Rubber composition for golf balls and golf balls using the same

A golf ball core composition using a base rubber, α,β-unsaturated carboxylic acid, and a crosslinking initiator addresses durability issues, enhancing resilience and shot feel through optimized crosslink density.

JP7581656B2Active Publication Date: 2024-11-13SUMITOMO RUBBER INDUSTRIES LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020086932
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-31
Filing Date
2020-05-18
Publication Date
2024-11-13
Estimated Expiration
2040-05-18

AI Technical Summary

Technical Problem

Existing golf ball rubber compositions do not provide sufficient durability, leading to reduced resilience and poor shot feel.

Method used

A rubber composition for golf ball cores comprising a base rubber, an α,β-unsaturated carboxylic acid or its metal salt as a co-crosslinking agent, and a crosslinking initiator, formulated to satisfy the equation Y < 0.1 × X - 1.30, where Y is the effective crosslink density and X is the amount of the co-crosslinking agent, enhancing durability and resilience.

Benefits of technology

The composition achieves improved durability and resilience in golf balls, ensuring better shot feel and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581656000020
    Figure 0007581656000020
  • Figure 0007581656000001
    Figure 0007581656000001
  • Figure 0007581656000002
    Figure 0007581656000002
Patent Text Reader

Abstract

To provide a cured product of a golf ball rubber composition imparting excellent durability.SOLUTION: The present invention provides a cured product of a golf ball rubber composition, which is cured from a golf ball rubber composition containing (a) a base rubber, (b) an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or a metal salt thereof as a co-crosslinking agent, and (c) a crosslinking initiator, wherein the cured product of the golf ball rubber composition satisfies the following mathematical formula (1): Y<0.1×X-1.30 in the formula (1), Y represents an effective crosslinking density of the cured product of the rubber composition (mmol / cc), and X represents an amount of the component (b) with respect to 100 pts.mass of (a) the base rubber (pts.mass).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for a golf ball, and more particularly to an improvement in a rubber composition for a core of a golf ball. [Background technology]

[0002] As a material for forming the core of a golf ball, a rubber composition containing a base rubber, a co-crosslinking agent, and a crosslinking initiator is widely used because of its good resilience.

[0003] For example, Patent Document 1 discloses a golf ball having a core and at least one cover layer, in which the cross-sectional hardness of the core is expressed by the following formulas (1) to (4): R (mm) is the radius of the core, A is the JIS-C hardness at the center of the core, B is the JIS-C hardness at a position R / 3 mm away from the center of the core, C is the JIS-C hardness at a position R / 1.8 mm away from the center of the core, D is the JIS-C hardness at a position R / 1.3 mm away from the center of the core, and E is the JIS-C hardness of the surface of the core. (1) DC ≥ 7 (2)CB≦7 (3)(DC)-(CB)≧7 (4) EA≧16 A golf ball characterized by satisfying the following is disclosed.

[0004] Patent Document 2 also describes a golf ball having a core and a cover of one or more layers, the core comprising the following components (A) to (C): (A) Base rubber (B) Organic peroxide (C) Water and / or a metal monocarboxylate The rubber composition is formed by hot molding the rubber composition, The difference in crosslink density between the core surface and the core center, P (mol / m 3 ) and the deflection E (mm) of the core from the initial load of 98N (10kgf) to the final load of 1275N (130kgf) is 28×102 mol / m 3 .mm or more.

[0005] Patent Document 3 discloses a one-piece golf ball comprising a ball body made of a white rubber composition containing a base rubber, an α,β-unsaturated carboxylic acid and / or a metal salt thereof, and an organic peroxide, and a clear coat applied to the surface of the ball body, wherein the white rubber composition is a rubber composition containing 0.1 to 5.0 parts by mass of an antioxidant and 0.05 to 3.0 parts by mass of a light stabilizer per 100 parts by mass of the base rubber, and the clear coat contains 0.05 to 5.0 parts by mass of an ultraviolet absorbing agent per 100 parts by mass of a resin component.

[0006] Patent Document 4 describes a polymer that contains 60% by weight or more of cis-1,4-bonds and has a Mooney viscosity (ML 1+4 The present invention discloses a golf ball characterized in that the ball comprises, as a component, a hot-molded product of a rubber composition that contains polybutadiene having a modulus of elasticity (100°C) of 40 or more, an unsaturated carboxylic acid and / or a metal salt thereof, an organic peroxide, and a monophenol-based antioxidant.

[0007] Patent Document 5 discloses a solid golf ball having at least a part of an elastic portion formed from a rubber composition containing a base rubber, a metal salt of an α,β-ethylenically unsaturated carboxylic acid, an ethylenically unsaturated carboxylic acid ester having a hindered phenol group, and a peroxide.

[0008] Patent Document 6 describes the following components (A) to (E): (A) a modified polybutadiene having a vinyl content of 0 to 2% and a cis-1,4-bond content of 80% or more and having an active terminal, the active terminal of which is modified with at least one alkoxysilane compound, in an amount of 1 to 50% by mass based on the total amount of the rubber component; (B) The polybutadiene synthesized using a rare earth element catalyst having a stress relaxation time (T80) of less than 4.0 is 50% by mass or more of the total rubber component, and Relative to 100 parts by mass of the total amount of the above components (A) and (B), (C) 10 to 50 parts by mass of an unsaturated carboxylic acid and / or a metal salt thereof, (D) 5 to 80 parts by mass of an inorganic filler, and (E) 0.1 to 10 parts by mass of organic peroxide The present invention discloses a golf ball comprising, as a constituent element, a hot-molded product of a rubber composition containing the above as an essential component.

[0009] Patent Document 7 describes the following components (A) to (E): (A) 1 to 30 mass % of the total rubber component of a modified polybutadiene having a vinyl content of 0 to 2% and a cis-1,4-bond content of 80% or more and having an active terminal, the active terminal being modified with at least one alkoxysilane compound and having a Mooney viscosity of 40 or more; (B) The diene rubber having a Mooney viscosity of less than 50 other than the rubber component (A) accounts for 70 mass % or more of the total rubber component, and For 100 parts by mass of the total amount of the above components (A) and (B), (C) 10 to 50 parts by mass of an unsaturated carboxylic acid and / or a metal salt thereof, (D) 5 to 80 parts by mass of an inorganic filler, and (E) 0.1 to 10 parts by mass of organic peroxide The present invention discloses a golf ball comprising, as a constituent element, a hot-molded product of a rubber composition containing the above as an essential component.

[0010] Patent Document 8 discloses a golf ball characterized in that the ball comprises, as a constituent element, a product molded by heating from a rubber composition containing the following components (A) to (E) as essential components: (A) Modified polybutadiene having a vinyl content of 0 to 2% and a cis-1,4-bond content of 80% or more and having an active terminal, the active terminal being modified with at least one alkoxysilane compound and having a Mooney viscosity of less than 40: 1% by mass or more and less than 30% by mass; (B) diene rubber other than the rubber component (A): 70% by mass or more, For 100 parts by mass of the total amount of the above components (A) and (B), (C) Unsaturated carboxylic acid and / or metal salt thereof: 10 to 50 parts by mass (D) inorganic filler: 5 to 80 parts by mass, and (E) Organic peroxide: 0.1 to 10 parts by mass [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2015-077405 A [Patent Document 2] JP 2015-47502 A [Patent Document 3] JP 2001-149504 A [Patent Document 4] JP 2004-121815 A [Patent Document 5] Japanese Patent Application Publication No. 63-212377 [Patent Document 6] JP 2009-119253 A [Patent Document 7] JP 2009-119254 A [Patent Document 8] JP 2009-112806 A Summary of the Invention [Problem to be solved by the invention]

[0012] An object of the present invention is to provide a rubber composition for a golf ball that imparts excellent durability to the golf ball. The present invention further provides a golf ball having excellent durability. [Means for solving the problem]

[0013] The cured product of the rubber composition for golf balls of the present invention is obtained by curing a rubber composition for golf balls that contains (a) a base rubber, (b) an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or a metal salt thereof as a co-crosslinking agent, and (c) a crosslinking initiator, and is characterized in that it satisfies the following mathematical formula (1): Y<0.1×X-1.30 (1) In formula (1), Y: effective crosslink density (mmol / cc) of the cured rubber composition X: Amount (parts by mass) of component (b) per 100 parts by mass of base rubber (a) Effect of the Invention

[0014] According to the present invention, it is possible to provide a rubber composition for a golf ball that imparts excellent durability. According to the present invention, it is possible to provide a golf ball having excellent durability. [Brief description of the drawings]

[0015] [Figure 1] 1 is a partially cutaway cross-sectional view showing a golf ball according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The cured product of the rubber composition for golf balls of the present invention is obtained by curing a rubber composition for golf balls that contains (a) a base rubber, (b) an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or a metal salt thereof as a co-crosslinking agent, and (c) a crosslinking initiator, and is characterized in that it satisfies the following mathematical formula (1): Y<0.1×X-1.30 (1) In formula (1), Y: effective crosslink density (mmol / cc) of the cured rubber composition X: Amount (parts by mass) of component (b) per 100 parts by mass of base rubber (a)

[0017] The rubber composition for golf balls of the present invention satisfies the following mathematical formula (1), more preferably satisfies the following mathematical formula (2), and even more preferably satisfies the following mathematical formula (3). By satisfying mathematical formula (1), a rubber composition for golf balls having excellent durability can be obtained. Y<0.1×X-1.30 (1) Y<0.1×X-1.50 (2) Y<0.1×X-2.00 (3) In formulas (1), (2), and (3), Y is the effective crosslink density (mmol / cc) of the cured product of the rubber composition, and X is the amount (parts by mass) of component (b) per 100 parts by mass of base rubber (a).

[0018] The cured product of the rubber composition for measuring the effective crosslink density is preferably in a state where vulcanization is almost completed (where the crosslink density is at its maximum). Specifically, it is preferable that the cured product of the rubber composition is vulcanized for 30 minutes or more at a temperature within the 1-minute half-life temperature of the crosslinking initiator ±10°C.

[0019] The particle surface of the α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or its metal salt used as the co-crosslinking agent (b) may be treated with stearic acid or zinc stearate. In such a case, the amount excluding the treating agent such as stearic acid or zinc stearate is defined as the blending amount X of the (b) component.

[0020] The slab hardness of the cured product of the rubber composition for golf balls of the present invention is preferably 50 or more, more preferably 60 or more, and even more preferably 65 or more, in Shore C hardness, and is preferably 95 or less, more preferably 90 or less, and even more preferably 85 or less.

[0021] The materials contained in the rubber composition for golf balls of the present invention will be described below.

[0022] [(a) Base rubber] As the base rubber (a), natural rubber and / or synthetic rubber can be used, for example, polybutadiene rubber, natural rubber, polyisoprene rubber, styrene polybutadiene rubber, ethylene-propylene-diene rubber (EPDM), etc. These may be used alone or in combination of two or more. Among these, high cis polybutadiene having cis-1,4-bonds, which are advantageous in terms of resilience, in an amount of 40% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more is particularly suitable.

[0023] In order to obtain a core with higher resilience, the content of high-cis polybutadiene in the base rubber is preferably at least 60 mass%, more preferably at least 80 mass%, and even more preferably at least 90 mass%. It is also preferable that the (a) base rubber consists solely of high-cis polybutadiene.

[0024] The high-cis polybutadiene preferably has a 1,2-vinyl bond content of 2.0% by mass or less, more preferably 1.7% by mass or less, and further preferably 1.5% by mass or less. If the 1,2-vinyl bond content is too high, the resilience may decrease.

[0025] The high-cis polybutadiene is preferably one synthesized using a rare earth element catalyst. In particular, the use of a neodymium-based catalyst using a neodymium compound, which is a lanthanum series rare earth element compound, is preferred because it can produce a polybutadiene rubber having a high content of 1,4-cis bonds and a low content of 1,2-vinyl bonds with excellent polymerization activity.

[0026] The high cis polybutadiene has a Mooney viscosity (ML 1+4 (100°C)) is preferably 30 or more, more preferably 32 or more, even more preferably 35 or more, and is preferably 140 or less, more preferably 120 or less, even more preferably 100 or less, and most preferably 55 or less. The Mooney viscosity (ML 1+4(100°C) is a value measured in accordance with JIS K6300 using an L rotor with a preheating time of 1 minute, rotor rotation time of 4 minutes, and at 100°C.

[0027] The high cis polybutadiene preferably has a molecular weight distribution Mw / Mn (Mw: weight average molecular weight, Mn: number average molecular weight) of 2.0 or more, more preferably 2.2 or more, even more preferably 2.4 or more, most preferably 2.6 or more, and preferably 6.0 or less, more preferably 5.0 or less, even more preferably 4.0 or less, and most preferably 3.0 or less. If the molecular weight distribution (Mw / Mn) of the high cis polybutadiene is too small, the workability may decrease, and if it is too large, the resilience may decrease. The molecular weight distribution is measured by gel permeation chromatography (manufactured by Tosoh Corporation, "HLC-8120GPC") using a differential refractometer as a detector under the conditions of column: GMHHXL (manufactured by Tosoh Corporation), column temperature: 40°C, and mobile phase: tetrahydrofuran, and calculated as a standard polystyrene equivalent value.

[0028] [(b) Co-crosslinking agent] The (b) α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or its metal salt used in the rubber composition is blended into the rubber composition as a co-crosslinking agent, and has the effect of crosslinking rubber molecules by graft polymerization with base rubber molecular chains.

[0029] Examples of the α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms include acrylic acid, methacrylic acid, fumaric acid, maleic acid, and crotonic acid.

[0030] Examples of the metal constituting the metal salt of the α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms include monovalent metal ions such as sodium, potassium, and lithium; divalent metal ions such as magnesium, calcium, zinc, barium, and cadmium; trivalent metal ions such as aluminum; and other ions such as tin and zirconium. The metal components can be used alone or in a mixture of two or more kinds. Among these, divalent metals such as magnesium, calcium, zinc, barium, and cadmium are preferable as the metal components. This is because the use of a divalent metal salt of an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms facilitates the formation of metal crosslinks between rubber molecules. In particular, zinc acrylate is preferable as the divalent metal salt because it increases the resilience of the resulting golf ball. The α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or its metal salt may be used alone or in combination of two or more kinds.

[0031] The content of the (b) α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or its metal salt is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and preferably 55 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 45 parts by mass or less, per 100 parts by mass of the (a) base rubber. If the content of the (b) α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or its metal salt is less than 20 parts by mass, the amount of the (c) crosslinking initiator described below must be increased in order to provide an appropriate hardness to the cured product (e.g., core) formed from the rubber composition, and the resilience of the resulting golf ball tends to decrease. On the other hand, if the content of the α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or its metal salt exceeds 55 parts by mass, the cured product (e.g., core) formed from the rubber composition may become too hard, and the shot feeling of the resulting golf ball may decrease.

[0032] [(c) Crosslinking initiator] The (c) crosslinking initiator used in the rubber composition is compounded to crosslink the (a) base rubber component. As the (c) crosslinking initiator, an organic peroxide is suitable. Specific examples of the organic peroxide include dicumyl peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and di-t-butyl peroxide. These organic peroxides may be used alone or in combination of two or more. Among these, dicumyl peroxide is preferably used.

[0033] When the rubber composition contains at least one of the following components (d) and (e), the content of the crosslinking initiator (c) is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.7 parts by mass or more, and preferably 5.0 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less, per 100 parts by mass of the base rubber (a). If the content of the crosslinking initiator is less than 0.2 parts by mass, the cured product (e.g., core) formed from the rubber composition tends to be too soft, and the resilience of the resulting golf ball tends to decrease, whereas if the content exceeds 5.0 parts by mass, the amount of the co-crosslinking agent (b) described above must be reduced in order to give the cured product (e.g., core) formed from the rubber composition an appropriate hardness, and the resulting golf ball may have insufficient resilience or poor durability.

[0034] When the rubber composition does not contain either of the following components (d) and (e), it is also preferable to set the content of the crosslinking initiator (c) to 0.1 parts by mass or less per 100 parts by mass of the base rubber. By setting the content of the crosslinking initiator (c) to 0.1 parts by mass or less per 100 parts by mass of the base rubber, the effective crosslinking density becomes low relative to the amount of co-crosslinking agent added, the breaking strain increases, and durability is improved.

[0035] The rubber composition for golf balls of the present invention preferably contains a radical scavenger (d). Examples of the radical scavenger (d) include a hindered phenol compound (d1) and a hindered amine compound (d2). When the rubber composition for golf balls contains the component (d), the crosslink density can be reduced while maintaining the hardness of the cured product.

[0036] [(d1) Hindered phenol compounds] The hindered phenol compound is a compound having a hydroxyphenyl structure in which a hydroxy group is sterically protected by a bulky functional group. The bulky functional group is preferably present at a position adjacent to the hydroxy group. Examples of the bulky functional group include a t-butyl group and a long-chain alkyl group in which a part of the carbon number may be substituted with sulfur. As the hindered phenol compound, a compound having a tert-butylhydroxyphenyl structure having at least one tert-butyl group is preferred, and a compound having a di-tert-butylhydroxyphenyl structure having two tert-butyl groups is more preferred.

[0037] Examples of the compound having a tert-butylhydroxyphenyl structure having at least one tert-butyl group include compounds having a structure such as 3-tert-butyl-4-hydroxyphenyl or 3,5-di-tert-butyl-4-hydroxyphenyl. Among these, compounds having a 3,5-di-tert-butyl-4-hydroxyphenyl structure are preferred.

[0038] Specific examples of the hindered phenol compounds include compounds having one hydroxyphenyl structure, such as dibutylhydroxytoluene (BHT), 4,6-bis(octylthiomethyl)-o-cresol, 4,6-bis[(dodecylthio)methyl]-o-cresol, 2,4-dimethyl-6-(1-methylpentadecyl)phenol (e.g., Irganox 1141 manufactured by BASF Japan Ltd.), and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (e.g., Adeka STAB AO-50 manufactured by Adeka Corporation).

[0039] Other specific examples of the hindered phenol compound include 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) (e.g., Yoshinox 425 manufactured by Mitsubishi Chemical Corporation), 2,2'-methylenebis(4-methyl-6-tert-butylphenol) (e.g., Sandant 2246 manufactured by Sanshin Chemical Industry Co., Ltd.), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol) (e.g., Yoshinox BB manufactured by Mitsubishi Chemical Corporation), 4,4'-thiobis(3-methyl-6-tert-butylphenol) (e.g., Knocklac 300 manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 4,4 Examples of the compound having two hydroxyphenyl structures include 2,6-di-tert-butylphenol), 2,6-di-tert-butyl-4-({2-[(3,5-di-tert-butyl-4-hydroxyphenyl)sulfanyl]propan-2-yl}sulfanyl)phenol (probucol), and 3,9-bis[2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane (e.g., Adeka STAB AO-80 manufactured by Adeka Corporation).

[0040] Other specific examples of the hindered phenol compound include compounds having three hydroxyphenyl structures, such as 1,3,5-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3-5-triazine-2,4,6(1H,3H,5H-)-trione (e.g., Adeka STAB AO-20 manufactured by Adeka Corporation) and 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene (e.g., Adeka STAB AO330 manufactured by Adeka Corporation).

[0041] Another specific example of the hindered phenol compound is a compound having four hydroxyphenyl structures, such as pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (e.g., Adeka STAB AO-60 manufactured by Adeka Corporation).

[0042] The hindered phenol compounds may be used alone or in combination of two or more kinds.

[0043] The hindered phenol compound is preferably at least one compound selected from the group consisting of dibutylhydroxytoluene (3,5-di-tert-butyl-4-hydroxytoluene), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,6-di-tert-butyl-4-({2-[(3,5-di-tert-butyl-4-hydroxyphenyl)sulfanyl]propan-2-yl}sulfanyl)phenol, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.

[0044] As the (d2) hindered amine compound, a compound having a 2,2,6,6-tetramethyl-4-piperidyl group as represented by the following chemical formula (1) is preferable. [ka] In formula (1), R 11 is a hydrogen atom, a hydroxy group, an alkyl group having 1 to 30 carbon atoms, a hydroxyalkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a hydroxyalkoxy group having 1 to 30 carbon atoms, or an oxy radical.

[0045] The hindered amine compound represented by chemical formula (1) includes hindered amine compounds represented by chemical formula (2) or chemical formula (3).

[0046] The hindered amine compound represented by the following chemical formula (2) is what is called an N-alkyl type hindered amine compound or an NH type hindered amine compound. [ka] In formula (2), R 12 is a hydrogen atom, a hydroxy group, an alkyl group having 1 to 30 carbon atoms, a hydroxyalkyl group having 1 to 30 carbon atoms, or an oxy radical.

[0047] The hindered amine compound represented by the following chemical formula (3) is what is called an N-alkoxy type hindered amine compound. [ka] In chemical formula (3), R 12 is an alkyl group having 1 to 30 carbon atoms or a hydroxyalkyl group having 1 to 30 carbon atoms.

[0048] Specific examples of the (d2) hindered amine compound include compounds represented by chemical formulas (4) and (5). [ka] In chemical formula (4), R 13 R is an alkylene group having 1 to 30 carbon atoms. 14 , R 15 are each independently a hydrogen atom, a hydroxy group, an alkyl group having 1 to 30 carbon atoms, a hydroxyalkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a hydroxyalkoxy group having 1 to 30 carbon atoms, or an oxy radical.

[0049] [ka] In chemical formula (5), R 16 R is a hydrogen atom, a hydroxy group, an alkyl group having 1 to 30 carbon atoms, a hydroxyalkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a hydroxyalkoxy group having 1 to 30 carbon atoms, or an oxy radical. 17 is an alkyl group having 1 to 30 carbon atoms or an alkenyl group having 2 to 30 carbon atoms.

[0050] [ka] In chemical formula (6), R 18 , R 19 are each independently a hydrogen atom, a hydroxy group, an alkyl group having 1 to 30 carbon atoms, a hydroxyalkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a hydroxyalkoxy group having 1 to 30 carbon atoms, or an oxy radical.

[0051] (d2) Specific examples of the hindered amine compound include Adeka STAB LA-52 (tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate), Adeka STAB LA-57 (tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate), and Adeka STAB L, both manufactured by Adeka Corporation. A-63P, ADK STAB LA-68, ADK STAB LA-72 (bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, ADK STAB LA-77Y (bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, ADK STAB LA-81 (bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate), and the like.

[0052] (d2) Specific examples of the hindered amine compound include the following, which are commercially available from BASF Japan Ltd. 1) Chimassorb 2020FDL 1,6-Hexanediamine, N,N'―bis(2,2,6,6-tetramethyl-4-piperidinyl)-polymer with 2,4,6-trichloro-1,3,5-triazine, reaction products with N-butyl-1-butanamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine 2) Chimassorb 944FDL Poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]]) 3) Tinubin 622SF Butanedioic acid, dimethylester, polymer with 4-hydroxy-2,2,6,6- tetramethyl-1-piperidine ethanol), 4) Tinuvin PA144 Bis(1,2,2,6,6-pentamethyl-4-piperidinyl)-2-butyl-2-(4-hydroxy-3,5-di-tert.-butylbenzyl)propanedioate

[0053] The hindered amine compound (d2) may be used alone or in combination of two or more kinds. Also, the hindered phenol compound (d1) and the hindered amine compound (d2) may be used in combination.

[0054] (d) The amount of the radical scavenger is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of the base rubber (a). This is because, when the amount of the radical scavenger (d) is within the above range, the effective crosslink density is low relative to the amount of co-crosslinking agent added, the breaking strain is increased, and durability is improved.

[0055] [(e) Terpene resin] The rubber composition for golf balls of the present invention also preferably contains a terpene resin. When the rubber composition for golf balls contains component (e), the crosslink density can be reduced while maintaining the hardness of the cured product. The terpene resin is not particularly limited as long as it is a polymer containing a terpene compound as a constituent component. The terpene resin is preferably at least one selected from the group consisting of, for example, terpene polymers, terpene-phenol copolymers, terpene-styrene copolymers, terpene-phenol-styrene copolymers, hydrogenated terpene-phenol copolymers, hydrogenated terpene-styrene copolymers, and hydrogenated terpene-phenol-styrene copolymers.

[0056] The terpene polymer is a homopolymer obtained by polymerizing a terpene compound. The terpene compound is (C5H8) n The hydrocarbons and their oxygen-containing derivatives represented by the composition 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32 ) are compounds having a basic skeleton of terpene classified as one of the following compounds. Examples of the terpene compounds include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, γ-terpineol, and the like. The terpene compounds can be used alone or in combination of two or more kinds.

[0057] The terpene polymer can be obtained by, for example, polymerizing the terpene compound. Examples of the terpene polymer include an α-pinene polymer, a β-pinene polymer, a limonene polymer, a dipentene polymer, and a β-pinene / limonene polymer.

[0058] Terpene-phenol copolymers (sometimes referred to as "terpene phenol resins") are, for example, copolymers of the above-mentioned terpene compounds and phenolic compounds. Examples of the above-mentioned phenolic compounds include phenol, cresol, xylenol, catechol, resorcinol, hydroquinone, and bisphenol A. As the terpene-phenol copolymers, copolymers of terpene compounds and phenols are preferred.

[0059] The acid value of the terpene-phenol copolymer is preferably 10 mgKOH / g or more, more preferably 35 mgKOH / g or more, and even more preferably 60 mgKOH / g or more. The acid value of the terpene-phenol copolymer is preferably 300 mgKOH / g or less, more preferably 250 mgKOH / g or less, even more preferably 200 mgKOH / g or less, particularly preferably 150 mgKOH / g or less, and most preferably 90 mgKOH / g or less. In the present invention, the acid value of the terpene-phenol copolymer is the amount of potassium hydroxide required to neutralize the acid contained in 1 g of the terpene-phenol copolymer, expressed in milligrams, and is a value measured by potentiometric titration (JIS K 0070:1992).

[0060] The hydroxyl value of the terpene-phenol copolymer is preferably 30 mgKOH / g or more, more preferably 50 mgKOH / g or more. The hydroxyl value of the terpene-phenol copolymer is preferably 150 mgKOH / g or less, more preferably 100 mgKOH / g or less. In this specification, the hydroxyl value is the amount of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl group when acetylating 1 g of resin, expressed in milligrams, and is a value measured by potentiometric titration (JIS K 0070:1992).

[0061] The terpene-styrene copolymer is, for example, a copolymer of the terpene compound and a styrene-based compound. Examples of the styrene-based compound include styrene and α-methylstyrene. The terpene-styrene copolymer is preferably a copolymer of the terpene compound and α-methylstyrene.

[0062] The terpene-phenol-styrene copolymer is, for example, a copolymer of the terpene compound, the phenolic compound, and the styrene compound. The terpene-phenol-styrene copolymer is preferably a copolymer of the terpene compound, phenol, and α-methylstyrene.

[0063] A hydrogenated terpene-phenol copolymer is obtained by hydrogenating the terpene-phenol copolymer. A hydrogenated terpene-styrene copolymer is obtained by hydrogenating the terpene-styrene copolymer. A hydrogenated terpene-phenol-styrene copolymer is obtained by hydrogenating the terpene-phenol-styrene copolymer.

[0064] (e) The terpene resin is preferably at least one selected from the compounds having structures represented by the following chemical formulas (7) to (10).

[0065] [ka]

[0066] [ka]

[0067] [ka]

[0068] [ka]

[0069] [In chemical formulas (7) to (10), R 1 and R 2 each independently represents a divalent residue of a phenolic compound and / or a styrene compound; m 1 ~m 4 Each independently represents a natural number from 1 to 30, 1 ~n 2 each independently represents a natural number from 1 to 20.

[0070] The compounds having the structures represented by the above chemical formulas (7) to (10) all have a structure derived from pinene in the molecule.

[0071] A compound having a structure represented by chemical formula (7) is a compound having a structural portion derived from α-pinene and R bonded to the structural portion derived from α-pinene. 1 R 1 is preferably a divalent residue in which two hydrogen atoms have been removed from the benzene ring of a phenolic compound and / or a styrene compound. Examples of compounds having a structure represented by chemical formula (7) include copolymers of α-pinene and a phenolic compound and / or a styrene compound.

[0072] Examples of the phenol-based compounds include phenol, cresol, xylenol, catechol, resorcin, hydroquinone, and bisphenol A. Examples of the styrene-based compounds include styrene and α-methylstyrene.

[0073] In chemical formula (7), m 1 represents the degree of polymerization of the structural unit derived from α-pinene, and is preferably a natural number of 1 to 30. 1 is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more; and is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less.

[0074] In chemical formula (7), n 1 is a structural part derived from α-pinene and R bound to this structural part derived from α-pinene. 1 It is preferable that n is a natural number of 1 to 20. 1 is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more; and is preferably 20 or less, more preferably 18 or less, and even more preferably 15 or less.

[0075] A compound having a structure represented by chemical formula (8) has a structural part derived from β-pinene in the molecule and R bonded to this structural part. 2 The compound having the structure represented by chemical formula (8) is, for example, a copolymer of β-pinene with a phenolic compound and / or a styrene compound. 2 is a divalent residue formed by removing two hydrogen atoms from the benzene ring of a phenolic compound and / or a styrene compound.

[0076] Examples of the phenol-based compounds include phenol, cresol, xylenol, catechol, resorcin, hydroquinone, and bisphenol A. Examples of the styrene-based compounds include styrene and α-methylstyrene.

[0077] In chemical formula (8), m 2 represents the degree of polymerization of the structural unit derived from β-pinene, and is preferably a natural number of 1 to 30. 2 is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more; and is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less.

[0078] In chemical formula (8), n 2 is a structural part derived from β-pinene and R bound to this structural part. 2 It is preferable that n is a natural number of 1 to 20. 2 is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more; and is preferably 20 or less, more preferably 18 or less, and even more preferably 15 or less.

[0079] The compound having a structure represented by chemical formula (9) is a polymer having structural units derived from α-pinene, and more preferably a polymer having only structural units derived from α-pinene.

[0080] In chemical formula (9), m 3represents the degree of polymerization of the structural unit derived from α-pinene, and is preferably a natural number of 1 to 30. 3 is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more; and is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less.

[0081] The compound having a structure represented by chemical formula (10) is a β-pinene polymer having structural units derived from β-pinene in the molecule, and more preferably a polymer having only structural units derived from β-pinene.

[0082] In chemical formula (10), m 4 represents the degree of polymerization of the structural unit derived from β-pinene, and is preferably a natural number of 1 to 30. 4 is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more; and is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less.

[0083] Particularly preferred examples of the terpene resin (e) include α-pinene-phenol copolymer, α-pinene-α-methylstyrene copolymer, α-pinene-α-methylstyrene-phenol copolymer, β-pinene-phenol copolymer, β-pinene-α-methylstyrene copolymer, and β-pinene-α-methylstyrene-phenol copolymer. As the terpene resin (e), these copolymers may be used alone or in combination of two or more.

[0084] The softening point of the (e) terpene resin is preferably 60° C. or higher, more preferably 80° C. or higher, and even more preferably 100° C. or higher, and is preferably 150° C. or lower, more preferably 130° C. or lower, and even more preferably 120° C. or lower. By using the (d) terpene resin having a softening point within the above range, the resin dispersibility during rubber kneading is improved. The softening point of the (e) terpene resin is the temperature at which the ball drops when the softening point as defined in JIS K 6220-1:2001 is measured using a ring and ball softening point measuring device.

[0085] As the (e) terpene resin, commercially available products can be used, for example, Sylvares TP2019 and Sylvatra xx6720 manufactured by KRATON Corporation; YS Resin PX1150N manufactured by Yasuhara Chemical Co., Ltd.

[0086] The content of the (e) terpene resin is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 4 parts by mass or more, and preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 15 parts by mass or less, per 100 parts by mass of the (a) base rubber. If the content of the (e) component is less than 2 parts by mass, the effect of adding the (e) component is small, and the effect of improving the hitting feeling at the time of a driver shot may not be obtained. On the other hand, if the content of the (e) component is more than 20 parts by mass, the obtained core may become too soft overall, and the resilience may decrease.

[0087] The blending ratio of the component (b) to the component (e) (component (b) / component (e)), by mass, is preferably 2.0 or more, more preferably 2.5 or more, even more preferably 2.8 or more, and is preferably 15.0 or less, more preferably 12.0 or less, even more preferably 10.0 or less, and particularly preferably 8.0 or less. When the blending ratio of the component (b) to the component (e) (component (b) / component (e)) is within the above range, the shot feel of the resulting golf ball when shot with a driver is improved.

[0088] [(f) Organic sulfur compounds] The rubber composition for golf balls of the present invention preferably further contains (f) an organosulfur compound, which improves the resilience of the resulting core.

[0089] The (f) organic sulfur compound is preferably at least one compound selected from the group consisting of thiols (thiophenols, thionaphthols), polysulfides, thiurams, thiocarboxylic acids, dithiocarboxylic acids, sulfenamides, dithiocarbamates, and thiazoles.

[0090] Examples of the thiols include thiophenols and thionaphthols. Examples of the thiophenols include thiophenol; thiophenols substituted with a fluoro group such as 4-fluorothiophenol, 2,4-difluorothiophenol, 2,5-difluorothiophenol, 2,6-difluorothiophenol, 2,4,5-trifluorothiophenol, 2,4,5,6-tetrafluorothiophenol, and pentafluorothiophenol; and chloro group such as 2-chlorothiophenol, 4-chlorothiophenol, 2,4-dichlorothiophenol, 2,5-dichlorothiophenol, 2,6-dichlorothiophenol, 2,4,5-trichlorothiophenol, 2,4,5,6-tetrachlorothiophenol, and pentachlorothiophenol. thiophenols substituted with thiophenol; thiophenols substituted with bromo groups such as 4-bromothiophenol, 2,4-dibromothiophenol, 2,5-dibromothiophenol, 2,6-dibromothiophenol, 2,4,5-tribromothiophenol, 2,4,5,6-tetrabromothiophenol, and pentabromothiophenol; thiophenols substituted with iodo groups such as 4-iodothiophenol, 2,4-diiodothiophenol, 2,5-diiodothiophenol, 2,6-diiodothiophenol, 2,4,5-triiodothiophenol, 2,4,5,6-tetraiodothiophenol, and pentaiodothiophenol; or metal salts thereof. As the metal salt, zinc salts are preferred.

[0091] The thionaphthols (naphthalene thiols) include 2-thionaphthol, 1-thionaphthol, 1-chloro-2-thionaphthol, 2-chloro-1-thionaphthol, 1-bromo-2-thionaphthol, 2-bromo-1-thionaphthol, 1-fluoro-2-thionaphthol, 2-fluoro-1-thionaphthol, 1-cyano-2-thionaphthol, 2-cyano-1-thionaphthol, 1-acetyl-2-thionaphthol, 2-acetyl-1-thionaphthol, or metal salts thereof, and 2-thionaphthol, 1-thionaphthol, or metal salts thereof are preferred. The metal salt is preferably a divalent metal salt, more preferably a zinc salt. Specific examples of the metal salt include the zinc salt of 1-thionaphthol and the zinc salt of 2-thionaphthol.

[0092] The polysulfides are organic sulfur compounds having polysulfide bonds, and examples of the polysulfides include disulfides, trisulfides, and tetrasulfides. As the polysulfides, diphenyl polysulfides are preferred.

[0093] Diphenyl polysulfides include, in addition to diphenyl disulfide, bis(4-fluorophenyl) disulfide, bis(2,5-difluorophenyl) disulfide, bis(2,6-difluorophenyl) disulfide, bis(2,4,5-trifluorophenyl) disulfide, bis(2,4,5,6-tetrafluorophenyl) disulfide, bis(pentafluorophenyl) disulfide, bis(4-chlorophenyl) disulfide, Bis(2,5-dichlorophenyl) disulfide, bis(2,6-dichlorophenyl) disulfide, bis(2,4,5-trichlorophenyl) disulfide, bis(2,4,5,6-tetrachlorophenyl) disulfide, bis(pentachlorophenyl) disulfide, bis(4-bromophenyl) disulfide, bis(2,5-dibromophenyl) disulfide, bis(2,6-dibromophenyl) disulfide, bis(2,4,5-tribromophenyl) disulfide phenyl) disulfide, bis(2,4,5,6-tetrabromophenyl) disulfide, bis(pentabromophenyl) disulfide, bis(4-iodophenyl) disulfide, bis(2,5-diiodophenyl) disulfide, bis(2,6-diiodophenyl) disulfide, bis(2,4,5-triiodophenyl) disulfide, bis(2,4,5,6-tetraiodophenyl) disulfide, bis(pentaiodophenyl) disulfide diphenyl disulfides substituted with halogen groups such as bis(4-methylphenyl) disulfide, bis(2,4,5-trimethylphenyl) disulfide, bis(pentamethylphenyl) disulfide, bis(4-t-butylphenyl) disulfide, bis(2,4,5-tri-t-butylphenyl) disulfide, bis(penta-t-butylphenyl) disulfide, and the like.

[0094] Examples of thiurams include thiuram monosulfides such as tetramethylthiuram monosulfide, thiuram disulfides such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, and tetrabutylthiuram disulfide, and thiuram tetrasulfides such as dipentamethylenethiuram tetrasulfide. Examples of thiocarboxylic acids include naphthalene thiocarboxylic acid. Examples of dithiocarboxylic acids include naphthalene dithiocarboxylic acid. Examples of sulfenamides include N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, and Nt-butyl-2-benzothiazole sulfenamide.

[0095] The (f) organic sulfur compound is preferably a thiophenol and / or a metal salt thereof, a thionaphthol and / or a metal salt thereof, a diphenyl disulfide, or a thiuram disulfide, and more preferably 2,4-dichlorothiophenol, 2,6-difluorothiophenol, 2,6-dichlorothiophenol, 2,6-dibromothiophenol, 2,6-diiodothiophenol, 2,4,5-trichlorothiophenol, pentachlorothiophenol, 1-thionaphthol, 2-thionaphthol, diphenyl disulfide, bis(2,6-difluorophenyl) disulfide, bis(2,6-dichlorophenyl) disulfide, bis(2,6-dibromophenyl) disulfide, bis(2,6-diiodophenyl) disulfide, or bis(pentabromophenyl) disulfide.

[0096] The (f) organic sulfur compounds can be used alone or in combination of two or more.

[0097] The content of the (f) organic sulfur compound is preferably 0.05 parts by weight or more, more preferably 0.1 parts by weight or more, and even more preferably 0.2 parts by weight or more, and is preferably 5.0 parts by weight or less, more preferably 3.0 parts by weight or less, and even more preferably 2.0 parts by weight or less, per 100 parts by weight of the (a) base rubber. If the content of the (f) organic sulfur compound is less than 0.05 parts by weight, the effect of adding the (f) organic sulfur compound may not be obtained, and the resilience of the golf ball may not be improved. If the content of the (f) organic sulfur compound is more than 5.0 parts by weight, the compressive deformation of the resulting golf ball may increase, and the resilience may decrease.

[0098] [(g) Metal compounds] The rubber composition for golf balls of the present invention preferably further contains (g) a metal compound. (g) The metal compound can be used, for example, as a weight adjuster for the rubber composition or as a neutralizing agent for an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms.

[0099] Examples of the (g) metal compound include metal hydroxides such as magnesium hydroxide, zinc hydroxide, calcium hydroxide, sodium hydroxide, lithium hydroxide, potassium hydroxide, and copper hydroxide; metal oxides such as magnesium oxide, calcium oxide, zinc oxide, and copper oxide; and metal carbonates such as magnesium carbonate, zinc carbonate, calcium carbonate, sodium carbonate, lithium carbonate, and potassium carbonate. The (g) metal compound is preferably a divalent metal compound, and more preferably a zinc compound. This is because the divalent metal compound reacts with an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms to form a metal bridge. Furthermore, by using a zinc compound, a golf ball with high resilience can be obtained.

[0100] The (g) metal compound may be used alone or in combination of two or more kinds. The content of the (g) metal compound may be appropriately adjusted depending on the desired degree of neutralization of the (b) α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms.

[0101] The rubber composition for golf balls of the present invention may contain additives such as pigments, fillers for adjusting the weight, antioxidants, peptizing agents, softeners, etc., as required.

[0102] The filler used in the rubber composition for golf balls is mainly blended as a weight adjusting agent for adjusting the weight of the golf ball obtained as a final product, and may be blended as necessary. Examples of the filler include inorganic fillers such as zinc oxide, barium sulfate, calcium carbonate, magnesium oxide, tungsten powder, and molybdenum powder. Zinc oxide is particularly preferred as the filler. Zinc oxide functions as a vulcanization aid and is considered to increase the hardness of the cured product (for example, the entire core). The content of the filler is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the (a) base rubber. If the content of the filler is less than 0.5 parts by mass, it becomes difficult to adjust the weight, and if it exceeds 30 parts by mass, the weight fraction of the rubber component tends to decrease, resulting in a decrease in resilience.

[0103] The content of the peptizing agent is preferably 0.1 part by mass or more and 5 parts by mass or less per 100 parts by mass of the (a) base rubber.

[0104] The rubber composition for golf balls of the present invention may be used in any of the constituent parts of a golf ball. For example, it can be suitably used in the body, core, or intermediate layer of a one-piece golf ball. Among these, the rubber composition for golf balls of the present invention can be suitably used in the inner core layer and / or the outer core layer of a two-layer core consisting of a single-layer core, an inner core layer, and an outer core layer.

[0105] The present invention includes a golf ball having components formed from the rubber composition for golf balls of the present invention. A preferred embodiment of the golf ball of the present invention is a golf ball having a core and at least one layer of cover covering the core, the core being formed from the rubber composition for golf balls of the present invention (hereinafter sometimes referred to as "rubber composition for core"). The golf ball of the present invention will be described below.

[0106] When the core is made of the rubber composition for golf balls of the present invention, the cured product on the core surface preferably satisfies the formula (1), and more preferably satisfies the formula (2). Specifically, the cured product in a region 0.5 mm thick from the core surface preferably satisfies the formula (1), more preferably satisfies the formula (2), and even more preferably satisfies the formula (3).

[0107] [core] The core of the golf ball of the present invention can be obtained by mixing and kneading the above-mentioned rubber composition for the core and molding it in a mold. The conditions for this are not particularly limited, but the process is usually carried out at 130°C to 200°C and a pressure of 2.9MPa to 11.8MPa for 10 minutes to 60 minutes. For example, it is preferable to heat the rubber composition for the core at 130°C to 200°C for 10 minutes to 60 minutes, or to heat it in two stages at 130°C to 150°C for 20 minutes to 40 minutes and then at 160°C to 180°C for 5 minutes to 15 minutes.

[0108] The core of the golf ball of the present invention has a surface hardness (Hs) of preferably 50 or more, more preferably 55 or more, and even more preferably 60 or more, and preferably 95 or less, more preferably 90 or less, and even more preferably 85 or less, in Shore C hardness. If the surface hardness (Hs) of the core is 50 or more in Shore C hardness, the resilience of the core will be better. If the surface hardness (Hs) of the core is 95 or less in Shore C hardness, the shot feeling upon driver shots will be improved.

[0109] The central hardness (Ho) of the core is preferably 30 or more, more preferably 35 or more, and even more preferably 40 or more, in Shore C hardness. If the central hardness (Ho) of the core is 30 or more in Shore C hardness, the core is not too soft and has good resilience. Furthermore, the central hardness (Ho) of the core is preferably 70 or less in Shore C hardness, more preferably 68 or less, and even more preferably 67 or less. If the central hardness (Ho) is 70 or less in Shore C hardness, the core is not too hard and has a good shot feeling.

[0110] The hardness difference (Hs-Ho) between the surface hardness (Hs) and the center hardness (Ho) of the core is preferably 5 or more, more preferably 6 or more, and even more preferably 8 or more, and is preferably 35 or less, more preferably 30 or less, and even more preferably 28 or less, in Shore C hardness. If the hardness difference (Hs-Ho) between the surface hardness (Hs) and the center hardness (Ho) of the core is 5 or more in Shore C hardness, a golf ball with good resilience can be obtained. Also, if the hardness difference (Hs-Ho) between the surface hardness (Hs) and the center hardness (Ho) of the core is 35 or less in Shore C hardness, a golf ball with an improved shot feeling upon driver shot can be obtained.

[0111] The diameter of the core of the golf ball of the present invention is preferably 34.8 mm or more, more preferably 36.8 mm or more, even more preferably 38.8 mm or more, and is preferably 42.2 mm or less, more preferably 41.8 mm or less, even more preferably 41.2 mm or less, and most preferably 40.8 mm or less. If the diameter of the core is 34.8 mm or more, the thickness of the cover is not too thick, and the resilience is better. On the other hand, if the diameter of the core is 42.2 mm or less, the cover is not too thin, and the function of the cover is more fully exhibited.

[0112] When the core has a diameter of 34.8 mm to 42.2 mm, the amount of compressive deformation (the amount the core shrinks in the compressive direction) from when an initial load of 98 N is applied to when a final load of 1275 N is applied is preferably 2.0 mm or more, more preferably 2.3 mm or more, and even more preferably 2.5 mm or more, preferably 5.0 mm or less, more preferably 4.5 mm or less, and even more preferably 4.3 mm or less. If the amount of compressive deformation is 2.0 mm or more, the hitting feel will be better, and if it is 5.0 mm or less, the resilience will be better.

[0113] [cover] The cover of the golf ball of the present invention is formed from a cover composition containing a resin component, such as an ionomer resin, a thermoplastic polyurethane elastomer available from BASF Japan Ltd. under the trade name "Elastollan (registered trademark)", a thermoplastic polyamide elastomer available from Arkema K.K. under the trade name "Pebax (registered trademark)", a thermoplastic polyester elastomer available from DuPont-Toray Co., Ltd. under the trade name "Hytrel (registered trademark)", and a thermoplastic styrene elastomer available from Mitsubishi Chemical Corporation under the trade name "Labalon (registered trademark)".

[0114] Examples of the ionomer resin include a binary copolymer of an olefin and an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms, in which at least a part of the carboxyl groups is neutralized with a metal ion, a ternary copolymer of an olefin, an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms, and an α,β-unsaturated carboxylic acid ester, in which at least a part of the carboxyl groups is neutralized with a metal ion, or a mixture thereof. The olefin is preferably an olefin having 2 to 8 carbon atoms, such as ethylene, propylene, butene, pentene, hexene, heptene, octene, etc., and ethylene is particularly preferred. Examples of the α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms include acrylic acid, methacrylic acid, fumaric acid, maleic acid, crotonic acid, etc., and acrylic acid or methacrylic acid is particularly preferred. Examples of the α,β-unsaturated carboxylic acid ester include methyl, ethyl, propyl, n-butyl, and isobutyl esters of acrylic acid, methacrylic acid, fumaric acid, and maleic acid, and acrylic acid esters and methacrylic acid esters are particularly preferred. Among these, the ionomer resin is preferably a metal ion neutralized product of an ethylene-(meth)acrylic acid binary copolymer or a metal ion neutralized product of an ethylene-(meth)acrylic acid-(meth)acrylic acid ester ternary copolymer.

[0115] The cover composition constituting the cover of the golf ball of the present invention preferably contains a thermoplastic polyurethane elastomer or an ionomer resin as a resin component. When an ionomer resin is used, it is also preferable to use a thermoplastic styrene elastomer in combination. The content of the polyurethane or ionomer resin in the resin component of the cover composition is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more.

[0116] In addition to the resin components described above, the cover composition may contain pigment components such as white pigments (e.g., titanium oxide), blue pigments, and red pigments, weight adjusters such as zinc oxide, calcium carbonate, and barium sulfate, dispersants, antioxidants, ultraviolet absorbing agents, light stabilizers, fluorescent materials, or fluorescent brighteners, to the extent that the performance of the cover is not impaired.

[0117] The content of the white pigment (e.g., titanium oxide) is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, based on 100 parts by mass of the resin component constituting the cover. By making the content of the white pigment 0.5 parts by mass or more, it is possible to impart hiding properties to the cover. In addition, if the content of the white pigment exceeds 10 parts by mass, the durability of the obtained cover may decrease.

[0118] The slab hardness of the cover composition is preferably set appropriately according to the desired performance of the golf ball. For example, in the case of a distance-type golf ball that emphasizes flight distance, the slab hardness of the cover composition is preferably 50 or more, more preferably 55 or more, even more preferably 60 or more, preferably 80 or less, more preferably 70 or less, and even more preferably 68 or less in Shore D hardness. By making the slab hardness of the cover composition 50 or more, a golf ball with a high launch angle and low spin is obtained in driver shots and iron shots, and the flight distance is improved. In addition, by making the slab hardness of the cover composition 80 or less, a golf ball with excellent durability is obtained. In addition, in the case of a spin-type golf ball that emphasizes controllability, the slab hardness of the cover composition is preferably less than 50, preferably 20 or more, more preferably 25 or more, and even more preferably 30 or more in Shore D hardness. If the cover composition has a slab hardness of less than 50 Shore D hardness, the spin rate of approach shots is increased, resulting in a golf ball that stops easily on the green. Furthermore, by making the slab hardness 20 or more, the abrasion resistance is improved. In the case of a cover having multiple layers, the slab hardness of the cover composition constituting each layer may be the same or different.

[0119] Methods for molding the cover of the golf ball of the present invention include, for example, a method in which a hollow shell is molded from a cover composition, the core is coated with multiple shells, and the resulting mixture is compression molded (preferably, a method in which a hollow half shell is molded from the cover composition, the core is coated with two half shells, and the resulting mixture is compression molded), or a method in which the cover composition is directly injection molded onto the core.

[0120] When the cover is molded by the compression molding method, the molding of the half shell can be performed by either the compression molding method or the injection molding method, but the compression molding method is preferable. The conditions for compressing and molding the cover composition into the half shell include, for example, a pressure of 1 MPa or more and 20 MPa or less, and a molding temperature of -20°C or more and 70°C or less relative to the flow start temperature of the cover composition. By using the above molding conditions, a half shell having a uniform thickness can be molded. The method for molding the cover using the half shell includes, for example, a method of covering the core with two half shells and compression molding. The conditions for compressing and molding the half shell into the cover include, for example, a molding pressure of 0.5 MPa or more and 25 MPa or less, and a molding temperature of -20°C or more and 70°C or less relative to the flow start temperature of the cover composition. By using the above molding conditions, a golf ball cover having a uniform cover thickness can be molded.

[0121] When the cover composition is injection molded to form the cover, the cover composition in pellet form obtained by extrusion may be used for injection molding, or the cover material such as the base resin component and the pigment may be dry blended and directly injection molded. As the upper and lower molds for molding the cover, it is preferable to use those having a hemispherical cavity, with pimples, and a part of the pimples also serving as a hold pin that can move forward and backward. The cover can be molded by injection molding by protruding the hold pin, inserting the core and holding it, injecting the cover composition, and cooling it. For example, the cover composition heated to 200°C to 250°C is injected for 0.5 to 5 seconds into a mold clamped at a pressure of 9 MPa to 15 MPa, and cooled for 10 to 60 seconds, and then opening the mold.

[0122] When the cover is molded, depressions called dimples are usually formed on the surface. The total number of dimples formed on the cover is preferably 200 to 500 inclusive. If the total number of dimples is less than 200, the effect of the dimples is difficult to obtain. If the total number of dimples exceeds 500, the size of each dimple becomes small, making it difficult to obtain the effect of the dimples. The shape (shape in plan view) of the dimples formed is not particularly limited, and the following may be used alone or in combination: a circle; a polygon such as an approximately triangular, approximately rectangular, approximately pentagonal, or approximately hexagonal; or other irregular shape.

[0123] The thickness of the cover is preferably 4.0 mm or less, more preferably 3.0 mm or less, and even more preferably 2.0 mm or less. If the thickness of the cover is 4.0 mm or less, the resilience and hitting feeling of the resulting golf ball will be better. The thickness of the cover is preferably 0.3 mm or more, more preferably 0.5 mm or more, and even more preferably 0.8 mm or more. If the thickness of the cover is less than 0.3 mm, the durability and abrasion resistance of the cover may decrease. In the case of a plurality of cover layers, the total thickness of the plurality of cover layers is preferably within the above range.

[0124] The golf ball body with the cover molded thereon is preferably removed from the mold and, if necessary, subjected to surface treatment such as deburring, cleaning, and sandblasting. In addition, a coating film or markings can be formed as desired. The thickness of the coating film is not particularly limited, but is preferably 5 μm or more, more preferably 7 μm or more, preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less. If the thickness is less than 5 μm, the coating film is likely to be worn away by continuous use, and if the thickness exceeds 50 μm, the effect of the dimples is reduced, resulting in a decrease in the flight performance of the golf ball.

[0125] [Golf balls] The structure of the golf ball of the present invention is not particularly limited as long as it has a core and one or more layers of a cover that encases the core. Fig. 1 is a partially cutaway cross-sectional view showing a golf ball 1 according to one embodiment of the present invention. Golf ball 1 has a spherical core 2 and a cover 3 that encases the spherical core 2. A large number of dimples 31 are formed on the surface of this cover. The portion of the surface of this golf ball 1 other than the dimples 31 is a land 32. This golf ball 1 has a paint layer and a mark layer on the outside of the cover 3, but these layers are not shown in the figure.

[0126] The core is preferably spherical. The core may have either a single-layer structure or a multi-layer structure, but is preferably a single-layer structure. A single-layer core has no energy loss at the interface of the multi-layer structure when hitting, and improves resilience. The cover may have a structure of one layer or more, and may have a single-layer structure or a multi-layer structure of two or more layers. Examples of the golf ball of the present invention include a two-piece golf ball consisting of a core and a single-layer cover arranged to cover the core; a multi-piece golf ball (including a three-piece golf ball) having a core and a cover of two or more layers arranged to cover the core; and a thread-wound golf ball having a core, a rubber thread layer arranged around the core, and a cover arranged to cover the rubber thread layer. The present invention can be suitably used for golf balls of any of the above structures.

[0127] The diameter of the golf ball of the present invention is preferably 40 mm to 45 mm. From the viewpoint of satisfying the standards of the United States Golf Association (USGA), the diameter is particularly preferably 42.67 mm or more. From the viewpoint of suppressing air resistance, the diameter is more preferably 44 mm or less, and particularly preferably 42.80 mm or less. The mass of the golf ball of the present invention is preferably 40 g or more and 50 g or less. From the viewpoint of obtaining a large inertia, the mass is more preferably 44 g or more, and particularly preferably 45.00 g or more. From the viewpoint of satisfying the standards of the USGA, the mass is particularly preferably 45.93 g or less.

[0128] In the golf ball of the present invention, when the diameter is 40 mm to 45 mm, the amount of compressive deformation (amount of shrinkage in the compressive direction) when a final load of 1275 N is applied from an initial load of 98 N is preferably 2.0 mm or more, more preferably 2.3 mm or more, and even more preferably 2.5 mm or more, and is preferably 4.0 mm or less, more preferably 3.5 mm or less, and even more preferably 3.3 mm or less. A golf ball with the compressive deformation amount of 2.0 mm or more is not too hard and has a good shot feeling. On the other hand, by making the compressive deformation amount 4.0 mm or less, the resilience is increased. EXAMPLES

[0129] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.

[0130] [Evaluation method] (1) Effective crosslink density (mmol / cc) The effective crosslink density of the cured product of the rubber composition for golf balls is calculated from the swelling measurement of a slab sample of the cured product of the rubber composition for golf balls. The rubber composition for golf balls was kneaded with a kneading roll and vulcanized at 170°C for 30 minutes to prepare a slab with a thickness of 0.5 mm, a length of 12 cm, and a width of 14 cm. A slab with a thickness of 0.5 mm and a size of 2 cm x 2 cm was cut out from this slab to prepare a sample for measurement.

[0131] The swelling measurement was carried out by immersing the obtained slab sample in toluene for 24 hours at 40° C. The mass of the slab before and after swelling was measured, and the effective crosslink density was calculated using the Flory-Rehner equation.

[0132]

number

[0133]

number

[0134] (2) Compressive deformation amount (mm) The deformation in the compression direction (the amount the core or golf ball shrinks in the compression direction) was measured from when an initial load of 98 N was applied to the core or golf ball until a final load of 1275 N was applied.

[0135] (3) Core hardness (Shore C hardness) The Shore C hardness of the surface of the core was measured using an automatic hardness tester Digitest II manufactured by H. Burleith Co., Ltd. The core was cut into a hemisphere, and the hardness of the center of the cut surface was measured.

[0136] (4) Slab hardness A sheet having a thickness of about 2 mm was prepared by injection molding using the cover composition, and stored at 23°C for two weeks. The hardness of the sheet was measured using an automatic hardness tester (H. Burleith, Digitest II) in a state where three or more sheets were stacked so as not to be affected by the measurement substrate. The detector used was "Shore D". In the case of the rubber composition, a sheet having a thickness of about 2 mm was prepared by pressing at 170°C for 30 minutes. The sheet was stored at 23°C for two weeks, and measured using an automatic rubber hardness tester P1 type manufactured by Kobunshi Keiki Co., Ltd. equipped with a spring type Shore C type hardness tester specified in ASTM-D2240 in a state where three or more sheets were stacked so as not to be affected by the measurement substrate.

[0137] (5)Durability A metal head W#1 driver (Sumitomo Rubber Industries, XXIO S, loft 11°) was attached to a swing robot M / C manufactured by Golf Laboratory, and the golf balls were repeatedly hit at a head speed of 45 m / sec, and the number of hits until cracks occurred was measured. Measurements were performed on 12 golf balls each, and the average value was taken as the number of hits for that golf ball. The number of hits for each golf ball was expressed as an index value, with the number of hits for golf ball No. 1 being set at 100.

[0138] [Manufacturing golf balls] (1) Core preparation The rubber compositions having the formulations shown in Tables 1 and 2 were kneaded with kneading rolls and hot-pressed at 170° C. for 30 minutes in upper and lower molds having hemispherical cavities to obtain spherical cores having a diameter of 39.7 mm.

[0139] [Table 1]

[0140] [Table 2]

[0141] The materials used in Tables 1 and 2 are as follows: BR730: High cis polybutadiene rubber manufactured by JSR Corporation (cis-1,4-bond content = 95 mass%, 1,2-vinyl bond content = 1.3 mass%, Mooney viscosity (ML 1+4 (100℃)=55, molecular weight distribution (Mw / Mn)=3) ZDA: Zinc acrylate ZN-DA90S (10% surface treatment) manufactured by Nisshoku Techno Fine Chemical Co., Ltd. DCP: Dicumyl peroxide manufactured by Tokyo Chemical Industry Co., Ltd. (1 minute half-life temperature: 175.2 degrees) PBDS: Bis(pentabromophenyl) disulfide manufactured by Kawaguchi Chemical Industry Co., Ltd. DPDS: Diphenyl disulfide manufactured by Sumitomo Seika Chemicals White Seal: INDOLYSAGHT zinc oxide Barium sulfate: Sakai Chemical Industry Co., Ltd., "Barium Sulfate BD" Benzoic acid: Tokyo Chemical Industry Co., Ltd. H-BHT: Dibutyl hydroxytoluene manufactured by Tokyo Materials Adeka STAB LA-77Y: A hindered amine compound (bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate) manufactured by Adeka Corporation SylvaresTP2019 (pinene-phenol copolymer, softening point: 125°C): manufactured by KRATON Polystar T130: Terpene phenol resin (softening point 130±5℃) manufactured by Yasuhara Chemical Co., Ltd. Polystar U115: Terpene phenol resin manufactured by Yasuhara Chemical Co., Ltd. (softening point 115±5℃) Polystar K125: Terpene phenol resin (softening point 125±5℃) manufactured by Yasuhara Chemical Co., Ltd.

[0142] (2) Making the cover and making the golf ball The cover material having the composition shown in Table 3 was extruded by a twin-screw kneading extruder to prepare a pellet-shaped cover composition. The extrusion conditions for the cover composition were a screw diameter of 45 mm, a screw rotation speed of 200 rpm, and a screw L / D of 35, and the composition was heated to 160 to 230°C at the die position of the extruder. The cover composition thus obtained was injection molded onto the spherical core obtained as described above to a thickness of 1.5 mm to produce a golf ball having a spherical core and a cover covering the core. The evaluation results of the obtained golf balls are shown in Tables 1 and 2.

[0143] [Table 3]

[0144] The materials used in Table 3 are as follows: Himilan 1555: Sodium neutralized ionomer manufactured by Mitsui DuPont Polychemicals Himilan 1605: Sodium neutralized ionomer manufactured by Mitsui DuPont Polychemicals Himilan AM7329: Zn neutralized ionomer manufactured by Mitsui DuPont Polychemicals A-220: Titanium dioxide manufactured by Ishihara Sangyo Kaisha JF-90: Light stabilizer manufactured by Johoku Chemical Co., Ltd.

[0145] As shown in Tables 1 and 2, all of the golf balls of the present invention are excellent in durability. [Industrial Applicability]

[0146] The rubber composition of the present invention can be suitably used as a rubber composition for golf balls.

Claims

1. The cured product of the rubber composition for golf balls is obtained by curing a rubber composition for golf balls, which contains (a) a base rubber, (b) an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or a metal salt thereof as a co-crosslinking agent, and (c) a crosslinking initiator, and is characterized in that the cured product of the rubber composition for golf balls satisfies the following mathematical formula (3): Y<0.1×X-2.00...(3) In formula (3), Y is the effective crosslink density (mmol / cc) of the cured product of the rubber composition (wherein the cured product of the rubber composition has a maximum crosslink density). X: Amount (parts by mass) of component (b) per 100 parts by mass of base rubber (a)

2. 1. A cured product of a rubber composition for a golf ball, comprising (a) a base rubber, (b) an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or a metal salt thereof as a co-crosslinking agent, and (c) a crosslinking initiator, the cured product being obtained by curing a rubber composition for a golf ball, the rubber composition comprising (a) an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or a metal salt thereof, and (d) 2 to 15 parts by mass of a radical scavenger per 100 parts by mass of the base rubber, the cured product satisfying the following mathematical formula (1): Y<0.1×X-1.30...(1) In formula (1), Y is the effective crosslink density (mmol / cc) of the cured product of the rubber composition (wherein the cured product of the rubber composition has a maximum crosslink density). X: Amount (parts by mass) of component (b) per 100 parts by mass of base rubber (a)

3. 3. The cured product of the rubber composition for golf balls according to claim 2, wherein the radical scavenger is a hindered phenol compound or a hindered amine compound.

4. 4. The cured product of the rubber composition for golf balls according to claim 1, wherein the rubber composition for golf balls further comprises (e) a terpene resin.

5. The cured product of the rubber composition for golf balls is obtained by curing a rubber composition for golf balls, which contains (a) a base rubber, (b) an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms and / or a metal salt thereof as a co-crosslinking agent, (c) a crosslinking initiator, and (e) a terpene resin, and is characterized in that the cured product of the rubber composition for golf balls satisfies the following mathematical formula (1): Y<0.1×X-1.30...(1) In formula (1), Y is the effective crosslink density (mmol / cc) of the cured product of the rubber composition (wherein the cured product of the rubber composition has a maximum crosslink density). X: Amount (parts by mass) of component (b) per 100 parts by mass of base rubber (a)

6. 6. The cured product of the rubber composition for golf balls according to claim 4, further comprising (e) 2 to 20 parts by weight of a terpene resin per 100 parts by weight of the base rubber (a).

7. (e) The cured product of the rubber composition for golf balls according to any one of claims 4 to 6, wherein the terpene resin is at least one selected from the group consisting of a terpene polymer, a terpene-phenol copolymer, a terpene-styrene copolymer, a terpene-phenol-styrene copolymer, a hydrogenated terpene-phenol copolymer, a hydrogenated terpene-styrene copolymer, and a hydrogenated terpene-phenol-styrene copolymer.

8. (e) The cured product of the rubber composition for golf balls according to any one of claims 4 to 7, wherein the terpene resin is at least one selected from the compounds having structures represented by the following chemical formulas (7) to (10): [Case 1] [chemical 2] [C3] [C4] [In chemical formulas (7) to (10), R 1 and R 2 each independently represents a divalent residue of a phenolic compound and / or a styrene compound; m 1 ~m 4 Each independently represents a natural number from 1 to 30; 1 ~n 2 each independently represents a natural number from 1 to 20.

9. (e) The cured product of the rubber composition for golf balls according to any one of claims 4 to 8, wherein the terpene resin has a softening point of 60°C to 150°C.

10. 2. The cured product of claim 1, wherein the rubber composition for golf balls contains not more than 0.1 part by weight of (c) a crosslinking initiator per 100 parts by weight of (a) the base rubber.

11. 11. A golf ball comprising, as a constituent member, a cured product of the rubber composition for golf balls according to claim 1.

Citation Information

Patent Citations

  • Solid golf ball

    JP1988212377A

  • One-piece golf ball

    JP2001149504A

  • Golf ball

    JP2004121815A

  • Golf ball

    JP2009112806A

  • Golf ball

    JP2009119253A