersion medium and then deforming at least some of the polymer binder particles 21 by a second heating operation to be described below.
[0078] The formation of the film-forming region F may include exposing the coating to a temperature T of the glass transition temperature T of the polymer binder particles 21. g or higher and T g +40°C or lower, and may be referred to as a second heating operation. Specifically, the second heating operation may include heating the polymer binder particles 21 at a temperature of g +5℃ or higher and T g +35℃ or lower, T g +10℃ or higher and T g +30℃ or lower, or T g +15℃ or higher and T g The coating is heated at a temperature of +25°C or lower. Preferably, the second heating operation may include heating the coating at T g +20℃ or higher and T g Heat the coating at +40°C or below.
[0079] The second heating operation may include heating the coating within the above-mentioned temperature range for 1 hour or longer and 24 hours or less. Specifically, the second heating operation may include heating the coating within the above-mentioned temperature range for 2 hours or longer and 23 hours or less, 3 hours or longer and 22 hours or less, 4 hours or longer and 21 hours or less, 5 hours or longer and 20 hours or less, 6 hours or longer and 19 hours or less, 7 hours or longer and 18 hours or less, 8 hours or longer and 17 hours or less, 9 hours or longer and 16 hours or less, 10 hours or longer and 15 hours or less, 11 hours or longer and 14 hours or less, or 12 hours or longer and 13 hours or less. Preferably, the second heating operation may include heating the coating within the above-mentioned temperature range for 6 hours or longer and 24 hours or less. Film forming region F may be formed by deforming polymer binder particles 21 of 3 wt % to 50 wt % relative to the gross weight of polymer binder particles 21 at the above-mentioned temperature or within the temperature and time range. When the heating temperature or time is outside the above range, the film-forming region F is excessively formed or densely formed on any one surface of the porous coating layer 20 , resulting in rapid increases in the air permeability and resistance of the separator 1 .
[0080] The second heating operation may be a single operation performed at a heating temperature within the above range. Alternatively, the second heating operation may be performed in a combination of multiple operations with the same or different heating temperatures and times. For example, the second heating operation may include heating at T g +30℃ or higher and T g Heat the coating at a temperature of +40°C or less for 1 hour or less 2-1 heating operation, at T g +20℃ or higher and T g 2-2 Heating operation for heating the coating at a temperature of +30°C or less for 1 hour or more and 2 hours or less, at T g +10℃ or higher and T g Heating the coating at a temperature of +20°C or less for 2 hours or more and 4 hours or less for 2-3 heating operations, and at T g or higher and T g The coating is heated at a temperature of +10° C. or lower for 4 hours or longer and 8 hours or shorter. Preferably, the aforementioned heating operation may include uniformly forming the film formation region F in the thickness direction of the porous coating 20 by heating the coating at a higher temperature than the subsequent heating operation.
[0081] The polymer binder particles 21 contained in the porous coating layer 20 may not maintain the original shape within the above-mentioned temperature and time range, and may form a film. Because the polymer binder particles 21 may form a film to additionally bind the inorganic particles 22, additionally bind the inorganic particles 22 and the porous polymer substrate 10, or additionally bind the polymer binder particles 21 and the inorganic particles 22 or the polymer binder particles 21 and the porous polymer substrate 10. Therefore, a separator 1 having improved durability of the porous coating layer 20 is provided because the film-forming region F improves the mechanical properties of the porous coating layer 20 while increasing the bonding strength between the porous coating layer 20 and the porous polymer substrate 10.
[0082] The method for manufacturing the separator 1 may further include storing the separator 1 on which the porous coating layer 20 is formed at room temperature or cooling the separator 1 on which the porous coating layer 20 is formed after forming the film-forming region F. The film-forming region F may be placed at a temperature lower than the glass transition temperature of the polymer binder particles 21 to allow the irregularly formed film-forming region F to harden in a state where the above-mentioned additional bonding is formed.
[0083] A specific example of the present disclosure provides a separator for an electrochemical device, the electrochemical device comprising a positive electrode, a negative electrode, and a separator 1 inserted between the positive electrode and the negative electrode, wherein the separator 1 is a separator for an electrochemical device of the above specific example. The electrochemical device can be manufactured by inserting an electrode assembly comprising a positive electrode, a negative electrode, and a separator 1 inserted between the positive electrode and the negative electrode into a housing or a bag and sealing it. Before the housing or bag is sealed, the electrode assembly can be impregnated with an electrolyte by injecting an electrolyte. The shape of the housing or bag is not limited. For example, the electrochemical device can be a cylindrical, prismatic, coin-type or pouch-type lithium secondary battery.
[0084] The positive electrode and the negative electrode can be coated by applying an electrode active material on at least one surface of each current collector and drying. The current collector can be made of a material that has conductivity and does not cause chemical changes in the electrochemical device. For example, the current collector for the positive electrode can be made of aluminum, nickel, titanium, fired carbon, or stainless steel; or it can be a current collector formed by treating the surface of aluminum or stainless steel with carbon, nickel, titanium, silver, etc., but is not limited thereto. For example, the current collector for the negative electrode can be made of copper, nickel, titanium, fired carbon, or stainless steel; or it can be a current collector formed by treating the surface of copper or stainless steel with carbon, nickel, titanium, silver, etc., but is not limited thereto. The current collector can be formed in a variety of forms, such as a thin metal plate, a film, a foil, a mesh, a porous material, or a foam.
[0085] The positive electrode includes a positive electrode current collector and a positive electrode active material layer containing a positive electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The positive electrode active material can be one type or a mixture of two types of the following: layered compounds such as lithium manganese composite oxides (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), or lithium nickel oxide (LiNiO2); or compounds substituted with one or more transition metals; lithium manganese oxides represented by the chemical formula Li 1+x Mn 2-x O4 (where x represents 0 to 0.33), such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, or Cu2V2O7; Ni-site type lithium nickel oxides represented by the chemical formula LiNi 1-x M x O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x = 0.01 to 0.3); lithium manganese composite oxides represented by the chemical formula LiMn 1- x M x O2 (where M = Co, Ni, Fe, Cr, Zn, or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which part of Li in the chemical formula is replaced by alkaline earth metal ions; disulfide compounds; and Fe2(MoO4)3.
[0086] The negative electrode includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode can contain one type or a mixture of two types selected from the following as the negative electrode active material: lithium metal oxides; carbon such as non-graphitized carbon and graphitic carbon; silicon-based materials such as Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Si, SiO x (0 < x < 2), SiC, and Si alloys; metal composite oxides such as Sn x Me 1-x Me’ y O z(Me: Mn, Fe, Pb, Ge, Me', Al, B, P, and Si, elements of Groups 1, 2, and 3 of the periodic table, and halogens, 0 < x ≤ 1, 1 ≤ y ≤ 3, 1 ≤ z ≤ 8); lithium metal; lithium alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, or Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; and titanium oxide.
[0087] The conductive material can be any one selected from the following: graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whisker, conductive metal oxide, carbon nanotube, activated carbon, and polyphenylene derivative, or a mixture of two or more types of conductive materials. The carbon nanotube has a cylindrical shape including graphite sheets with a nanoscale diameter and has a sp 2 bond structure and exhibits conductor or semiconductor characteristics depending on the angle and structure of the wound graphite sheets. The carbon nanotube can be classified into single-walled carbon nanotube (SWCNT), double-walled carbon nanotube (DWCNT), and multi-walled carbon nanotube (MWCNT) according to the number of bonds forming the wall, and the carbon nanotube can be appropriately selected according to the purpose of the dispersion solution. More specifically, the conductive material can be one selected from the following or a mixture of two or more of them: natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide.
[0088] As the binder resin, a polymer resin commonly used for the electrodes of electrochemical devices can be used. Non-limiting examples of the binder resin can include polyvinylidene fluoride-copoly-hexafluoropropylene, polyvinylidene fluoride-copoly-trichloroethylene, polymethyl methacrylate, polyethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-copoly-vinyl acetate, poly(ethylene oxide), polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, etc., but are not limited thereto.
[0089] The electrolyte solution is a salt having the same structure as A + B- dissolved or dissociated in an organic solvent, where A + includes ions composed of alkali metal cations such as Li + , Na + , K + or a combination thereof, and B - includes those containing PF6- 、BF4 - , Cl - Br - ,I - 、ClO4 - 、AsF6 - 、CH3CO2 - CF3SO3 - 、N(CF3SO2)2 - 、C(CF2SO2)3 - or a salt of an anion composed of a combination thereof, the organic solvent is composed of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone (γ-butyrolactone) or a mixture thereof, but is not limited thereto.
[0090] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, as well as a device including a battery module including the unit cell, a battery pack including the battery module, and a device including the battery pack as a power source. The device may include: small devices such as computers, mobile phones, and power tools; electric vehicles that move by receiving power provided by an electric motor, including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc.; electric two-wheeled vehicles, including electric bicycles and electric scooters; electric golf carts, medium and large devices, such as energy storage systems, but not limited thereto.
[0091] Hereinafter, the present disclosure will be described in more detail through specific embodiments and experimental examples. The following embodiments and experimental examples illustrate the present disclosure, and the present disclosure is not limited to the following embodiments and experimental examples.
[0092] Example 1
[0093] Provide coating slurry
[0094] 100 mL of an aqueous dispersion medium was provided by mixing water and isopropyl alcohol at a weight ratio of 95:5 at room temperature (25° C.). 7.7 g of an acrylic polymer binder (styrene-acryl, particle size: 350 nm to 400 nm, T g : 40° C.) and 27.3 g of inorganic particles (Al 2 O 3 , particle size: 400 nm) were added to the aqueous dispersion medium, and stirred for 60 minutes by using an oscillator to prepare a coating slurry in which the polymer binder particles and the inorganic particles were dispersed.
[0095] Provide porous substrate
[0096] As the porous substrate, a polyethylene film (MI: 0.2 g / 10 min, T m : 135°C, porosity: 45%, average pore size: 45 nm, size: 20 cm×30 cm, and thickness: 9 μm).
[0097] Manufacturing of separators
[0098] A porous coating layer each having a thickness of 2 μm was formed by coating both surfaces of a polyethylene film with the coating slurry by using a bar coater.
[0099] The following process was repeated five times: applying a low-temperature air flow to the polyethylene film on which the porous coating layer was formed, drying it (first heating) while adjusting the surface temperature of the porous coating layer not to exceed 50° C., and removing the dispersion medium.
[0100] Subsequently, a separator having a thickness of 13 μm was manufactured by applying a high-temperature air flow of 70° C. to the separator for 24 hours (second heating).
[0101] Example 2
[0102] A separator was manufactured in the same method as in Example 1, except that, in manufacturing the separator, after the dispersion medium was removed, a high-temperature air flow of 80° C. was applied to the separator for 24 hours.
[0103] Example 3
[0104] A separator was manufactured in the same method as in Example 1, except that, in manufacturing the separator, after the dispersion medium was removed, a high-temperature air flow of 70° C. was applied to the separator for 1 hour.
[0105] Example 4
[0106] A separator was manufactured in the same method as in Example 1, except that, in manufacturing the separator, after the dispersion medium was removed, a low-temperature air flow of 40° C. was applied to the separator for 24 hours.
[0107] Comparative Example 1
[0108] The separator was manufactured in the same method as in Example 1, except that, in manufacturing the separator, after the dispersion medium was removed, no additional high-temperature gas flow was applied to the separator.
[0109] Comparative Example 2
[0110] A separator was manufactured in the same method as in Example 1, except that, in manufacturing the separator, after the dispersion medium was removed, a high-temperature air flow of 80° C. was applied to the separator for 48 hours.
[0111] Comparative Example 3
[0112] A separator was manufactured in the same method as in Example 1, except that, in manufacturing the separator, after the dispersion medium was removed, a high-temperature air flow of 90° C. was applied to the separator for 24 hours.
[0113] Experimental Example 1. Testing the durability of porous coating
[0114] The separators of Example and Comparative Example were each placed on a surface property tester model 14FW device of Heidon, a 5 g / dia tip was attached to the device as an accessory, and then the end of the diamond tip was inserted at a depth of 1 μm into the porous coating layer of the separator.
[0115] Thereafter, by reciprocating the diamond tip at a speed of 100 mm / min to generate repeated friction, the static friction coefficient was measured at the moment when the diamond tip started to move, and the first dynamic friction coefficient was measured during the first reciprocating movement. While reciprocating, the number of reciprocating movements required until the porous coating was peeled off from the porous polymer substrate was counted. The measured friction coefficients and the number of reciprocating movements required for the peeling time point are shown in Table 1 below.
[0116] Experimental Example 2. Testing the physical properties of the separator
[0117] Measurement of peel strength
[0118] The test samples were provided by sampling each separator to a width of 20 mm and attaching it to a glass slide by using a double-sided tape (3M) having a width of 18 mm.
[0119] The peel strength was measured by separating the glass slide from the separator at a speed of 300 mm / min in a direction of 180° relative to the bonding direction by using UTM.
[0120] Measurement of electrode-separator adhesion strength
[0121] The negative electrode was manufactured by mixing a negative electrode active material (natural graphite and artificial graphite in a weight ratio of (5:5)), a conductive material (super P), and a binder (polyvinylidene fluoride (PVdF)) in a weight ratio of 92:2:6, dispersing them in water, and then coating them on a copper foil.
[0122] An electrode adhesive strength test sample was manufactured by sampling the separators and negative electrodes of Examples and Comparative Examples at a width of 20 mm, overlapping them, and then pressing them at 60° C. under a pressure of 6.5 MPa for 1 second.
[0123] The electrode adhesion strength of the separator was measured by separating the negative electrode from the separator at a speed of 300 mm / min in a direction of 180° with respect to the bonding direction by using UTM.
[0124] Air permeability measurement
[0125] For air permeability, the diameter of air permeation of 100cc was measured by using a Gurley densometer (Gurley, 4110N) with an area of 645mm and a diameter of 28.6mm. 2 The time required for the separators.
[0126] Resistance measurement
[0127] Regarding the resistance, after manufacturing a 2016-size coin cell by using the separators of the example and the comparative example and then leaving it for 3 hours, the resistance of the coin cell was measured by using an EIS (Electrochemical Impedance Spectroscopy) apparatus.
[0128] As the electrolyte of the coin cell, a drop of an electrolyte containing 3 mol of vinylene carbonate (VC), 1.5 mol of propane sultone (PS), 1 mol of ethylene sulfate (ESa) and 1 mol of lithium salt LiPF6 as an additive in a solvent mixed with ethylene carbonate (EC) / ethyl methyl carbonate (EMC) in a ratio of 3 / 7 is used.
[0129] [Table 1]
[0130]
[0131] [Explanation of Reference Numerals]
[0132] 1: separator 10: porous polymer substrate 20: porous coating layer 21: polymer binder particles 22: inorganic particles P: particle region F: film formation region T: diamond tip.
Claims
1. A separator for an electrochemical device, include: a porous polymer substrate; and a porous coating layer comprising a particle region formed of polymer binder particles and inorganic particles and a film-forming region comprising deformed polymer binder particles, and formed on at least any one surface of the porous polymer substrate, The film-forming region is in the range of 3 wt % to 50 wt % relative to the total weight of the polymer binder particles.
2. The separator according to claim 1, in, When the end of the diamond tip is disposed in a region between a surface of the porous coating layer contacting the porous polymer substrate and an opposite surface facing the surface, and the diamond tip is moved in a direction parallel to the porous polymer substrate at a speed of 100 mm / min, a first dynamic friction coefficient caused by friction loss is in the range of 1 to 2.
3. The separator according to claim 1, in, When the end of the diamond tip is disposed in a region between a surface of the porous coating layer contacting the porous polymer substrate and an opposite surface facing the surface, and the diamond tip is moved in a direction parallel to the porous polymer substrate at a speed of 100 mm / min, the difference between the static friction coefficient caused by friction loss and the first dynamic friction coefficient is 3 or less.
4. The separator according to claim 1, wherein the bonding strength between the porous polymer substrate and the porous coating layer is in the range of 1.5 to 6 times the bonding strength exhibited by the opposite surface of the porous coating layer facing the surface contacting the porous polymer substrate.
5. The separator according to claim 1, wherein the polymer binder particles comprise one or more selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethylhexyl acrylate, methyl methacrylate, styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber.
6. The separator according to claim 1, wherein the film-forming region is formed by exposing the polymer binder particles to a temperature below the glass transition temperature (T g ) to T g Formed at temperatures in the range of +40°C.
7. An electrochemical device comprising a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, The separator is a separator for an electrochemical device according to any one of claims 1 to 6.
8. A method for manufacturing a separator for an electrochemical device, include: forming a coating layer including a particle region formed of the polymer binder particles and the inorganic particles by coating at least one surface of a porous polymer substrate with a coating slurry comprising polymer binder particles, inorganic particles, and a dispersion medium; removing the dispersion medium by drying the coating; as well as The film-forming region is formed by deforming 3 wt % to 50 wt % relative to the total weight of the polymer binder particles by drying the coating layer.
9. The method of claim 8, wherein the removing of the dispersion medium comprises preventing the surface of the coating from exceeding 50°C.
10. The method of claim 8, wherein the formation of the film-forming region comprises exposing the coating to a temperature below the glass transition temperature (T g ) to T g Temperatures in the range of +40°C for 24 hours or less.
Citation Information
Cited By
Separator, method of manufacturing the same, and electrode assembly comprising the same
EP4776418A1