Chromium-activated calcium tin garnet-based near-infrared fluorescent powder and preparation method thereof
Through the chemical structure of Ca3Sn2.935Si0.05Ga2O12:0.02Cr3+, a chromium-activated calcium-tin garnet-based near-infrared phosphor was prepared, which solved the problems of the emission wavelength of existing materials and the narrow width of the half-maximum, and achieved a range of 700-1200nm Broadband near-infrared transmission has enhanced its application potential in the fields of food quality testing and medical diagnosis.
Patent Information
- Application Number
- CN202411040012.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The emission wavelength of existing garnet-based near-infrared fluorescent materials is short and have a narrow half-maximum width, which cannot effectively cover the range of 700 to 1200 nm, limiting its application in food quality testing, night vision and medical diagnosis.
Using the chemical structure of Ca3Sn2.935Si0.05Ga2O12:0.02Cr3+, chromium-activated calcium-tin garnet-based near-infrared phosphor is prepared by high-temperature sintering method, providing absorption in the blue-green and red light regions, achieving a broadband near-band of 700-1200nm Infrared emission.
A longer emission wavelength and wider coverage are achieved, which improves the application potential of materials, and is simple in preparation and easy to mass production.
Smart Images

Figure CN118954580A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of inorganic luminescent materials, and in particular to a chromium-activated calcium tin garnet-based near-infrared phosphor and a preparation method thereof. Background technology:
[0002] At present, broadband near-infrared luminescent materials emitting in the range of 700 to 1200 nm have attracted people's attention due to their wide demand in food quality detection and analysis, night vision and medical diagnosis. 3 Electronic configuration, trivalent chromium ions in a suitable crystal field environment can obtain 4 T 2 → 4 A 2 The broadband near-infrared emission dominated by transitions has become the first choice for near-infrared activators. 3+ Doped near-infrared phosphors have been developed, among which garnet-type materials with the formula A3B2C3O12 stand out due to their high luminous efficiency and good thermal stability. However, due to the high structural symmetry, most existing garnet-based near-infrared fluorescent materials have relatively short emission wavelengths and narrow half-peak widths, and the coverage range of 700-1200nm is insufficient. These characteristics seriously hinder the actual application needs. Therefore, it is necessary to find Cr with a wide emission range and excellent performance. 3+ Activating garnet-based near-infrared phosphors has become a problem that needs to be solved by those skilled in the art. Summary of the invention:
[0003] The invention aims to provide a chromium-activated calcium tin garnet-based near-infrared phosphor and a preparation method thereof, which solves the problem that the garnet-based near-infrared fluorescent material has a short main peak wavelength and a narrow half-peak width.
[0004] The present invention is achieved through the following technical solutions:
[0005] A chromium-activated calcium tin garnet-based near-infrared phosphor, whose chemical structure is Ca 3 Sn 2.935 Si 0.05 Ga 2 O 12 :0.02Cr 3+ .
[0006] Through research, it was found that the phosphor with this specific chemical structure has absorption in the blue-green light region, red light and deep red light region, and can emit broadband near-infrared light of 700 to 1200nm with a half-width of 154nm.
[0007] Therefore, the present invention also protects the application of the calcium tin garnet-based near-infrared phosphor in the fields of eye-feeding light instruments and plant growth lighting.
[0008] The calcium tin garnet-based near-infrared phosphor is used as a near-infrared light conversion material excited by a blue light LED chip.
[0009] The present invention also provides a method for preparing the near-infrared phosphor, comprising the following steps:
[0010] S1: According to the chemical formula Ca 3 Sn 2.935 Si 0.05 Ga 2 O 12 :0.02Cr 3+ Weigh the raw materials containing calcium, tin, silicon, gallium and chromium elements respectively according to the molar ratio of each element, and weigh the flux, and fully grind and mix the raw materials and the flux to obtain a mixture;
[0011] S2: placing the mixture obtained in S1 into an alumina crucible and sintering at 1200-1400° C. for 3-7 hours, cooling to room temperature after sintering, and grinding into powder to obtain the phosphor.
[0012] Preferably, the raw material containing calcium, tin, silicon, gallium and chromium elements is selected from one of oxides, carbonates and oxalates containing calcium, tin, silicon, gallium and chromium elements, preferably oxides.
[0013] The flux is one or more of boric acid, ammonium fluoride and calcium fluoride.
[0014] Preferably, in step S2, the high temperature sintering temperature is 1300° C. and the high temperature roasting time is 6 hours.
[0015] The present invention has the following beneficial effects: the near-infrared phosphor of the present invention is the first to be 3 Sn 2.95 Si 0.05 Ga 2 O 12 Cr doped into garnet matrix 3+ ions, the matrix is the activator Cr 3+ It provides a twisted octahedral coordination environment, so that it can absorb in the blue-green light region, red light and deep red light region under the excitation of blue light 467nm, and can emit 700-1200nm broadband near-infrared light with a half-width of 154nm. Compared with other garnet-based near-infrared phosphors, it has a longer emission wavelength and a wider emission coverage, which is conducive to practical applications. In addition, the preparation method adopted is a high-temperature solid-phase method, the preparation conditions are mild, the method is simple and feasible, and it is easy to mass produce. Description of the drawings:
[0016] Figure 1 This is the XRD spectrum of the phosphor obtained in Example 1 of the present invention.
[0017] Figure 2 This is the excitation spectrum of the sample in Example 1 of the present invention.
[0018] Figure 3 This is the emission spectrum of the sample of Example 1 of the present invention. Specific implementation method:
[0019] The following is a further description of the present invention, rather than a limitation of the present invention.
[0020] Embodiment 1:
[0021] Calcium oxide, tin oxide, silicon dioxide, gallium oxide and chromium oxide were selected as starting materials. The molar ratio of each element was Ca: Sn: Si: Ga: Cr: O = 3: 2.935: 0.05: 2: 0.02: 12. Five raw materials were weighed respectively to control the total weight of the raw material mixture to be 1 gram. Boric acid flux with a mass fraction of 3% of the total weight of the raw material mixture was weighed. The mixture was fully ground and mixed, put into an alumina crucible, put into a high-temperature furnace, and calcined at 1300 ° C for 6 hours. When cooled to room temperature, it was taken out and ground and dispersed to obtain Ca 3 Sn 2.935 Si 0.05 Ga 2 O 12 :0.02Cr 3+ Phosphor.
[0022] Figure 1 The XRD pattern of Example 1 of the present invention is measured by using a German Bruker D8 Advance X-ray diffractometer, with a test voltage of 40 kV, a test current of 40 mA, a scanning speed of 1 ° / min, and a Cu / Kα X-ray with a wavelength of
[0023] Figure 2 This is the excitation spectrum diagram of the sample of Example 1 of the present invention. When the sample is monitored at 843nm, the excitation wavelength range covers the blue-green light region, red light and deep red light region, and the maximum excitation peak is located at 465nm, which is a good match with the commercial blue light LED chip.
[0024] Figure 3 This is the emission spectrum of the sample of Example 1 of the present invention. Under 465nm blue light excitation, the emission band of the sample is in the range of 700-1200nm, the peak is at 843nm, and the half-peak width is 154nm.
[0025] Example 2
[0026] Calcium carbonate, tin oxide, silicon dioxide, gallium oxide and chromium oxide were selected as starting materials. The molar ratio of each element was Ca: Sn: Si: Ga: Cr: O = 3: 2.935: 0.05: 2: 0.02: 12. Five raw materials were weighed respectively to control the total weight of the raw material mixture to be 1 gram. Boric acid flux with a mass fraction of 3% of the total weight of the raw material mixture was weighed. The mixture was fully ground and mixed, put into an alumina crucible, put into a high-temperature furnace, and calcined at 1200 ° C for 5 hours. When cooled to room temperature, it was taken out and ground and dispersed to obtain Ca 3 Sn 2.935 Si 0.05 Ga 2 O 12 :0.02Cr 3+ Phosphor.
[0027] Example 3
[0028] Calcium oxalate, tin oxide, silicon dioxide, gallium oxide and chromium oxide were selected as starting materials. According to the molar ratio of each element, Ca: Sn: Si: Ga: Cr: O = 3: 2.935: 0.05: 2: 0.02: 12, five kinds of raw materials were weighed respectively, and the total weight of the raw material mixture was controlled to be 1 gram. Ammonium fluoride flux with a mass fraction of 3% of the total weight of the raw material mixture was weighed. The mixture was fully ground and mixed, put into an alumina crucible, put into a high-temperature furnace, and calcined at 1400 ° C for 6 hours. When cooled to room temperature, it was taken out and ground and dispersed to obtain Ca 3 Sn 2.935 Si 0.05 Ga 2 O 12 :0.02Cr 3+ Phosphor.
[0029] Example 4
[0030] Calcium carbonate, tin oxide, silicon dioxide, gallium oxide and chromium oxide were selected as starting materials. The molar ratio of each element was Ca: Sn: Si: Ga: Cr: O = 3: 2.935: 0.05: 2: 0.02: 12. Five raw materials were weighed respectively to control the total weight of the raw material mixture to be 1 gram. Calcium fluoride flux with a mass fraction of 3% of the total weight of the raw material mixture was weighed. The mixture was fully ground and mixed, put into an alumina crucible, put into a high-temperature furnace, and calcined at 1400 ° C for 3 hours. When cooled to room temperature, it was taken out and ground and dispersed to obtain Ca 3 Sn 2.935 Si 0.05 Ga 2 O 12 :0.02Cr 3+ Phosphor.
[0031] Example 5
[0032] Calcium oxide, tin oxide, silicon dioxide, gallium oxide and chromium oxide were selected as starting materials. The molar ratio of each element was Ca: Sn: Si: Ga: Cr: O = 3: 2.935: 0.05: 2: 0.02: 12. Five raw materials were weighed respectively to control the total weight of the raw material mixture to be 1 gram. Ammonium fluoride flux was weighed to be 3% of the total weight of the raw material mixture. The mixture was fully ground and mixed, put into an alumina crucible, put into a high-temperature furnace, and calcined at 1200 ° C for 7 hours. When cooled to room temperature, it was taken out and ground and dispersed to obtain Ca 3 Sn 2.935 Si 0.05 Ga 2 O 12 :0.02Cr 3+ Phosphor.
[0033] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0034] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A chromium-activated calcium tin garnet-based near-infrared phosphor, characterized in that: Its chemical formula is Ca3Sn 2.935 Si 0.05 Ga2O 12 :0.02Cr 3+ .
2. The method for preparing the chromium-activated calcium tin garnet-based near-infrared phosphor according to claim 1, characterized in that: The following steps are involved: S1: According to the chemical formula Ca3Sn 2.935 Si 0.05 Ga2O 12 :0.02Cr 3+ Weigh the raw materials containing calcium, tin, silicon, gallium and chromium elements respectively according to the molar ratio of each element, and weigh the flux, and fully grind and mix the raw materials and the flux to obtain a mixture; S2: placing the mixture obtained in S1 into an alumina crucible and sintering at 1200-1400° C. for 3-7 hours, cooling to room temperature after sintering, and grinding into powder to obtain the phosphor.
3. The preparation method according to claim 2, characterized in that: The raw material containing calcium, tin, silicon, gallium and chromium elements is selected from one of oxides, carbonates and oxalates containing calcium, tin, silicon, gallium and chromium elements.
4. The preparation method according to claim 2, characterized in that: The flux is one or more of boric acid, ammonium fluoride and calcium fluoride.
5. The preparation method according to claim 2, characterized in that: In step S2, the high temperature sintering temperature is 1300° C. and the high temperature roasting time is 6 hours.
6. Application of the calcium tin garnet-based near-infrared phosphor according to claim 1 in the fields of eye-feeding light instruments and plant growth lighting.
7. Use of the calcium tin garnet-based near-infrared phosphor according to claim 1 as a near-infrared light conversion material excited by a blue light LED chip.
Citation Information
Cited By
Chromium ion single-doped ultra-wideband near-infrared fluorescent material, preparation method thereof and LED device
CN122060495A