Photovoltaic cell, preparation method and photovoltaic cell assembly

By stacking dielectric layers and metal layers on the first passivation layer of TOPCon photovoltaic cells to form a back-reverse structure and electrically isolated from each other, the problems of poor long-wavelength response and reduced fill factor of photovoltaic cells are solved, and the photoelectric conversion efficiency and short-circuit current are improved. density.

CN118738152APending Publication Date: 2024-10-01JA SOLAR TECH YANGZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410996641.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

TOPCon photovoltaic cells have poor spectral responsiveness in the long-wavelength band, resulting in infrared light escape loss and limited photoelectric conversion efficiency. The direct contact between the metal back-reverse structure and the main grid results in a reduction in fill factor.

Method used

A dielectric layer and a metal layer are stacked on the first passivation layer of the substrate to form a back-reverse structure, and the metal layer and the main grid are electrically separated by the dielectric layer to avoid direct contact and improve the long-wavelength spectral response of the photovoltaic cell.

Benefits of technology

The photoelectric conversion efficiency and short-circuit current density of photovoltaic cells are improved, and the escape loss of long-wavelength light is reduced while keeping the fill factor unchanged.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738152A_ABST
    Figure CN118738152A_ABST
Patent Text Reader

Abstract

The invention provides a photovoltaic cell, a preparation method and a photovoltaic cell assembly, relates to the technical field of photovoltaics, and aims to solve the technical problem that a photovoltaic cell is poor in spectral responsiveness to a long wave band. The photovoltaic cell comprises a substrate, a main grid, a dielectric layer, a metal layer and a first passivation layer stacked on the substrate, and the dielectric layer is stacked on the side, away from the substrate, of the passivation layer and located on other areas, except the main grid, of the first passivation layer; the metal layer is stacked on the side, away from the first passivation layer, of the dielectric layer and is separated from the main grid, and the metal layer and the first passivation layer are electrically separated through the dielectric layer. According to the photovoltaic cell, the responsiveness of a long-wave-band spectrum is improved, the short-circuit current density is improved, and the photoelectric conversion efficiency is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photovoltaic technology, and in particular to a photovoltaic cell, a preparation method, and a photovoltaic cell assembly. Background Art

[0002] The statements in this section merely provide background art related to the present invention and do not necessarily constitute prior art.

[0003] Among the Tunnel Oxide Passivated Contact (TOPCon) photovoltaic cells, N-type TOPCon photovoltaic cells have the characteristics of high power generation and strong stability due to their high minority carrier lifetime and low photo-induced attenuation. Although TOPCon photovoltaic cells have excellent passivation effect and obtain good open circuit voltage by using back tunneling oxide passivation contact, the absorption coefficient of crystalline silicon in the 900nm~1200nm band is low, and in order to reduce costs, the thickness of silicon wafers is continuously reduced. Thinner silicon wafers will cause a large amount of infrared light escape loss, which limits the improvement of the short-circuit current density Jsc of TOPCon photovoltaic cells, and also restricts the improvement of photoelectric conversion efficiency. Summary of the invention

[0004] The object of the present invention is to provide a photovoltaic cell, a preparation method, and a photovoltaic cell assembly to solve the technical problem that the photovoltaic cell has poor spectral responsiveness to long-wave bands.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] In a first aspect, the present invention provides a photovoltaic cell, comprising a substrate, a main grid, a dielectric layer, a metal layer, and a first passivation layer stacked on the substrate.

[0007] The dielectric layer is stacked on a side of the first passivation layer facing away from the substrate, and is located on other regions of the first passivation layer except the main gate;

[0008] The metal layer is stacked on a side of the dielectric layer away from the first passivation layer and is spaced apart from the main gate.

[0009] The metal layer and the first passivation layer are electrically isolated from each other by the dielectric layer.

[0010] According to at least one embodiment of the present invention, the dielectric layer is spaced apart from the main gate.

[0011] According to at least one embodiment of the present invention, there is a first distance between the dielectric layer and the main gate, and there is a second distance between the metal layer and the main gate, and the second distance is equal to or greater than the first distance.

[0012] According to at least one embodiment of the present invention, the material of the dielectric layer includes at least one of silicon oxide, silicon nitride, titanium oxide, aluminum oxide or magnesium fluoride; and / or,

[0013] The material of the metal layer includes at least one of gold, silver, aluminum or copper.

[0014] According to at least one embodiment of the present invention, the thickness of the dielectric layer ranges from 1 nm to 300 nm; and / or,

[0015] The thickness of the metal layer ranges from 200 nm to 1000 nm.

[0016] According to at least one embodiment of the present invention, the substrate includes a silicon substrate or a germanium substrate.

[0017] According to at least one embodiment of the present invention, the photovoltaic cell comprises one of a tunneling oxide passivation contact photovoltaic cell and an interdigitated back contact photovoltaic cell.

[0018] According to at least one embodiment of the present invention, the photovoltaic cell further includes a tunneling oxide layer and a doped polysilicon layer, wherein the tunneling oxide layer and the doped polysilicon layer are stacked between the substrate and the first passivation layer, and the tunneling oxide layer and the doped polysilicon layer are arranged in a direction away from the substrate.

[0019] According to at least one embodiment of the present invention, the photovoltaic cell further includes a diffusion layer, a second passivation layer and a passivation anti-reflection layer, wherein the diffusion layer, the second passivation layer and the passivation anti-reflection layer are sequentially formed on a side of the substrate away from the first passivation layer, and the diffusion layer, the second passivation layer and the passivation anti-reflection layer are arranged in a direction away from the substrate.

[0020] According to at least one embodiment of the present invention, the doped polysilicon layer is a phosphorus-doped polysilicon layer, and the diffusion layer is a boron-doped diffusion layer.

[0021] In a second aspect, the present invention further provides a method for preparing a photovoltaic cell, comprising:

[0022] providing a substrate stacked with a first passivation layer;

[0023] A dielectric layer is stacked on a side of the first passivation layer facing away from the substrate, and the dielectric layer is located on other regions of the first passivation layer except the main gate;

[0024] stacking a metal layer on a side of the dielectric layer away from the first passivation layer, and spacing the metal layer from the main gate;

[0025] The metal layer and the first passivation layer are electrically isolated by the dielectric layer.

[0026] According to at least one embodiment of the present invention, the step of stacking a dielectric layer on a side of the first passivation layer facing away from the substrate, wherein the dielectric layer is located on other regions of the first passivation layer except the main gate, comprises:

[0027] Covering the first mask plate on the side of the first passivation layer away from the substrate and shielding the main grid, wherein the width of the first shielding strip of the first mask plate shielding the main grid is greater than or equal to the width of the corresponding main grid;

[0028] The dielectric material is evaporated to form the dielectric layer on the first passivation layer.

[0029] According to at least one embodiment of the present invention, when the width of the first shielding strip is greater than the width of the corresponding main grid, a dielectric material is evaporated to form the dielectric layer on the first passivation layer, wherein the dielectric layer is spaced apart from the main grid.

[0030] According to at least one embodiment of the present invention, the step of stacking a metal layer on a side of the dielectric layer away from the first passivation layer and separating the metal layer from the main gate includes:

[0031] Covering the second mask plate on the side of the dielectric layer away from the first passivation layer and shielding the main grid, wherein the width of the second shielding strip of the second mask plate shielding the main grid is greater than or equal to the width of the first shielding strip of the first mask plate;

[0032] The metal layer is formed by evaporating a metal material on the dielectric layer.

[0033] According to at least one embodiment of the present invention, the step of stacking a dielectric layer on a side of the first passivation layer facing away from the substrate, wherein the dielectric layer is located on other regions of the first passivation layer except the main gate, comprises:

[0034] In a vacuum environment, the deposition rate of the dielectric layer is and / or,

[0035] The material of the dielectric layer includes at least one of silicon oxide, silicon nitride, titanium oxide, aluminum oxide or magnesium fluoride.

[0036] According to at least one embodiment of the present invention, the step of stacking a metal layer on a side of the dielectric layer away from the first passivation layer and separating the metal layer from the main gate includes:

[0037] In a vacuum environment, the deposition rate of the metal layer to a first preset thickness is The deposition rate of the metal layer from the first preset thickness to the second preset thickness is The deposition rate of the metal layer from the second preset thickness to the third preset thickness is The deposition rate of the metal layer from the third preset thickness to the fourth preset thickness is Wherein, the first preset thickness, the second preset thickness, the third preset thickness and the fourth preset thickness increase in sequence; and / or,

[0038] The material of the metal layer includes at least one of gold, silver, aluminum, or copper.

[0039] In a third aspect, the present invention further provides a photovoltaic cell assembly, comprising a plurality of electrically connected photovoltaic cells, at least one of which is the photovoltaic cell described in the first aspect, or,

[0040] At least one of the photovoltaic cells is a photovoltaic cell prepared by the preparation method described in the second aspect.

[0041] Among the one or more technical solutions provided in the exemplary embodiments of the present invention, at least one of the following beneficial effects can be achieved.

[0042] The photovoltaic cell of the exemplary embodiment of the present invention forms a back-reflection structure by stacking a dielectric layer and a metal layer on the passivation layer, so that the spectral response of the photovoltaic cell to the long-wave band is significantly increased, and the escape loss of the incident light is reduced, thereby obtaining a higher photoelectric conversion efficiency. The metal layer and the passivation layer are electrically isolated by the dielectric layer, which can avoid the carrier recombination caused by the direct contact between the fine grid on the passivation layer and the metal layer, so that the metal layer can enhance the optical absorption of the photovoltaic cell. At the same time, the applicant found that the carrier mobility of the metal layer is lower than the carrier mobility of the main grid, and the direct contact between the two will also cause carrier recombination at the contact position, thereby reducing the filling factor of the photovoltaic cell. Therefore, by separating the metal layer from the main grid and electrically isolating the metal layer from the fine grid through the dielectric layer, the back-reflection structure formed by the dielectric layer and the metal layer can be used to improve the responsiveness of the photovoltaic cell in the long-wave spectrum, increase the short-circuit current density, and thus improve the photoelectric conversion efficiency while ensuring that the filling factor of the photovoltaic cell remains unchanged. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The accompanying drawings illustrate exemplary embodiments of the present invention and together with the description serve to explain the principles of the present invention, and these drawings are included to provide a further understanding of the present invention and are incorporated in and constitute a part of this specification;

[0044] Figure 1 is a schematic cross-sectional structural diagram of a TOPCon photovoltaic cell according to an embodiment of the present invention;

[0045] Figure 2 is a schematic diagram of a top view structure of a first mask according to an embodiment of the present invention;

[0046] Figure 3 1 is a test curve of internal quantum efficiency and reflectivity of a TOPCon photovoltaic cell stacked with a back-inverted structure before and after the stacking according to an embodiment of the present invention;

[0047] Figure 4 2 is a test curve of the external quantum efficiency of the TOPCon photovoltaic cell stacked before and after the back-inverted structure according to an embodiment of the present invention;

[0048] Figure 5 Schematic diagram of a process for preparing a photovoltaic cell according to an embodiment of the present invention.

[0049] Figure numerals: 10, substrate; 21, tunneling oxide layer; 22, doped polysilicon layer; 23, first passivation layer; 24, dielectric layer; 25, metal layer; 26, main gate; 31, diffusion layer; 32, second passivation layer; 33, passivation anti-reflection layer; 34, gate; 40, first mask; 41, first shielding strip. DETAILED DESCRIPTION

[0050] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0051] Before introducing the embodiments of the present invention, the following definitions are given for the relevant terms involved in the embodiments of the present invention:

[0052] The main grid, also known as the busbar, is a wider metal conductive path that collects the current conducted from the thin grid lines and conducts it to the external circuit. The main grid lines are usually made of silver, aluminum or other highly conductive materials to ensure low resistance loss and high efficiency. The main grid lines generally span the entire photovoltaic cell, usually 2 to 5 or more, arranged in parallel. They need to be wide enough to reduce resistance, but not too wide, otherwise they will block too much light and reduce the light absorption efficiency of the photovoltaic cell.

[0053] Finger, also known as fine grid line (Finger), is a relatively narrow conductive path responsible for collecting charge carriers (electrons and holes) from the surface of photovoltaic cells and conducting them to the main grid line. Finger is usually made of highly conductive materials such as silver paste. Finger forms a grid-like structure on the surface of the cell, covering most of the cell surface area. Finger needs to be fine enough to maximize light absorption while ensuring that the resistance is not too high. The density and layout of the fine grid need to be optimized to capture and conduct as much charge as possible without significantly increasing the resistance.

[0054] Plasmon is a quantum excitation that exists on the metal surface. It is the result of the interaction between electrons and electromagnetic fields. When light shines on the metal surface, the free electrons in the metal will vibrate under the action of the electric field, thus forming plasmons. Plasmons have many special properties, including surface enhanced Raman scattering, local field enhancement equivalent, surface enhanced fluorescence, etc.

[0055] A carrier is a charged particle that participates in the transmission of electric current in a semiconductor material. It can be an electron or a hole. In semiconductors, electrons are the main carriers, and they conduct electric current by moving in the crystal lattice. When electrons gain energy from atoms and jump into the conduction band, they become free carriers, able to move in the material and conduct electricity. On the other hand, holes are positively charged carriers that are left behind as a result of the jump of electrons in the valence band. The movement of carriers is the basis for the operation of semiconductor devices, including transistors, diodes, etc.

[0056] Fill Factor (FF) can be used to measure the impact of internal resistance and electron loss on the performance of photovoltaic devices in photovoltaic cells and other optoelectronic devices. Fill factor is a characteristic of the current-voltage (IV) curve. Fill factor represents the ratio of the maximum output power ImVm to the limit output power IscVoc, that is: FF = ImVm / IscVoc.

[0057] The fill factor ranges from 0 to 1. The closer it is to 1, the better the performance of the optoelectronic device. The fill factor is mainly determined by the series resistance, bypass resistance and PN junction characteristics. When the series resistance increases, the bypass resistance decreases, and there are defects and impurities in the PN junction, the FF will become smaller. In addition, the fill factor increases with the increase of the bandgap width of the battery material.

[0058] Short Circuit Current Density (Jsc) refers to the current density per unit area generated by a photovoltaic cell in a short circuit state. In the short circuit state, the two electrodes of the photovoltaic cell are directly connected together without external load. Its value is expressed as the intercept size of the vertical axis in the JV curve diagram, and the unit is mA / cm 2 Jsc is mainly affected by the intensity of incident light and the size of the material absorption band gap. The smaller the band gap, the stronger the ability to convert photons into electrical energy. In addition, the thickness of the device, the quality of each layer of film, and the carrier transmission capacity will also affect the size of Jsc.

[0059] Open circuit voltage (Voc) refers to the voltage difference between the two electrodes when the photovoltaic cell is not connected to any load. The specific value of the open circuit voltage is expressed as the intercept length on the horizontal axis in the JV curve diagram, and its unit is generally mV or V.

[0060] External Quantum Efficiency (EQE) refers to the efficiency of a photoelectric device (such as a photovoltaic cell or a photodiode) in generating current under external light irradiation. It is one of the important indicators for measuring device performance and is usually expressed as a percentage. Specifically, the external quantum efficiency is expressed by measuring the ratio of the number of electron-hole pairs generated in the device per unit energy photon to the number of incident photons.

[0061] Internal Quantum Efficiency (IQE) refers to the efficiency with which photons are absorbed and converted into electron-hole pairs in optoelectronic devices (such as LEDs, photovoltaic cells, etc.). It measures the efficiency with which electron-hole pairs are generated in a device. For photovoltaic cells, the internal quantum efficiency indicates the efficiency with which photon energy is converted into electron energy. A high internal quantum efficiency means that photovoltaic cells can more efficiently convert sunlight into electrical energy.

[0062] In the related technology, TOPCon photovoltaic cells use back-side tunneling oxidation passivation contact, which has excellent passivation effect and obtains a good open-circuit voltage. However, the continuously thinning silicon wafer thickness will cause a large amount of infrared light escape loss, limiting the improvement of the short-circuit current density Jsc of TOPCon photovoltaic cells. Depositing metal nanoparticles separately on TOPCon photovoltaic cells with printed grid lines (including fine grids and main grids) to construct a back-reflective structure can improve the infrared spectral response of photovoltaic cells.

[0063] However, the above-mentioned metal back-inverted structure deposited directly on the grid line will cause the metal to directly contact the fine grid, resulting in carrier recombination, which will reduce the fill factor of the photovoltaic cell. The applicant has found that when the metal back-inverted structure is in direct contact with the main grid, the conductivity of the metal back-inverted structure is less than that of the main grid, which will also reduce the conductivity of the main grid, thereby reducing the fill factor of the photovoltaic cell.

[0064] In response to the above problems, in a photovoltaic cell provided by an exemplary embodiment of the present invention, a metal layer is stacked on a dielectric layer by depositing metal nanoparticles to form a back-reflective structure. Driven by a light field of a specific frequency, free electrons on the surface of the metal nanoparticles interact with photons to form a localized surface plasmon resonance. The resonance can significantly enhance the local field on the surface of the metal nanoparticles, thereby producing multi-angle scattering of the incident light, effectively extending the optical path of the light in the absorbing medium, and especially improving the spectral response in the long-wave band. Furthermore, the metal layer is electrically isolated from the fine grid by the dielectric layer, and at the same time, the metal layer is separated from the main grid located in the back field, so that the metal layer in the back-reflective structure avoids direct contact with both the fine grid and the main grid, which can significantly improve the reflectivity of the photovoltaic cell in the long-wave band while ensuring that the fill factor remains unchanged, which is beneficial to reducing the escape loss of the long-wave band light and improving the spectral response of the photovoltaic cell to the long-wave band.

[0065] The following description will be made using TOPCon photovoltaic cells as an example, but it should not be understood that the structure of the present invention can only be a TOPCon photovoltaic cell. For example, it can also be an interdigitated back contact photovoltaic cell (Interdigitated Back Contact, IBC) and the like.

[0066] Figure 1 Schematic diagram of the cross-sectional structure of a TOPCon photovoltaic cell according to an embodiment of the present invention. Figure 1 As shown, the TOPCon photovoltaic cell provided by the exemplary embodiment of the present invention includes a substrate 10, and on the light-receiving surface of the substrate 10, that is, the front side of the photovoltaic cell, it includes a diffusion layer 31, a second passivation layer 32 and a passivation anti-reflection layer 33 in sequence along the direction away from the substrate 10. The front side of the TOPCon photovoltaic cell is also printed with grid lines, including a front main grid (grid 34) and a front fine grid line (not shown in the figure). In the back field of the substrate 10, that is, the back side of the photovoltaic cell, it includes a tunneling oxide layer 21, a doped polysilicon layer 22, and a first passivation layer 23 in sequence along the direction away from the substrate 10. The back field of the photovoltaic cell is also printed with grid lines, including a back field main grid 26 and a back field fine grid (not shown in the figure). It should be noted that, Figure 1 The cross section of the TOPCon photovoltaic cell shown is a cross section perpendicular to the extension direction of the main grid 26 .

[0067] Exemplarily, the diffusion layer 31 may be a boron-doped diffusion layer, the second passivation layer 32 may be formed of at least one of aluminum oxide, silicon oxide, gallium oxide, silicon nitride, aluminum nitride, silicon oxynitride, and aluminum oxynitride; the doped polysilicon layer 22 may be a phosphorus-doped polysilicon layer.

[0068] For the convenience of description, unless otherwise specified, the main gate mentioned below refers to the main gate 26 of the back field, and the fine gate refers to the fine gate in the back field.

[0069] like Figure 1 As shown, the TOPCon photovoltaic cell of the exemplary embodiment of the present invention also includes a back-inverted structure formed by a dielectric layer 24 and a metal layer 25 in the back field. The dielectric layer 24 is stacked on the side of the first passivation layer 23 away from the substrate 10, and is located on the other regions of the first passivation layer 23 except the main grid 26. The metal layer 25 is stacked on the side of the dielectric layer 24 away from the first passivation layer 23, and is spaced apart from the main grid 26. That is, the dielectric layer 24 completely electrically isolates the fine grid on the first passivation layer 23 from the metal layer 25, so as to avoid the loss of carrier collection caused by direct contact between the metal layer 25 and the fine grid. At the same time, the metal layer 25 is also spaced apart from the main grid 26, that is, the metal layer 25 and the main grid 26 will not be in direct contact, avoiding the problem of reduced conductivity of the main grid caused by the conductivity of the metal layer 25 being less than the conductivity of the main grid 26, and ensuring that the fill factor of the photovoltaic cell will not be reduced. Based on this, the back-inverted structure of the photovoltaic cell of the exemplary embodiment of the present invention can effectively improve the optical absorption of the TOPCon photovoltaic cell while ensuring that the fill factor remains unchanged, especially the spectral response in the long-wave band is significantly improved, thereby effectively improving the short-circuit current density and photoelectric conversion efficiency of the TOPCon photovoltaic cell.

[0070] In some embodiments, Figure 1 As shown, the dielectric layer 24 is spaced apart from the main grid 26, that is, there is a certain distance between the dielectric layer 24 and the main grid 26 on both sides in the width direction. When the dielectric layer 24 is in direct contact with the main grid 26, the conductivity of the main grid 26 will be affected, thereby reducing the fill factor. Based on this, when the dielectric layer 24 is spaced apart from the main grid 26, the above-mentioned adverse effects caused by the direct contact between the two can be avoided.

[0071] Example 1: Preparation of an N-type TOPCon photovoltaic cell, comprising:

[0072] S1, performing texturing and boron diffusion on the front side of an N-type single crystal silicon wafer to obtain a diffusion layer 31;

[0073] S2, depositing a 0.5nm to 3nm silicon oxide tunneling oxide layer 21 and a 50nm to 150nm doped polysilicon layer 22 on the back side of the N-type single crystal silicon wafer, wherein the doping element is phosphorus;

[0074] S3, depositing a second passivation layer 32 and a passivation anti-reflection layer 33 on the diffusion layer 31, wherein the second passivation layer 32 / passivation anti-reflection layer 33 is an aluminum oxide / silicon nitride stacked structure; depositing a first passivation layer 23 on the doped polysilicon layer 22, wherein the first passivation layer 23 is an aluminum oxide layer;

[0075] S4, depositing a back-inverted structure on the first passivation layer 23, wherein the dielectric layer 24 in the back-inverted structure is made of MgF2, and the metal layer 25 is made of Ag;

[0076] S5. Print the main grid and fine grid paste on the front and back sides and sinter them to form a metal electrode on the front side and a metal electrode on the back side. The metal electrode on the back side penetrates the first passivation layer 23 and contacts the doped polysilicon layer 22. The back-inverted structure is separated from the metal electrode on the back side to form a TOPCon photovoltaic cell.

[0077] Comparative Example: The only difference between this comparative example and Example 1 is that the preparation of the TOPCon photovoltaic cell does not include step S4.

[0078] Figure 3 1 is a test curve of the internal quantum efficiency and reflectivity of the TOPCon photovoltaic cell stacked with the back-inverted structure before and after according to the embodiment of the present invention. Figure 3 As shown, the horizontal axis is the spectral wavelength (wavelength), and the vertical axis is the internal quantum efficiency (IQE) and reflectivity (R%). In Example 1, a TOPCon photovoltaic cell with a MgF2 / Ag stacked back-inverted structure was prepared. The average reflectivity in the 900nm-1200nm band is greater than the average reflectivity of the photovoltaic cell without a back-inverted structure in the comparative example. The excellent reflection characteristics for long-wave light are more helpful to improve the long-wave spectral response of the TOPCon cell. At the same time, it can be seen from the internal quantum efficiency test results that the TOPCon photovoltaic cell with a MgF2 / Ag stacked back-inverted structure prepared in Example 1 has a significantly improved spectral response in the 900nm-1200nm band compared to the comparative example, which increases the short-circuit current density of the TOPCon photovoltaic cell.

[0079] Figure 4 : is a test curve of the external quantum efficiency of the TOPCon photovoltaic cell stacked before and after the back-inverted structure according to the embodiment of the present invention. Figure 4 As shown, the horizontal axis is the spectral wavelength (wavelength), and the vertical axis is the external quantum efficiency (EQE). In Example 1, a TOPCon photovoltaic cell with a MgF2 / Ag stacked back-inverted structure was prepared. The spectral response in the 900nm-1200nm band was significantly improved compared with the spectral response of the comparative example, and the short-circuit current density obtained based on EQE was increased by 0.283mA / cm 2 It should be noted that the current density is calculated by the software based on the EQE integral.

[0080] Depend on Figure 3 and Figure 4The test results show that the TOPCon photovoltaic cell with MgF2 / Ag stacked back-inverted structure can effectively improve the optical absorption of the TOPCon photovoltaic cell while ensuring the fill factor remains unchanged, especially improve the spectral response in the long-wave band, thereby improving the photoelectric conversion efficiency of the TOPCon photovoltaic cell.

[0081] Considering that when the metal layer 25 is stacked on the dielectric layer 24, the metal particles forming the metal layer 25 may bypass the dielectric layer 24 and directly contact the fine gate or the main gate 26, thereby causing a reduction in the fill factor due to carrier recombination. In order to avoid this situation as much as possible, there is a first spacing L1 between the dielectric layer 24 and the main gate 26, and a second spacing L2 between the metal layer 25 and the main gate 26, and the second spacing L2 is equal to or greater than the first spacing L1.

[0082] like Figure 1 As shown, the two sides of the main grid 26 refer to the two sides of the main grid 26 in the width direction, and the width direction is perpendicular to the extension direction of the main grid 26. The first spacing L1 between the dielectric layer 24 and the main grid 26 means that the dielectric layer 24 located on both sides of the main grid 26 and the corresponding side edges of the main grid 26 have the first spacing L1 respectively; the second spacing L2 between the metal layer 25 and the main grid 26 means that the metal layer 25 located on both sides of the main grid 26 and the corresponding side edges of the main grid 26 have the second spacing L2 respectively.

[0083] Exemplarily, the second spacing L2 may be consistent with the first spacing L1. Optionally, the second spacing L2 may also be greater than the first spacing L1, so that when the metal layer 25 is stacked on the dielectric layer 24, the dielectric layer 24 can fully play an electrical isolation role to isolate the metal layer 25 from the fine grid.

[0084] Exemplarily, the value range of the first spacing L1 is 0.3 mm to 0.5 mm, for example, L1 can be 0.33 mm, 0.35 mm, 0.39 mm, 0.41 mm, 0.44 mm, 0.47 mm, etc.; the value range of the second spacing L2 is 0.5 mm to 1 mm, for example, L2 can be 0.55 mm, 0.59 mm, 0.65 mm, 0.7 mm, 0.77 mm, 0.85 mm, 0.87 mm, 0.93 mm, etc. Exemplarily, the value range of the width w of the main grid 26 is 30 μm to 80 μm, for example, the width w of the main grid 26 can be 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, etc.

[0085] In some embodiments, the refractive index of the dielectric layer 24 is less than the refractive index of the first passivation layer 23. For example, the refractive index n0 of the dielectric layer 24, the refractive index n1 of the first passivation layer 23, and the refractive index n2 of the substrate 10 satisfy the following relationship: At the same time, the absorption coefficient k of the dielectric layer 24 is 0 in the 900nm-1200nm band where the TOPCon photovoltaic cell has a spectral response.

[0086] Exemplarily, the material of the dielectric layer 24 includes at least one of silicon oxide, silicon nitride, titanium oxide, aluminum oxide, or magnesium fluoride. The material of the metal layer 25 includes at least one of gold, silver, aluminum, or copper.

[0087] For example, the metal layer 25 is formed on the dielectric layer 24 by depositing metal nanoparticles. Driven by a light field of a specific frequency, the free electrons on the surface of the metal nanoparticles interact with photons to form a localized surface plasmon resonance. The resonance can significantly enhance the local field on the surface of the metal nanoparticles, thereby generating multi-angle scattering of the incident light, effectively extending the optical path of the light in the absorbing medium. Based on this, the infrared spectral response of the TOPCon photovoltaic cell can be improved by depositing metal nanoparticles on the dielectric layer 24 to form a back-reflecting structure.

[0088] For example, the metal layer 25 is a layer formed by the deposition of silver nanoparticles, and the main grid 26 and the fine grid are formed by printing silver paste on the photovoltaic cell. The test results show that the conductivity of the main grid 26 and the fine grid is 1.80E5 (1 / Ω·cm); while the conductivity of the metal layer 25 is 1.747E5 (1 / Ω·cm). It can be seen that the conductivity of the metal layer 25 is less than that of the main grid 26 and the fine grid. When the two are in direct contact, the loss of carrier collection will be caused. However, the electrical isolation between the metal layer 25 and the fine grid through the dielectric layer 24 can avoid the above-mentioned loss of carrier collection.

[0089] In some embodiments, Figure 1 As shown, the thickness of the dielectric layer 24 ranges from 1 nm to 300 nm. The dielectric layer 24 is used to block direct contact between the metal layer 25 and the fine grid. When the thickness of the dielectric layer 24 is 1 nm, the barrier effect between the metal layer 25 and the fine grid can be ensured.

[0090] In some embodiments, Figure 1As shown, the thickness of the metal layer 25 ranges from 200nm to 1000nm. The back-reflective structure formed by stacking the metal layer 25 on the dielectric layer 24 needs to take into account excellent reflection characteristics. When the thickness of the metal layer 25 is greater than 200nm, the metal layer 25 can reach a reflectivity of more than 95% in the 900nm to 1200nm band, and as the thickness increases, the reflectivity will gradually approach 100%. For example, a 200nm thick metal layer 25 formed of silver has an average reflectivity of 97% in the 900nm to 1200nm band. Considering the high cost of silver, the thickness of the metal layer 25 is set to a maximum of 1000nm, i.e., 1μm. Exemplarily, the thickness of the metal layer 25 can be 230nm, 270nm, 300nm, 370nm, 400nm, 500nm, 630nm, 700nm, 800nm, 900nm, 950nm, etc. It can be understood that the thickness of the above-mentioned metal layer 25 can also be greater than 1μm.

[0091] Exemplarily, the substrate 10 of the photovoltaic cell of the exemplary embodiment of the present invention includes a silicon-based material, such as single crystal silicon, polycrystalline silicon, amorphous silicon, etc. The substrate 10 can be N-type crystalline silicon or P-type crystalline silicon; the substrate 10 can also be copper indium gallium selenide, perovskite or germanium, etc.

[0092] Figure 5 Schematic diagram of a method for preparing a photovoltaic cell according to an embodiment of the present invention. Figure 5 As shown, the exemplary embodiment of the present invention also provides a method for preparing a photovoltaic cell, which may include the following steps:

[0093] Step 501: Provide a substrate 10 stacked with a first passivation layer 23 .

[0094] A first passivation layer 23 is stacked in the back field of the substrate 10 , which is an N-type crystalline silicon substrate and serves as an absorption layer of the photovoltaic cell.

[0095] Specifically, Figure 1 As shown, a tunneling oxide layer 21, a doped polysilicon layer 22 and the above-mentioned first passivation layer 23 are stacked in sequence on the back side of the substrate 10; a diffusion layer 31, a second passivation layer 32 and a passivation anti-reflection layer 33 are formed in sequence on the front side of the substrate 10 to form a TOPCon photovoltaic cell; and a gate 34 (front main grid) and a corresponding front fine grid are printed on the front side of the photovoltaic cell, and a main grid 26 and a corresponding fine grid are printed on the back side of the photovoltaic cell.

[0096] Step 502 : stacking a dielectric layer 24 on a side of the first passivation layer 23 facing away from the substrate 10 , and the dielectric layer 24 is located on other regions of the first passivation layer 23 except the main gate 26 .

[0097] The dielectric layer 24 and the metal layer 25 can be formed on the first passivation layer 23 by plasma enhanced chemical vapor deposition, magnetron sputtering, vacuum evaporation coating, electron beam evaporation, atomic layer deposition, etc. The exemplary embodiment of the present invention is described by taking the preparation method of vacuum evaporation coating as an example.

[0098] Figure 2 is a schematic diagram of a top view of the structure of a first mask according to an embodiment of the present invention. Figure 2 As shown, the first mask plate 40 is formed by a peripheral frame structure and a plurality of first shielding strips 41 on the inner side, wherein the position of each first shielding strip 41 corresponds to the main grid 26 in the back field of the TOPCon photovoltaic cell. When the first mask plate 40 is covered with the first passivation layer 23, the plurality of first shielding strips 41 shield the surface of each main grid 26 in the back field, exposing the surface of other regions of the first passivation layer 23 except the main grid 26, so as to form a dielectric layer 24 on the other regions.

[0099] After the surface of each main grid 26 is shielded by the first mask plate 40 , the TOPCon photovoltaic cell is placed in the evaporation machine for vacuuming.

[0100] In the process of forming the dielectric layer 24, the evaporation rate ranges from For example, it can be wait.

[0101] In practical applications, when the vacuum degree reaches 5×10 -4 Pa, the evaporation rate is Under the condition of , MgF2 with a thickness of 120 nm is deposited on the exposed surface of the first passivation layer 23 away from the substrate 10 to form a dielectric layer 24.

[0102] In an optional embodiment, the width W1 of the first shielding strip 41 of the first mask plate 40 is the same as the width w of the main gate 26. In this embodiment, although the deposited dielectric layer 24 does not directly contact the top of the main gate 26, it will contact the side of the main gate 26.

[0103] In some embodiments, the width W1 of the first shielding strip 41 of the first mask plate 40 is greater than the width w of the main grid 26, for example, the first spacing L1 between the two side edges of the first shielding strip 41 and the two side edges of the shielded main grid 26 is 0.3 mm to 0.5 mm. The value range of W1 is 0.63 mm to 1.08 mm. The first shielding strip 41 in this width range can avoid wrap-around plating during the deposition of the dielectric layer 24, thereby making the dielectric layer 24 directly contact the two sides of the main grid 26, that is, the dielectric layer 24 can be spaced apart from the main grid 26, avoiding the possibility of reducing the conductivity of the main grid 26 and resulting in a reduced fill factor.

[0104] Step 503 : stacking a metal layer 25 on a side of the dielectric layer 24 away from the first passivation layer 23 , and separating the metal layer 25 from the main gate 26 ; wherein the metal layer 25 and the first passivation layer 23 are electrically isolated by the dielectric layer 24 .

[0105] In order to prevent the metal layer 25 from directly contacting the main grid 26 during the process of stacking the metal layer 25 on the dielectric layer 24, a second mask plate is used to shield the main grid 26. The second mask plate has the same structure as the first mask plate 40, that is, the outer periphery is a frame structure, and a plurality of second shielding strips corresponding to the main grid 26 are arranged inside. The difference is that the width of the second shielding strip of the second mask plate is greater than the width of the first mask plate 40.

[0106] For example, when the first shielding strips 41 of the first mask plate 40 are larger than the width of the main grid 26 , the structure and size of the second mask plate may be the same as those of the first mask plate 40 .

[0107] After the surface of each main grid 26 is shielded by the second mask plate, the TOPCon photovoltaic cell is placed in the evaporation machine for vacuuming.

[0108] In the process of forming the metal layer 25, the deposition rate of the metal layer to the first preset thickness is Optionally etc.; the deposition rate of the deposited metal layer from the first preset thickness to the second preset thickness is Optionally etc.; the deposition rate of the metal layer from the second preset thickness to the third preset thickness is Optionally etc.; the deposition rate of the deposited metal layer from the third preset thickness to the fourth preset thickness is Optionally etc., wherein the first preset thickness, the second preset thickness, the third preset thickness and the fourth preset thickness increase in sequence. Thus, the slow deposition rate at first is conducive to increasing the adhesion, and the fast deposition rate at last is conducive to shortening the preparation time.

[0109] Exemplarily, the first preset thickness can be 5nm to 15nm, optionally 7nm, 9nm, 11nm, 13nm, etc.; the second preset thickness can be 10nm to 30nm, optionally 11nm, 13nm, 17nm, 23nm, 25nm, 27nm, etc.; the third preset thickness can be 20nm to 70nm, optionally 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 65nm, etc.; the fourth preset thickness can be 100nm to 1000nm, optionally 110nm, 150nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, etc.

[0110] In practical applications, when the vacuum degree reaches 5×10 -4 Pa, at an evaporation rate of 0~10nm is deposited under the conditions of evaporation rate 10nm~20nm is deposited under the conditions of evaporation rate 20nm~50nm is deposited under the conditions of evaporation rate 50nm~200nm is deposited under the conditions of, and a total deposition thickness of 200nm of Ag metal layer 25 is formed.

[0111] A metal layer 25 with a total deposition thickness of 200 nm is formed under a variety of conditions with increasing evaporation rates, which is beneficial for the initially formed metal layer 25 to be stably attached to the dielectric layer 24 and increase the mechanical strength of the metal layer 25. Evaporation at an increasing evaporation rate can ensure the uniformity of the metal layer 25 and control the thickness, thereby obtaining the desired electrical and physical properties, thereby enhancing the long-wave spectral response of the TOPCon photovoltaic cell.

[0112] When the width of the second shielding strip of the second mask plate used is greater than the width of the first mask plate 40, the formed metal layer 25 can be deposited only on the dielectric layer 24 to prevent the second shielding strip from being circumvented when the metal layer 25 is deposited, that is, a portion of the metal particles bypass the second shielding strip and directly contact the main grid 26 and / or the fine grid, causing carrier recombination and reducing the fill factor of the TOPCon photovoltaic cell. Exemplarily, the second spacing L2 between the two sides of the second shielding strip and the two sides of the main grid 26 is in the range of 0.5mm to 1mm, for example, the width of the second shielding strip is in the range of 1.09mm to 2.08mm.

[0113] As can be seen from the above, by using the first mask plate 40 and the second mask plate, the surface of the main grid 26 in the back field is shielded when depositing the dielectric layer 24 and the metal layer 25, respectively, to avoid direct contact between the metal layer 25 and the main grid 26, without reducing the filling factor of the TOPCon photovoltaic cell. The back reflection structure formed by the dielectric layer 24 and the metal layer 25 can reflect light back to the n-type crystalline silicon substrate 10 as the absorption layer, effectively improving the long-wave spectral response of the TOPCon photovoltaic cell.

[0114] The exemplary embodiment of the present invention further provides a photovoltaic cell assembly, comprising a plurality of electrically connected photovoltaic cells, at least one of which is a photovoltaic cell of the above embodiment, or,

[0115] At least one photovoltaic cell is a photovoltaic cell prepared by the photovoltaic cell preparation method of the above embodiment.

[0116] The technical advantages of the above photovoltaic cell assembly over the prior art are the same as the advantages of the above photovoltaic cell or photovoltaic cell preparation method, which will not be described in detail here.

[0117] Technical Solution 1. A photovoltaic cell, comprising a substrate, a main grid, a dielectric layer, a metal layer, and a first passivation layer stacked on the substrate,

[0118] The dielectric layer is stacked on a side of the first passivation layer facing away from the substrate, and is located on other regions of the first passivation layer except the main gate;

[0119] The metal layer is stacked on a side of the dielectric layer away from the first passivation layer and is spaced apart from the main gate.

[0120] The metal layer and the first passivation layer are electrically isolated from each other by the dielectric layer.

[0121] Technical Solution 2. According to the photovoltaic cell described in Technical Solution 1, the dielectric layer is separated from the main grid.

[0122] Technical Solution 3. According to the photovoltaic cell described in Technical Solution 2, there is a first distance between the dielectric layer and the main grid, and there is a second distance between the metal layer and the main grid, and the second distance is equal to or greater than the first distance.

[0123] Technical Solution 4. According to the photovoltaic cell of Technical Solution 1, the material of the dielectric layer includes at least one of silicon oxide, silicon nitride, titanium oxide, aluminum oxide or magnesium fluoride; and / or,

[0124] The material of the metal layer includes at least one of gold, silver, aluminum or copper.

[0125] Technical Solution 5. According to the photovoltaic cell described in Technical Solution 1, the thickness of the dielectric layer ranges from 1 nm to 300 nm; and / or,

[0126] The thickness of the metal layer ranges from 200 nm to 1000 nm.

[0127] Technical Solution 6. According to the photovoltaic cell described in Technical Solution 1, the substrate includes a silicon substrate or a germanium substrate.

[0128] Technical Solution 7. According to the photovoltaic cell described in Technical Solution 1, the photovoltaic cell includes one of a tunneling oxidation passivation contact photovoltaic cell and an interdigitated back contact photovoltaic cell.

[0129] Technical Solution 8. According to the photovoltaic cell described in Technical Solution 1, the photovoltaic cell also includes a tunneling oxide layer and a doped polysilicon layer, the tunneling oxide layer and the doped polysilicon layer are stacked between the substrate and the first passivation layer, and the tunneling oxide layer and the doped polysilicon layer are arranged in a direction away from the substrate.

[0130] Technical Solution 9. The photovoltaic cell according to Technical Solution 8 further comprises a diffusion layer, a second passivation layer and a passivation anti-reflection layer, wherein the diffusion layer, the second passivation layer and the passivation anti-reflection layer are sequentially formed on the side of the substrate away from the first passivation layer, and the diffusion layer, the second passivation layer and the passivation anti-reflection layer are arranged in a direction away from the substrate.

[0131] Technical Solution 10. According to the photovoltaic cell described in Technical Solution 9, the doped polysilicon layer is a phosphorus-doped polysilicon layer, and the diffusion layer is a boron-doped diffusion layer.

[0132] Technical Solution 11. A method for preparing a photovoltaic cell, comprising:

[0133] providing a substrate stacked with a first passivation layer;

[0134] A dielectric layer is stacked on a side of the first passivation layer facing away from the substrate, and the dielectric layer is located on other regions of the first passivation layer except the main gate;

[0135] stacking a metal layer on a side of the dielectric layer away from the first passivation layer, and spacing the metal layer from the main gate;

[0136] The metal layer and the first passivation layer are electrically isolated by the dielectric layer.

[0137] Technical Solution 12. According to the preparation method of Technical Solution 11, the step of stacking a dielectric layer on a side of the first passivation layer away from the substrate, and the dielectric layer is located on other regions of the first passivation layer except the main gate, comprises:

[0138] Covering the first mask plate on the side of the first passivation layer away from the substrate and shielding the main grid, wherein the width of the first shielding strip of the first mask plate shielding the main grid is greater than or equal to the width of the corresponding main grid;

[0139] The dielectric material is evaporated to form the dielectric layer on the first passivation layer.

[0140] Technical Solution 13. According to the preparation method described in Technical Solution 12, when the width of the first shielding strip is greater than the width of the corresponding main grid, the dielectric material is evaporated on the first passivation layer to form the dielectric layer, wherein the dielectric layer is separated from the main grid.

[0141] Technical solution 14. According to the preparation method of technical solution 13, in the step of stacking a metal layer on a side of the dielectric layer away from the first passivation layer and separating the metal layer from the main gate, the step comprises:

[0142] Covering the second mask plate on the side of the dielectric layer away from the first passivation layer and shielding the main grid, wherein the width of the second shielding strip of the second mask plate shielding the main grid is greater than or equal to the width of the first shielding strip of the first mask plate;

[0143] The metal layer is formed by evaporating a metal material on the dielectric layer.

[0144] Technical Solution 15. According to the preparation method of Technical Solution 11, a dielectric layer is stacked on a side of the first passivation layer away from the substrate, and the dielectric layer is located on other regions of the first passivation layer except the main gate, comprising:

[0145] In a vacuum environment, the deposition rate of the dielectric layer is and / or,

[0146] The material of the dielectric layer includes at least one of silicon oxide, silicon nitride, titanium oxide, aluminum oxide or magnesium fluoride.

[0147] Technical Solution 16. According to the preparation method of Technical Solution 11, in the step of stacking a metal layer on a side of the dielectric layer away from the first passivation layer and separating the metal layer from the main gate, the step comprises:

[0148] In a vacuum environment, the deposition rate of the metal layer to a first preset thickness is The deposition rate of the metal layer from the first preset thickness to the second preset thickness is The deposition rate of the metal layer from the second preset thickness to the third preset thickness is The deposition rate of the metal layer from the third preset thickness to the fourth preset thickness is Wherein, the first preset thickness, the second preset thickness, the third preset thickness and the fourth preset thickness increase in sequence; and / or,

[0149] The material of the metal layer includes at least one of gold, silver, aluminum, or copper.

[0150] Technical solution 17. A photovoltaic cell assembly, comprising a plurality of electrically connected photovoltaic cells, at least one of the photovoltaic cells being a photovoltaic cell according to any one of technical solutions 1 to 10, or,

[0151] At least one of the photovoltaic cells is a photovoltaic cell produced by the preparation method described in any one of technical solutions 11-16.

[0152] It should be understood by those skilled in the art that the above embodiments are only for the purpose of clearly illustrating the present invention, and are not intended to limit the scope of the present invention. For those skilled in the art, other changes or modifications may be made based on the above disclosure, and these changes or modifications are still within the scope of the present invention.

Claims

1. A photovoltaic cell, It is characterized in that It includes a substrate, a main gate, a dielectric layer, a metal layer and a first passivation layer stacked on the substrate. The dielectric layer is stacked on a side of the first passivation layer facing away from the substrate, and is located on other regions of the first passivation layer except the main gate; The metal layer is stacked on a side of the dielectric layer away from the first passivation layer and is spaced apart from the main gate. The metal layer and the first passivation layer are electrically isolated from each other by the dielectric layer.

2. The photovoltaic cell according to claim 1, It is characterized in that The dielectric layer is spaced apart from the main gate.

3. The photovoltaic cell according to claim 2, It is characterized in that There is a first distance between the dielectric layer and the main grid, and there is a second distance between the metal layer and the main grid, and the second distance is equal to or greater than the first distance.

4. The photovoltaic cell according to claim 1, It is characterized in that The material of the dielectric layer includes at least one of silicon oxide, silicon nitride, titanium oxide, aluminum oxide, or magnesium fluoride; and / or, The material of the metal layer includes at least one of gold, silver, aluminum or copper; Preferably, the thickness of the dielectric layer ranges from 1 nm to 300 nm; and / or, The thickness of the metal layer ranges from 200nm to 1000nm; Preferably, the substrate comprises a silicon substrate or a germanium substrate; Preferably, the photovoltaic cell comprises one of a tunneling oxide passivation contact photovoltaic cell and an interdigitated back contact photovoltaic cell.

5. The photovoltaic cell according to claim 1, It is characterized in that The photovoltaic cell further includes a tunneling oxide layer and a doped polysilicon layer, wherein the tunneling oxide layer and the doped polysilicon layer are stacked between the substrate and the first passivation layer, and the tunneling oxide layer and the doped polysilicon layer are arranged in a direction away from the substrate; Preferably, the photovoltaic cell further comprises a diffusion layer, a second passivation layer and a passivation anti-reflection layer, wherein the diffusion layer, the second passivation layer and the passivation anti-reflection layer are sequentially formed on a side of the substrate away from the first passivation layer, and the diffusion layer, the second passivation layer and the passivation anti-reflection layer are arranged in a direction away from the substrate; Preferably, the doped polysilicon layer is a phosphorus-doped polysilicon layer, and the diffusion layer is a boron-doped diffusion layer.

6. A method for preparing a photovoltaic cell, It is characterized in that include: providing a substrate stacked with a first passivation layer; A dielectric layer is stacked on a side of the first passivation layer facing away from the substrate, and the dielectric layer is located on other regions of the first passivation layer except the main gate; stacking a metal layer on a side of the dielectric layer away from the first passivation layer, and spacing the metal layer from the main gate; The metal layer and the first passivation layer are electrically isolated by the dielectric layer.

7. The preparation method according to claim 6, It is characterized in that The step of stacking a dielectric layer on a side of the first passivation layer facing away from the substrate, wherein the dielectric layer is located on other regions of the first passivation layer except the main gate, comprises: Covering the first mask plate on the side of the first passivation layer away from the substrate and shielding the main grid, wherein the width of the first shielding strip of the first mask plate shielding the main grid is greater than or equal to the width of the corresponding main grid; Vapor depositing dielectric material to form the dielectric layer on the first passivation layer; Preferably, when the width of the first shielding strip is greater than the width of the corresponding main grid, a dielectric material is evaporated to form the dielectric layer on the first passivation layer, wherein the dielectric layer is spaced apart from the main grid; Preferably, the step of stacking a metal layer on a side of the dielectric layer away from the first passivation layer and spacing the metal layer apart from the main gate includes: Covering the second mask plate on the side of the dielectric layer away from the first passivation layer and shielding the main grid, wherein the width of the second shielding strip of the second mask plate shielding the main grid is greater than or equal to the width of the first shielding strip of the first mask plate; The metal layer is formed by evaporating a metal material on the dielectric layer.

8. The preparation method according to claim 6, It is characterized in that The step of stacking a dielectric layer on a side of the first passivation layer facing away from the substrate, wherein the dielectric layer is located on other regions of the first passivation layer except the main gate, comprises: In a vacuum environment, the deposition rate of the dielectric layer is and / or, The material of the dielectric layer includes at least one of silicon oxide, silicon nitride, titanium oxide, aluminum oxide or magnesium fluoride.

9. The preparation method according to claim 6, It is characterized in that The step of stacking a metal layer on a side of the dielectric layer away from the first passivation layer and spacing the metal layer apart from the main gate includes: In a vacuum environment, the deposition rate of the metal layer to a first preset thickness is The deposition rate of the metal layer from the first preset thickness to the second preset thickness is The deposition rate of the metal layer from the second preset thickness to the third preset thickness is The deposition rate of the metal layer from the third preset thickness to the fourth preset thickness is Wherein, the first preset thickness, the second preset thickness, the third preset thickness and the fourth preset thickness increase in sequence; and / or, The material of the metal layer includes at least one of gold, silver, aluminum, or copper.

10. A photovoltaic cell assembly, It is characterized in that comprising a plurality of electrically connected photovoltaic cells, at least one of the photovoltaic cells being the photovoltaic cell according to any one of claims 1 to 5, or, At least one of the photovoltaic cells is a photovoltaic cell prepared by the preparation method according to any one of claims 6 to 9.