A wear-resistant non-magnetic hard alloy and its preparation method
By using tungsten to coat components such as diamond particles and rare earth metal oxides in cemented carbides, the problem of difficulty in removing magnetic components and contradiction between wear resistance and hardness in traditional cemented carbides is solved, and high hardness, wear resistance and Non-magnetic cemented carbide avoids the magnetic influence of artificial diamonds and reduces production costs.
Patent Information
- Application Number
- CN202410351049.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-03-26
AI Technical Summary
It is difficult to completely remove magnetic components during the preparation process of traditional cemented carbides, and there is a contradiction between wear resistance and hardness. Artificial diamonds are susceptible to magnetic field interference and have low bonding strength, so they are easy to graphitize.
Using tungsten coated diamond particles as hardness enhancer, combining tungsten carbide, nickel carbonyl carbonyl powder, niobium hydride, rare earth metal oxides and vanadium carbide, wear-resistant magnetic hard carbide is prepared through impregnation and ball milling, and non-wovenous carbide using tungsten Magnetic and high hardness characteristics, combined with the grain refinement of rare earth oxides, improve the mechanical strength and wear resistance of the alloy.
The prepared cemented carbide has high hardness, wear resistance and non-magnetic properties, avoiding the magnetic influence of artificial diamonds, improving the mechanical strength and wear resistance of the alloy, and reducing production costs.
Smart Images

Figure CN118241095B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cemented carbide materials, in particular to a wear-resistant non-magnetic cemented carbide and a preparation method thereof. Background Art
[0002] With the rapid development of industry and technology, the demand for material performance is increasing. Wear-resistant non-magnetic cemented carbide has gradually become an important material in manufacturing and other fields because of its excellent performance in harsh environments, such as high hardness, wear resistance, corrosion resistance, etc. However, traditional cemented carbide often contains magnetic components, which may cause adverse effects in some special occasions, such as electronic equipment manufacturing, medical equipment, etc. Therefore, the research on the preparation of wear-resistant non-magnetic cemented carbide has important theoretical and practical significance. Although wear-resistant non-magnetic cemented carbide has broad application prospects in theory, there are still some problems that need to be solved in practical applications. First, the traditional preparation method often cannot fully guarantee the non-magnetic nature of the material, resulting in the prepared alloy still containing certain magnetic components; secondly, some existing non-magnetic cemented carbides have a certain contradiction between wear resistance and hardness. It is still a challenge to prepare alloys that have both high hardness and can maintain non-magnetic properties.
[0003] Adding non-magnetic elements can reduce the proportion of magnetic materials in the alloy on the one hand, and change the electromagnetic properties of the alloy and reduce magnetism on the other hand. Diamond is highly praised for its excellent hardness and wear resistance. However, its limitations in conventional applications are mainly reflected in the following two points: First, diamond has poor corrosion resistance. Second, unlike natural diamond, artificial diamond is easily disturbed by magnetic fields due to impurities in the production process. Although it is expected to utilize the high hardness of diamond in the preparation of wear-resistant non-magnetic cemented carbide, how to avoid artificial diamond from being disturbed by magnetic fields becomes a problem that needs to be solved. In addition, it also faces the problems of low bonding strength between diamond and matrix, easy detachment of diamond particles, and easy graphitization of diamond during sintering. However, wear-resistant non-magnetic cemented carbide with added diamond still has good application prospects. Summary of the invention
[0004] The invention proposes a wear-resistant non-magnetic hard alloy and a preparation method thereof. Specifically, tungsten-coated diamond particles are used as a hardness enhancer, tungsten carbide is used as a hard phase, carbonyl nickel powder, niobium hydride, rare earth metal oxides and are used as a bonding phase, and vanadium carbide is used as a grain growth inhibitor. The tungsten-coated diamond particles are prepared by an impregnation method, and the raw materials are mixed and ball milled. Finally, the wear-resistant non-magnetic hard alloy is prepared by a spark plasma sintering method. The alloy has the characteristics of high hardness, good wear resistance and non-magnetism.
[0005] In order to achieve the above technical objectives, the following technical solutions are mainly adopted:
[0006] A wear-resistant non-magnetic hard alloy, composed of a matrix powder and a hardness enhancer, the mass fractions of which are: 90-99wt% of the matrix powder and 1-10wt% of the hardness enhancer;
[0007] The matrix powder is composed of a hard phase, a binder phase and a grain growth inhibitor. The mass fraction of each component raw material in the matrix powder is as follows: the hard phase is 80-90wt% tungsten carbide, the binder phase is 6-12wt% carbonyl nickel powder, 3-5wt% niobium hydride, 0.1-1wt% rare earth metal oxide and 0.5-1wt% graphite, and the grain growth inhibitor is 0.4-1wt% vanadium carbide;
[0008] Tungsten carbide is in powder form, with a purity of 99.9% and a particle size of 2μm. The purity of carbonyl nickel powder is 99% and a particle size of 2~3μm. The purity of niobium hydride is 99% and a particle size of 40~45μm. The rare earth metal oxide is one of yttrium trioxide and cerium trioxide, and the purity of the rare earth metal oxide is 99.9%. The purity of graphite is 98% and a particle size of 45μm. Vanadium carbide is in powder form, with a purity of 99.9% and a particle size of 2μm.
[0009] The hardness enhancer is tungsten-coated diamond particles, which are prepared from ammonium tungstate, diamond, and polyvinyl alcohol, and the mass ratio of ammonium tungstate, polyvinyl alcohol, and diamond is 0.1-0.5:0.05-0.1:5;
[0010] The diamond is of analytical grade with a particle size of 15-25 μm, the ammonium tungstate is of analytical grade with a purity of 99.99%, and the polyvinyl alcohol is of analytical grade with Mw=30000-70000.
[0011] Further, the preparation of the hardness enhancer comprises the following steps:
[0012] Q1, take the diamond and use distilled water to ultrasonically clean it for 10-20 minutes until there is no impurity on the surface, treat it in 65wt% nitric acid for 15-25 hours to roughen its surface, then use deionized water and anhydrous ethanol to clean it in turn to make no nitric acid residue on the surface, and bake it in an oven at 80℃ for 20 minutes until it is dry to obtain pretreated diamond;
[0013] Q2, weigh ammonium tungstate according to the proportion, add it into deionized water, heat it to 50℃ and stir until dissolved, the stirring speed is 200~300rpm, and obtain ammonium tungstate solution;
[0014] Q3, weigh polypropylene alcohol according to proportion and add it into deionized water, heat it to 90°C until the polypropylene alcohol is dissolved, to obtain a PVA aqueous solution;
[0015] Q4, mixing the ammonium tungstate solution prepared in step Q2 and the PVA aqueous solution prepared in step Q3 in proportion to obtain an impregnation solution;
[0016] Q5, taking the pretreated diamond and the impregnation solution prepared in step Q1 in proportion, heating to 50°C and stirring at a stirring speed of 100-200 rpm, stirring until dry, to obtain diamond particles coated with ammonium tungstate;
[0017] Q6, heat treating the ammonium tungstate coated diamond particles obtained in Q5, 2 -Ar mixed gas atmosphere, heat treatment at 700-1100°C for 1-3h with a heating rate of 5°C / min to obtain tungsten-coated diamond particles, namely the hardness enhancer.
[0018] Preferably, the mass fraction of the ammonium tungstate solution in step Q2 is 5-15wt%, and the mass fraction of the PVA aqueous solution in step Q3 is 5-15wt%.
[0019] Preferably, the H2-Ar mixed gas in step Q6 is composed of 5% H 2 and 95% Ar.
[0020] Furthermore, a method for preparing a wear-resistant non-magnetic cemented carbide comprises the following steps:
[0021] S1, firstly mix carbonyl nickel powder, niobium hydride, rare earth metal oxide and graphite in proportion, add them into a planetary ball mill, and perform ball milling with isopropanol as the medium at a ball milling speed of 600 rpm for 1-2 h to obtain a binder phase powder;
[0022] S2, adding tungsten carbide, tungsten-coated diamond particles and vanadium carbide in proportion to the binder phase powder obtained in step S1, continuing ball milling with isopropanol as the medium, ball milling at a ball milling speed of 600 rpm for 3 hours, then adjusting the ball milling speed to 150 rpm and continuing ball milling for 48 hours, and drying in an oven at 70° C. for 2 hours after ball milling to obtain a mixed powder;
[0023] S3, placing the mixed powder prepared in step S2 in a graphite mold, and performing primary sintering in a vacuum plasma sintering furnace at a sintering temperature of 400-600° C., a heating rate of 150° C. / min, and a sintering time of 2-5 min to obtain a primary sintered body;
[0024] S4, plasma sintering the primary sintered body prepared in step S3, in an Ar atmosphere, with a sintering temperature of 800-1000° C., a heating rate of 200° C. / min, and a sintering time of 4-10 min, to obtain a plasma sintered body;
[0025] S5, performing secondary sintering on the plasma sintered body obtained in step S4, with a sintering temperature of 900-1100° C., a heating rate of 100° C. / min, and a sintering time of 8-12 min to obtain a sintered cemented carbide;
[0026] S6, cooling the sintered cemented carbide prepared in step S5 to room temperature in a cooling system at a cooling rate of 150°C / min to obtain the wear-resistant non-magnetic cemented carbide.
[0027] Preferably, the vacuum degree of the vacuum plasma sintering furnace in step S3 is 10Pa.
[0028] The beneficial effects achieved by the present invention are as follows:
[0029] The wear-resistant non-magnetic hard alloy prepared by the invention has tungsten carbide as hard phase, carbonyl nickel powder, niobium hydride, rare earth metal oxide and graphite as bonding phase, vanadium carbide as grain growth inhibitor, and tungsten-coated diamond particles as hardness enhancer.
[0030] First, the hard phase tungsten carbide is non-magnetic, and Fe, Co, Ni, etc. are commonly used as bonding phases. However, the corrosion resistance of the Co bonding phase is poor, and the hardness and strength of the Ni bonding phase are low. The present invention adopts carbonyl nickel powder-niobium hydride-graphite-rare earth oxide as a substitute for the bonding phase. The carbonyl nickel powder has the characteristics of high purity, fine particle size, highly developed surface and easy sintering. Niobium hydride loses the flexibility and ductility of niobium metal in the hydrogenated form, becomes brittle and hard, and the use of niobium can also limit the grain size of tungsten carbide, which helps to improve the mechanical strength and toughness of cemented carbide. The introduction of rare earth oxide can not only control the influence of impurities on cemented carbide during the preparation process, such as the increase of the porosity of the sample after sintering, but also refine the grains, control the growth of tungsten carbide grains, improve the strength of cemented carbide, and will not affect the hard alloy. The magnetism of the alloy is affected; secondly, tungsten-coated diamond particles are introduced to improve the wear resistance and hardness of the cemented carbide. The tungsten-coated diamond particles prepared by the impregnation method have the characteristics of uniform coating thickness and smooth surface. Tungsten has good wear resistance and high hardness. The synergistic effect with diamond helps to further optimize its wear resistance. At the same time, tungsten is a non-magnetic material. The use of tungsten-coated diamond particles can reduce the influence of the magnetism of artificial diamond itself on the performance of cemented carbide. In addition, a tungsten carbide layer can be generated on the tungsten-diamond interface during heat treatment to prevent the internal diamond from graphitizing and causing its performance to deteriorate; finally, since the rare earth metal in the bonding phase has a certain grain refining effect, the amount of grain growth inhibitor can be reduced when preparing the non-magnetic wear-resistant cemented carbide, which helps to reduce production costs.
[0031] In summary, the non-magnetic wear-resistant cemented carbide prepared by the present invention consists of four parts: a hard phase, a bonding phase, a grain growth inhibitor and a hardness enhancer. The components work together to achieve remarkable results in improving performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions therein, the following briefly introduces the drawings required for use in the descriptions of the embodiments and comparative examples. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0033] Figure 1 This is the circuit diagram for magnetic permeability testing;
[0034] Figure 2 It is a line graph of the wear rate and hardness test of each embodiment and comparative example;
[0035] Figure 3 It is a bar-line graph of tensile strength and yield strength test of each embodiment and comparative example;
[0036] Figure 4 It is a line graph of magnetic induction intensity test of each embodiment and comparative example. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are part of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0038] A wear-resistant non-magnetic hard alloy, composed of a matrix powder and a hardness enhancer, the mass fractions of which are: 95wt% of the matrix powder and 5wt% of the hardness enhancer;
[0039] The matrix powder is composed of a hard phase, a binder phase and a grain growth inhibitor. The raw materials and their mass fractions in the matrix powder are as follows: the hard phase is 80wt% tungsten carbide, the binder phase is 12wt% carbonyl nickel powder, 5wt% niobium hydride, 1wt% rare earth metal oxide and 1wt% graphite, and the grain growth inhibitor is 1wt% vanadium carbide;
[0040] Tungsten carbide is in powder form, with a purity of 99.9% and a particle size of 2μm, carbonyl nickel powder is in a purity of 99% and a particle size of 3μm, niobium hydride is in a purity of 99% and a particle size of 40μm, rare earth metal oxide is one of yttrium trioxide and cerium trioxide, the purity of rare earth metal oxide is 99.9%, graphite is in a purity of 98% and a particle size of 45μm, and vanadium carbide is in a powder form, with a purity of 99.9% and a particle size of 2μm;
[0041] The hardness enhancer is tungsten-coated diamond particles, which are prepared from ammonium tungstate, diamond, and polyvinyl alcohol, and the mass ratio of ammonium tungstate, polyvinyl alcohol, and diamond is 0.3:0.07:5;
[0042] The diamond is of analytical grade with a particle size of 20 μm, the ammonium tungstate is of analytical grade with a purity of 99.99%, and the polyvinyl alcohol is of analytical grade with Mw=55,000.
[0043] The preparation of the hardness enhancer comprises the following steps:
[0044] Q1, the diamond was ultrasonically cleaned with distilled water for 15 minutes until there was no impurity on the surface, and then treated with 65wt% nitric acid for 20 hours to roughen the surface, and then cleaned with deionized water and anhydrous ethanol in sequence to make no nitric acid residue on the surface, and baked in an oven at 80°C for 20 minutes until dry, to obtain pretreated diamond;
[0045] Q2, weigh ammonium tungstate in proportion, add it into deionized water, heat it to 50℃ and stir until dissolved, the stirring speed is 250rpm, and obtain ammonium tungstate solution, the mass fraction of which is 10wt%;
[0046] Q3, weigh polypropylene alcohol according to proportion and add it into deionized water, heat it to 90°C until the polypropylene alcohol is dissolved, and obtain a PVA aqueous solution, the mass fraction of the PVA aqueous solution is 10wt%;
[0047] Q4, mixing the ammonium tungstate solution prepared in step Q2 and the PVA aqueous solution prepared in step Q3 in proportion to obtain an impregnation solution;
[0048] Q5, take the pretreated diamond and the impregnation solution prepared in step Q1 in proportion, heat to 50°C and stir at a stirring speed of 150 rpm, stir until dry, and obtain diamond particles coated with ammonium tungstate;
[0049] Q6, heat treating the ammonium tungstate coated diamond particles obtained in Q5, 2 -Ar mixed gas atmosphere, heat treatment at 900℃ for 2h, heating rate of 5℃ / min, H 2 -Ar gas mixture consists of 5% H 2 and 95% Ar to obtain tungsten-coated diamond particles, which are the hardness enhancer.
[0050] A method for preparing a wear-resistant non-magnetic hard alloy comprises the following steps:
[0051] S1, firstly mix carbonyl nickel powder, niobium hydride, rare earth metal oxide and graphite in proportion, add them into a planetary ball mill, and perform ball milling with isopropanol as the medium at a ball milling speed of 600 rpm for 1.5 h to obtain a binder phase powder;
[0052] S2, adding tungsten carbide, tungsten-coated diamond particles and vanadium carbide in proportion to the binder phase powder obtained in step S1, continuing ball milling with isopropanol as the medium, ball milling at a ball milling speed of 600 rpm for 3 hours, then adjusting the ball milling speed to 150 rpm and continuing ball milling for 48 hours, and drying in an oven at 70° C. for 2 hours after ball milling to obtain a mixed powder;
[0053] S3, placing the mixed powder prepared in step S2 in a graphite mold, and performing primary sintering in a vacuum plasma sintering furnace, with a sintering temperature of 500°C, a heating rate of 150°C / min, a sintering time of 4min, and a vacuum degree of 10Pa in the vacuum plasma sintering furnace, to obtain a primary sintered body;
[0054] S4, plasma sintering the primary sintered body prepared in step S3, in an Ar atmosphere, with a sintering temperature of 900° C., a heating rate of 200° C. / min, and a sintering time of 7 min, to obtain a plasma sintered body;
[0055] S5, performing secondary sintering on the plasma sintered body obtained in step S4, with a sintering temperature of 1000° C., a heating rate of 100° C. / min, and a sintering time of 10 min to obtain a sintered cemented carbide;
[0056] S6, cooling the sintered cemented carbide prepared in step S5 to room temperature in a cooling system at a cooling rate of 150°C / min to obtain the wear-resistant non-magnetic cemented carbide. Example
[0057] A wear-resistant non-magnetic hard alloy, composed of a matrix powder and a hardness enhancer, the mass fractions of which are: 95wt% of the matrix powder and 5wt% of the hardness enhancer;
[0058] The matrix powder is composed of a hard phase, a binder phase and a grain growth inhibitor. The mass fraction of each component raw material and its proportion in the matrix powder is as follows: the hard phase is 85wt% tungsten carbide, the binder phase is 9wt% carbonyl nickel powder, 4wt% niobium hydride, 0.5wt% rare earth metal oxide and 0.8wt% graphite, and the grain growth inhibitor is 0.7wt% vanadium carbide;
[0059] Tungsten carbide is in powder form, with a purity of 99.9% and a particle size of 2μm, carbonyl nickel powder is in a purity of 99% and a particle size of 3μm, niobium hydride is in a purity of 99% and a particle size of 40μm, rare earth metal oxide is one of yttrium trioxide and cerium trioxide, the purity of rare earth metal oxide is 99.9%, graphite is in a purity of 98% and a particle size of 45μm, and vanadium carbide is in a powder form, with a purity of 99.9% and a particle size of 2μm;
[0060] The hardness enhancer is tungsten-coated diamond particles, which are prepared from ammonium tungstate, diamond, and polyvinyl alcohol, and the mass ratio of ammonium tungstate, polyvinyl alcohol, and diamond is 0.3:0.07:5;
[0061] The diamond is of analytical grade with a particle size of 20 μm, the ammonium tungstate is of analytical grade with a purity of 99.99%, and the polyvinyl alcohol is of analytical grade with Mw=55,000.
[0062] The preparation method of the hardness enhancer and the preparation method of a wear-resistant non-magnetic hard alloy are consistent with those in Example 1. Example
[0063] A wear-resistant non-magnetic hard alloy, composed of a matrix powder and a hardness enhancer, the mass fractions of which are: 95wt% of the matrix powder and 5wt% of the hardness enhancer;
[0064] The matrix powder is composed of a hard phase, a binder phase and a grain growth inhibitor. The raw materials and their mass fractions in the matrix powder are as follows: the hard phase is 90wt% tungsten carbide, the binder phase is 6wt% carbonyl nickel powder, 3wt% niobium hydride, 0.1wt% rare earth metal oxide and 0.5wt% graphite, and the grain growth inhibitor is 0.4wt% vanadium carbide;
[0065] Tungsten carbide is in powder form, with a purity of 99.9% and a particle size of 2μm, carbonyl nickel powder is in a purity of 99% and a particle size of 3μm, niobium hydride is in a purity of 99% and a particle size of 40μm, rare earth metal oxide is one of yttrium trioxide and cerium trioxide, the purity of rare earth metal oxide is 99.9%, graphite is in a purity of 98% and a particle size of 45μm, and vanadium carbide is in a powder form, with a purity of 99.9% and a particle size of 2μm;
[0066] The hardness enhancer is tungsten-coated diamond particles, which are prepared from ammonium tungstate, diamond, and polyvinyl alcohol, and the mass ratio of ammonium tungstate, polyvinyl alcohol, and diamond is 0.3:0.07:5;
[0067] The diamond is of analytical grade with a particle size of 20 μm, the ammonium tungstate is of analytical grade with a purity of 99.99%, and the polyvinyl alcohol is of analytical grade with Mw=55,000.
[0068] The preparation method of the hardness enhancer and the preparation method of a wear-resistant non-magnetic hard alloy are consistent with those in Example 1. Example
[0069] A wear-resistant non-magnetic hard alloy, composed of a matrix powder and a hardness enhancer, the mass fractions of which are: 99wt% of the matrix powder and 1wt% of the hardness enhancer;
[0070] The matrix powder is composed of a hard phase, a binder phase and a grain growth inhibitor. The mass fraction of each component raw material and its proportion in the matrix powder is as follows: the hard phase is 85wt% tungsten carbide, the binder phase is 9wt% carbonyl nickel powder, 4wt% niobium hydride, 0.5wt% rare earth metal oxide and 0.8wt% graphite, and the grain growth inhibitor is 0.7wt% vanadium carbide;
[0071] Tungsten carbide is in powder form, with a purity of 99.9% and a particle size of 2μm, carbonyl nickel powder is in a purity of 99% and a particle size of 3μm, niobium hydride is in a purity of 99% and a particle size of 40μm, rare earth metal oxide is one of yttrium trioxide and cerium trioxide, the purity of rare earth metal oxide is 99.9%, graphite is in a purity of 98% and a particle size of 45μm, and vanadium carbide is in a powder form, with a purity of 99.9% and a particle size of 2μm;
[0072] The hardness enhancer is tungsten-coated diamond particles, which are prepared from ammonium tungstate, diamond, and polyvinyl alcohol, and the mass ratio of ammonium tungstate, polyvinyl alcohol, and diamond is 0.3:0.07:5;
[0073] The diamond is of analytical grade with a particle size of 20 μm, the ammonium tungstate is of analytical grade with a purity of 99.99%, and the polyvinyl alcohol is of analytical grade with Mw=55,000.
[0074] The preparation method of the hardness enhancer and the preparation method of a wear-resistant non-magnetic hard alloy are consistent with those in Example 1. Example
[0075] A wear-resistant non-magnetic hard alloy, composed of a matrix powder and a hardness enhancer, the mass fractions of which are: 90wt% of the matrix powder and 10wt% of the hardness enhancer;
[0076] The matrix powder is composed of a hard phase, a binder phase and a grain growth inhibitor. The mass fraction of each component raw material and its proportion in the matrix powder is as follows: the hard phase is 85wt% tungsten carbide, the binder phase is 9wt% carbonyl nickel powder, 4wt% niobium hydride, 0.5wt% rare earth metal oxide and 0.8wt% graphite, and the grain growth inhibitor is 0.7wt% vanadium carbide;
[0077] Tungsten carbide is in powder form, with a purity of 99.9% and a particle size of 2μm, carbonyl nickel powder is in a purity of 99% and a particle size of 3μm, niobium hydride is in a purity of 99% and a particle size of 40μm, rare earth metal oxide is one of yttrium trioxide and cerium trioxide, the purity of rare earth metal oxide is 99.9%, graphite is in a purity of 98% and a particle size of 45μm, and vanadium carbide is in a powder form, with a purity of 99.9% and a particle size of 2μm;
[0078] The hardness enhancer is tungsten-coated diamond particles, which are prepared from ammonium tungstate, diamond, and polyvinyl alcohol, and the mass ratio of ammonium tungstate, polyvinyl alcohol, and diamond is 0.3:0.07:5;
[0079] The diamond is of analytical grade with a particle size of 20 μm, the ammonium tungstate is of analytical grade with a purity of 99.99%, and the polyvinyl alcohol is of analytical grade with Mw=55,000.
[0080] The preparation method of the hardness enhancer and the preparation method of a wear-resistant non-magnetic hard alloy are consistent with those in Example 1.
[0081] Comparative Example 1:
[0082] Based on Example 2, the difference is that no tungsten-coated diamond particles are added, the matrix powder accounts for 100wt%, and the rest of the preparation method and proportion are consistent with Example 2.
[0083] Comparative Example 2:
[0084] Based on Example 2, the difference is that diamond particles are directly used without tungsten coating, and the rest of the preparation method and proportion are consistent with Example 2.
[0085] Experimental example:
[0086] 1. Magnetic induction intensity measurement:
[0087] Use DC Gauss meter, multi-range DC ammeter, DC regulated power supply, sliding line rheostat and ring test specimen according to Figure 1 The circuit shown in the figure is connected, and the size of the ring sample meets the following requirements to ensure that the strength of the ring is uniform at all locations on the cross section, that is (D 0 -D 1 ) / (D 0 +D 1 )≤1 / 9, where D 0 is the outer diameter, D 1 The inner diameter of the test sample should be smooth and regular, and as small as possible while meeting the requirements of immersion measurement of the Gaussmeter probe to reduce magnetic leakage. It is generally believed that the influence of magnetic leakage can be ignored at 1 / 10Oe.
[0088] Test parameters: outer diameter of annular sample D 0 =60mm, inner diameter D 1 =50mm, thickness t=5mm, air gap length L 0 =5mm, the number of coil turns is 1000, and the test is carried out at room temperature. In the test, the magnetism of the material refers to the magnitude of the magnetization ability under the action of the external magnetic field, that is, the larger the magnetism, the easier the material is to magnetize, and its change is consistent with the change of magnetic permeability.
[0089] The variation of magnetic induction intensity of each embodiment and comparative example sample with current is shown in Table 1 and Figure 4 shown.
[0090] 2. Wear resistance test:
[0091] A sample with a size of 15 mm × 15 mm × 5 mm was prepared, and the wear resistance of the wear-resistant non-magnetic cemented carbide sample was tested using a reciprocating friction and wear tester; the reciprocating friction was carried out at room temperature, and the grinding ball was Φ4 mm Al 2 O 3 The ball, load is 30N, reciprocating friction length is 5mm, friction speed is 200mm / min, friction time is 30min, weigh the sample before and after the friction test, and calculate the wear rate according to the following formula:
[0092] K = (mm 0 ) / t;
[0093] K——wear rate, mg / min;
[0094] m 0 ——mass before friction test, mg;
[0095] m——mass after friction test, mg;
[0096] t——friction time, min.
[0097] The wear rates of the samples of the embodiments and comparative examples are shown in Table 2 and Figure 2 shown.
[0098] 3. Hardness test:
[0099] The hardness test was conducted using a Rockwell hardness tester, with a steel ball diameter of 10 mm, a load of 30D2 = 30000 N, and a duration of 10 s.
[0100] The hardness test results of the samples of the embodiments and comparative examples are shown in Table 2 and Figure 2 shown.
[0101] 4. Tensile test:
[0102] The tensile test adopts a hydraulic tensile testing machine, and the specimens are processed into standard specimens with a diameter of 10 mm and a gauge length of 100 mm. The test conditions are: at room temperature with a chuck moving speed of 2 mm / min, and the specimens are subjected to tensile tests to obtain the tensile strength and yield strength of the specimens.
[0103] The tensile strength and yield strength of the samples of each embodiment and comparative example are shown in Table 2 and Figure 3 shown.
[0104] Table 1 Magnetic induction intensity of each embodiment and comparative example sample
[0105]
[0106] Table 2 Wear rate, hardness, tensile strength and yield strength of samples of various embodiments and comparative examples
[0107]
[0108] Through the experimental examples, the magnetic induction intensity, wear rate, and hardness of each embodiment and comparative sample were tested, and tensile tests were performed to determine their tensile strength and yield strength. From the test results, the influence of non-magnetic wear-resistant alloy components on its performance can be explored. First, the magnetic induction intensity was tested under different currents, as shown in Table 1 and Figure 4 As shown in the figure, it can be seen that the use of non-magnetic tungsten coated diamond particles has a significant effect on reducing or avoiding the magnetism caused by impurities in artificial diamonds. While improving the hardness and wear resistance of the alloy, the magnetism of the sample is basically not affected, and the electromagnetic induction intensity is maintained at the bottom under high current; secondly, the wear rate and hardness of each sample are measured. Through Table 2 and Figure 2 It can be seen that with the increase of tungsten carbide content and tungsten coated diamond particle content, the hardness and wear resistance of the sample can be improved, while the wear resistance and hardness of the sample without tungsten coated diamond particles are reduced. Although the diamond is not tungsten coated, the hardness and wear resistance of the sample are reduced due to the easy graphitization of diamond during the sintering process. It can be seen that tungsten coating has a significant effect on avoiding or alleviating diamond graphitization. Finally, the sample is subjected to a tensile test to obtain its yield strength and tensile strength. The results in Table 2 and Figure 3 It can be seen that the yield strength and tensile strength of the sample are positively correlated with the addition amount of tungsten-coated diamond particles and the proportion of tungsten carbide. However, diamond and its graphitization will increase the toughness of the sample, but excessive amounts will increase its brittleness and have a negative impact on the mechanical properties.
[0109] The present invention and its embodiments are described above. The described embodiments are only some embodiments of the present invention, not all embodiments. The drawings are only one of many embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but only represents the selected embodiments of the present invention. Based on this, other specific embodiments of the present invention obtained by those skilled in the art under the inspiration of the technical solution without creative labor should fall within the protection scope of the present invention.
Claims
1. A wear-resistant non-magnetic hard alloy, characterized in that: It is composed of base powder and hardness enhancer, with the mass fractions being: base powder 90~99wt%, hardness enhancer 1~10wt%; The matrix powder is composed of a hard phase, a binder phase and a grain growth inhibitor, and the mass fraction of each component raw material in the matrix powder is as follows: the hard phase is 80-90wt% of tungsten carbide, the binder phase is 6-12wt% of carbonyl nickel powder, 3-5wt% of niobium hydride, 0.1-1wt% of rare earth metal oxide and 0.5-1wt% of graphite, and the grain growth inhibitor is 0.4-1wt% of vanadium carbide; The tungsten carbide is in powder form, with a purity of 99.9% and a particle size of 2 μm, the carbonyl nickel powder is in a purity of 99% and a particle size of 2-3 μm, the niobium hydride is in a purity of 99% and a particle size of 40-45 μm, the rare earth metal oxide is one of yttrium trioxide and cerium trioxide, the purity of the rare earth metal oxide is 99.9%, the graphite is in a purity of 98% and a particle size of 45 μm, and the vanadium carbide is in a powder form, with a purity of 99.9% and a particle size of 2 μm; The hardness enhancer is tungsten-coated diamond particles, which are prepared from ammonium tungstate, diamond, and polyvinyl alcohol, and the mass ratio of ammonium tungstate, polyvinyl alcohol, and diamond is 0.1-0.5:0.05-0.1:5; The diamond is of analytical grade with a particle size of 15-25 μm, the ammonium tungstate is of analytical grade with a purity of 99.99%, and the polyvinyl alcohol is of analytical grade with Mw=30000-70000.
2. The wear-resistant non-magnetic hard alloy according to claim 1, characterized in that: The preparation of the hardness enhancer comprises the following steps: Q1, take the diamond and use distilled water to ultrasonically clean it for 10-20 minutes until there is no impurity on the surface, treat it in 65wt% nitric acid for 15-25 hours to roughen its surface, then use deionized water and anhydrous ethanol to clean it in turn to make no nitric acid residue on the surface, and bake it in an oven at 80℃ for 20 minutes until it is dry to obtain pretreated diamond; Q2, weigh ammonium tungstate according to the proportion, add it into deionized water, heat it to 50℃ and stir until dissolved, the stirring speed is 200~300rpm, and obtain ammonium tungstate solution; Q3, weigh polypropylene alcohol according to proportion and add it into deionized water, heat it to 90°C until the polypropylene alcohol is dissolved, to obtain a PVA aqueous solution; Q4, mixing the ammonium tungstate solution prepared in step Q2 and the PVA aqueous solution prepared in step Q3 in proportion to obtain an impregnation solution; Q5, taking the pretreated diamond and the impregnation solution prepared in step Q1 in proportion, heating to 50°C and stirring at a stirring speed of 100-200 rpm, stirring until dry, to obtain diamond particles coated with ammonium tungstate; Q6, heat treating the ammonium tungstate coated diamond particles obtained in Q5 at 700-1100°C for 1-3h in a H2-Ar mixed gas atmosphere with a heating rate of 5°C / min to obtain tungsten coated diamond particles, which are the hardness enhancer.
3. The wear-resistant non-magnetic hard alloy according to claim 2, characterized in that: The mass fraction of the ammonium tungstate solution in step Q2 is 5-15wt%, and the mass fraction of the PVA aqueous solution in step Q3 is 5-15wt%.
4. The wear-resistant non-magnetic hard alloy according to claim 3, characterized in that: The H2-Ar mixed gas described in step Q6 consists of 5% H2 and 95% Ar.
5. A method for preparing wear-resistant non-magnetic hard alloy according to claim 4, characterized in that: The following steps are involved: S1, firstly mix carbonyl nickel powder, niobium hydride, rare earth metal oxide and graphite in proportion, add them into a planetary ball mill, and perform ball milling with isopropanol as the medium at a ball milling speed of 600 rpm for 1-2 h to obtain a binder phase powder; S2, adding tungsten carbide, tungsten-coated diamond particles and vanadium carbide in proportion to the binder phase powder obtained in step S1, continuing ball milling with isopropanol as the medium, ball milling at a ball milling speed of 600 rpm for 3 hours, then adjusting the ball milling speed to 150 rpm and continuing ball milling for 48 hours, and drying in an oven at 70° C. for 2 hours after ball milling to obtain a mixed powder; S3, placing the mixed powder prepared in step S2 in a graphite mold, and performing primary sintering in a vacuum plasma sintering furnace at a sintering temperature of 400-600° C., a heating rate of 150° C. / min, and a sintering time of 2-5 min to obtain a primary sintered body; S4, plasma sintering the primary sintered body prepared in step S3, in an Ar atmosphere, with a sintering temperature of 800-1000° C., a heating rate of 200° C. / min, and a sintering time of 4-10 min, to obtain a plasma sintered body; S5, performing secondary sintering on the plasma sintered body obtained in step S4, with a sintering temperature of 900-1100° C., a heating rate of 100° C. / min, and a sintering time of 8-12 min to obtain a sintered cemented carbide; S6, cooling the sintered cemented carbide prepared in step S5 to room temperature in a cooling system at a cooling rate of 150°C / min to obtain the wear-resistant non-magnetic cemented carbide.
6. The method for preparing a wear-resistant non-magnetic hard alloy according to claim 5, characterized in that: The vacuum degree of the vacuum plasma sintering furnace in step S3 is 10Pa.
Citation Information
Patent Citations
Manufacturing method for diamond honing oilstone
CN105772730A
Hard alloy composite material, and preparation method and application thereof
CN106868374A