N2O decomposition catalyst
By supporting iron elements on SiO2 and Al2O3 carriers and optimizing the TPD spectrum characteristics, a catalyst with excellent water resistance and sulfur oxide resistance was developed, and the decomposition of nitrous oxide and nitric oxide in the prior art was solved in the high humidity environment. The problem of low efficiency has achieved efficient exhaust gas purification.
Patent Information
- Application Number
- CN202380029521.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to effectively decompose nitrous oxide (N2O) and nitric oxide (NO) especially in exhaust gases containing water and sulfur oxides, and their water resistance and sulfur oxide resistance are insufficient, which affects the stability and efficiency of the catalyst. .
Using a catalyst containing SiO2 and Al2O3 supports, it supports iron and optimizes the specific TPD spectrum characteristics and pyridine adsorption characteristics to design a catalyst with excellent water resistance and sulfur oxide resistance, which can effectively decompose in high temperature and high humidity environments. N2O and NO.
Even under the conditions that contain a large amount of water and sulfur oxides, the catalyst can efficiently decompose nitrous oxide and nitric oxide, maintaining the NO2 decomposition rate of more than 60% and the NO decomposition rate of more than 90%, significantly improving the exhaust gas purification treatment. Effect.
Smart Images

Figure CN118973708A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst (hereinafter sometimes referred to as an N2O decomposition catalyst) which is configured to promote the decomposition reaction of dinitrogen monoxide or the decomposition reaction of dinitrogen monoxide and nitric oxide. More specifically, it relates to a catalyst which is configured to promote the decomposition reaction of dinitrogen monoxide or the decomposition reaction of dinitrogen monoxide and nitric oxide, and which can be appropriately used for the purification of exhaust gas containing a large amount of water and / or sulfur oxides, coal-fired fluidized bed boilers, exhaust gas from ammonia fuel ship engines, exhaust gas from ammonia fuel gas turbines, exhaust gas from nitrification processes or denitrification processes in water treatment, etc., preferably can be appropriately used for the purification of ammonia fuel combustion exhaust gas, and has excellent water resistance and / or sulfur oxide resistance; and a method for reducing dinitrogen monoxide or dinitrogen monoxide and nitric oxide from a gas containing water and / or sulfur oxides and dinitrogen monoxide, or from a gas containing water and / or sulfur oxides, dinitrogen monoxide and nitric oxide. Background Art
[0002] Nitrous oxide (N2O) is produced by the reaction of NO produced during combustion (3NO→NO2+N2O), the oxidation reaction of ammonia (2NH3+2O2→N2O+3H2O), etc. In general, N2O is easily produced if fossil fuels containing a large amount of nitrogen are used. The chemical reaction that produces N2O is temperature-dependent, and the lower the temperature, the easier it is to produce N2O. Therefore, in furnaces that burn at low temperatures of around 800 to 900°C, such as fluidized bed boilers, the emission of N2O will increase. In addition, N2O is sometimes produced by contact between a NOx removal catalyst and NOx (=NO, NO2). In addition to nitrogen oxides (NO, NO2) derived from nitrogen in the air, engines or gas turbines that use ammonia fuel sometimes emit nitrogen oxides (NO, NO2, N2O) derived from ammonia fuel. In general, nitrous oxide has a greenhouse effect that is about 300 times stronger than CO2. Generally speaking, nitrous oxide remaining in the atmosphere is decomposed by ultraviolet rays to generate nitric oxide, which has the effect of destroying the ozone layer. Therefore, various technologies for decomposing nitrous oxide in exhaust gas and rendering it harmless have been proposed.
[0003] For example, Patent Document 1 discloses a method for removing nitrous oxide from exhaust gas, characterized in that the nitrous oxide in the exhaust gas is reduced and removed by mixing ammonia with the exhaust gas containing nitrous oxide and bringing the mixture into contact with a catalyst loaded with iron on β-zeolite in a temperature range of 350 to 500°C.
[0004] Patent document 2 discloses a method for purifying exhaust gas using a nitrous oxide treatment catalyst, which is characterized in that a nitrous oxide treatment catalyst for decomposing nitrous oxide in exhaust gas with a high sulfur content is used and is contacted with the exhaust gas containing nitrous oxide, thereby decomposing and treating the nitrous oxide. In this exhaust gas purification method, the nitrous oxide treatment catalyst is characterized in that iron is supported on a silica and alumina carrier as an active metal, and the proportion of strong acid is higher relative to the total amount of strong acid and weak acid.
[0005] Patent document 3 discloses: a method for producing a zeolite catalyst loaded with iron ions for reducing nitrous oxide alone or simultaneously reducing nitrous oxide and nitric oxide by means of an ammonia reducing agent, characterized in that it includes the following stages (A) to (F): (A) a stage of pre-treating the zeolite with water at a high temperature; (B) a stage of loading the iron ions on the zeolite pre-treated in the aforementioned stage (A) or the zeolite not pre-treated in the aforementioned stage (A) by means of a solution of a precursor substance of the iron ions; (C) a stage of filtering and drying the zeolite particles loaded with iron ions in the aforementioned stage (B); (D) a stage of repeatedly performing the stage (B) in order to increase the iron content of the powder dried in the aforementioned stage (C) and (C) stage; (E) a stage of calcining the catalyst manufactured in the aforementioned (D) stage in air; (F) a stage of treating the catalyst obtained through the aforementioned (E) stage with water from a zeolite that has not been subjected to the aforementioned (A) stage at a high temperature; and a method for reducing nitrous oxide or nitrous oxide and nitric oxide by an ammonia reducing agent, characterized in that: nitrous oxide is supplied alone or nitrous oxide and nitric oxide are supplied simultaneously, and a contact reaction is carried out with a zeolite catalyst loaded with activated iron ions manufactured by the aforementioned manufacturing method, and nitrous oxide is reduced alone and reduced or nitrous oxide and nitric oxide are reduced and reduced simultaneously by an ammonia reducing agent at a low catalyst reaction temperature.
[0006] Patent document 4 discloses a catalyst composition suitable for use as a selective contact reduction catalyst, which comprises: small pore molecular sieve particles having a pore structure and a maximum ring size of 8 tetrahedral atoms and impregnated with a promoter metal; and metal oxide particles, which are within the small pore molecular sieve particles and dispersed outside the pore structure of the small pore molecular sieve particles, and comprise one or more oxides of transition metals or lanthanide elements of Group 3 or Group 4 of the periodic table.
[0007] Patent document 5 discloses a method for converting NO X and a catalyst for N2O, comprising iron chabazite and iron beta zeolite.
[0008] Patent document 6 discloses a denitrification catalyst for high-temperature exhaust gas, which is a catalyst that adds ammonia to exhaust gas containing nitrogen oxides and removes nitrogen oxides by contact reduction in a reaction temperature range of 500 to 700°C. The catalyst is characterized in that 0.5 to 5 wt% of iron, calculated as Fe2O3, is supported on a high-silica zeolite having a SiO2 / Al2O3 molar ratio of 20 or more.
[0009] In addition, as a technology for decomposing nitrogen oxides in exhaust gas and rendering them harmless, Patent Document 7 discloses a metal-containing zeolite beta, characterized in that: the metal-containing zeolite beta does not contain an organic component and has a silica / alumina molar ratio (SAR) in the range of 5 to 20, wherein the metal contains at least 1.0 wt% of iron and / or copper. In addition, Patent Document 7 discloses a method for decomposing nitrogen oxides (NO X ) is characterized in that it includes the step of causing the aforementioned exhaust gas to at least partially contact an article containing metal-containing zeolite β that does not contain organic components, and the aforementioned metal contains at least 0.5% by weight of iron and / or copper.
[0010] Patent document 8 discloses an organic template-free zeolite material having a BEA framework structure, comprising at least one alkali metal M, and at least a portion of the atoms of the alkali metal M is substituted by Fe and / or Cu. Patent document 8 also discloses the following: the organic template-free zeolite material is used as a catalyst for selectively reducing nitrogen oxides NO x Catalyst and / or catalyst support in the selective contact reduction (SCR) process; used for oxidizing NH3, especially for oxidizing NH3 leakage in diesel engine system; used for decomposing N2O.
[0011] Previous technical literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 8-57262
[0014] Patent Document 2: Japanese Patent Application Publication No. 2014-176808
[0015] Patent Document 3: Japanese Patent Application No. 2012-521288
[0016] Patent Document 4: Japanese Patent Application No. 2019-502550
[0017] Patent Document 5: Japanese Patent Application No. 2020-527453
[0018] Patent Document 6: Japanese Patent Application Laid-Open No. 3-296436
[0019] Patent Document 7: Japanese Patent Application Publication No. 2013-526406
[0020] Patent Document 8: Japanese Patent Application Publication No. 2013-49624 Summary of the invention
[0021] Technical issues to be solved by the invention
[0022] The object of the present invention is to provide: a catalyst which is configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, and which can be appropriately used for the purification of exhaust gas from catalyst-fired coal-fired fluidized bed boilers, exhaust gas from ammonia-fueled ship engines, exhaust gas from ammonia-fueled gas turbines, exhaust gas from nitrification processes or denitrification processes in water treatment, etc., which contains a large amount of water and / or sulfur oxides, and which can preferably be appropriately used for the purification of ammonia fuel combustion exhaust gas and has excellent water resistance and / or sulfur oxide resistance; and a method for reducing nitrous oxide or nitrous oxide and nitric oxide from a gas containing water and / or sulfur oxides and nitrous oxide, or from a gas containing water and / or sulfur oxides, nitrous oxide and nitric oxide.
[0023] Means for solving technical problems
[0024] As a result of conducting studies to achieve the above-mentioned object, the present invention including the following aspects has been completed.
[0025] [1] A catalyst configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein the catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and in a TPD spectrum, the total amount of pyridine released in the range of 150°C to less than 450°C is 100 μmol or more relative to 1 g of the catalyst.
[0026] [2] The catalyst according to [1], wherein in the TPD spectrum, the ratio of the pyridine desorption amount at the maximum peak top in the range of 150°C to less than 450°C to the pyridine desorption amount at the maximum peak top in the range of 450°C to 800°C is greater than 1.
[0027] [3] The catalyst according to [1] or [2], wherein in the TPD spectrum, the ratio of the total amount of pyridine released in the range of 150°C to less than 450°C to the total amount of pyridine released in the range of 450°C to 800°C is 0.9 or more.
[0028] [4] The catalyst according to [1], [2] or [3], wherein in the TPD spectrum, the temperature of the maximum peak top in the range of 450°C to 800°C is 490°C to 650°C.
[0029] [5] The catalyst according to [1], [2], [3] or [4], wherein the saturated adsorption amount of pyridine is 100 μmol or more per 1 g of the catalyst.
[0030] [6] The catalyst according to [1], [2], [3], [4] or [5], wherein the crystallite size is 20 nm or more.
[0031] [7] A catalyst configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein the catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and in a TPD spectrum, the ratio of the pyridine release amount at the maximum peak top in the range of greater than 150°C and less than 450°C to the pyridine release amount at the maximum peak top in the range of greater than 450°C and less than 800°C is greater than 1.
[0032] [8] The catalyst according to [7], wherein in the TPD spectrum, the ratio of the total amount of pyridine released in the range of 150°C to less than 450°C to the total amount of pyridine released in the range of 450°C to 800°C is 0.9 or more.
[0033] [9] The catalyst according to [7] or [8], wherein in the TPD spectrum, the temperature of the maximum peak top in the range of 450°C to 800°C is 490°C to 650°C.
[0034]
[10] The catalyst according to [7], [8] or [9], wherein the saturated adsorption amount of pyridine is 100 μmol or more per 1 g of the catalyst.
[0035]
[11] The catalyst according to [7], [8], [9] or
[10] , wherein the crystallite size is 20 nm or more.
[0036]
[12] A catalyst configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein the catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and in a TPD spectrum, the ratio of the total amount of pyridine released in the range of 150°C to less than 450°C to the total amount of pyridine released in the range of 450°C to 800°C is greater than 0.9.
[0037]
[13] The catalyst according to
[12] , wherein in the TPD spectrum, the temperature of the maximum peak top in the range of 450°C to 800°C is 490°C to 650°C.
[0038]
[14] The catalyst according to
[12] or
[13] , wherein the saturated adsorption amount of pyridine is 100 μmol or more per 1 g of the catalyst.
[0039]
[15] The catalyst according to
[12] ,
[13] or
[14] , wherein the crystallite size is greater than 20 nm.
[0040]
[16] A catalyst configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein the catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and in a TPD spectrum, the temperature of the maximum peak in the range of 450°C to 800°C is 490°C to 650°C.
[0041]
[17] The catalyst according to
[16] , wherein the saturated adsorption amount of pyridine is 100 μmol or more per 1 g of the catalyst.
[0042]
[18] The catalyst according to
[16] or
[17] , wherein the crystallite size is greater than 20 nm.
[0043]
[19] A catalyst configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein the catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and the saturated adsorption amount of pyridine is greater than 100 μmol relative to 1 g of the catalyst.
[0044]
[20] The catalyst according to
[19] , wherein the crystallite size is greater than 20 nm.
[0045]
[21] A catalyst configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein the catalyst contains a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and the crystallite size is greater than 20 nm.
[0046]
[22] A catalyst configured to promote a decomposition reaction of nitrous oxide or a decomposition reaction of nitrous oxide and nitric oxide, wherein the catalyst comprises a zeolite not containing OSDA and an iron element supported on the zeolite.
[0047]
[23] The catalyst according to [1] to
[22] , wherein even after exposure to a 530°C gas containing 20% H2O and 20 ppm SO2 for 70 hours, the NO2 decomposition rate is still above 60% and the NO decomposition rate is still above 90% at 450°C.
[0048]
[24] A catalyst element comprising a substrate and the catalyst according to any one of [1] to
[23] covering the substrate.
[0049]
[25] A method for reducing nitrous oxide or nitrous oxide and nitric oxide from a gas containing at least one selected from water and sulfur oxides and nitrous oxide, or from a gas containing at least one selected from water and sulfur oxides, nitrous oxide and nitric oxide, comprising the following steps: decomposing nitrous oxide or nitrous oxide and nitric oxide by bringing the gas containing at least one selected from water and sulfur oxides and nitrous oxide or the gas containing at least one selected from water and sulfur oxides, nitrous oxide and nitric oxide, and a reducing agent into contact with the catalyst described in any one of [1] to
[23] or the catalyst element described in
[24] .
[0050]
[26] The method according to
[25] , wherein the reducing agent is ammonia or urea.
[0051]
[27] The method according to
[25] or
[26] , wherein the gas containing at least one selected from water and sulfur oxides and nitrous oxide, or the gas containing at least one selected from water and sulfur oxides, nitrous oxide and nitric oxide is combustion exhaust gas of ammonia fuel.
[0052]
[28] The method according to any one of
[25] to
[27] , wherein the water content in the gas is 10% or more and the sulfur oxide content is 15 ppm or more.
[0053]
[29] An exhaust gas treatment device comprising: a reactor containing the catalyst described in any one of [1] to
[23] or the catalyst element described in
[24] ;
[0054] a first supply pipeline configured to allow the processed gas to flow into the reactor;
[0055] a second supply pipeline configured to allow the reducing agent to flow into the reactor; and
[0056] an exhaust line configured to allow gas to flow from the reactor,
[0057] The gas to be treated is a gas containing at least one selected from water and sulfur oxides and nitrous oxide, or a gas containing at least one selected from water and sulfur oxides, nitrous oxide and nitric oxide.
[0058]
[30] The device according to
[29] , wherein the treated gas is exhaust gas from a coal-fired fluidized bed boiler, exhaust gas from an ammonia fuel engine, or exhaust gas from an ammonia fuel gas turbine.
[0059]
[31] The exhaust gas treatment device according to
[29] or
[30] , wherein the water content in the treated gas is 10% or more and the sulfur oxide content is 15 ppm or more.
[0060]
[32] An ammonia fuel engine comprising the device described in
[29] ,
[30] or
[31] .
[0061] Effects of the Invention
[0062] Even if the treated gas contains a large amount of water and / or sulfur oxides, the N2O decomposition catalyst of the present invention can still effectively promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide in the presence of ammonia. The method of the present invention can effectively reduce nitrous oxide from a gas containing water and / or sulfur oxides and nitrous oxide. The method of the present invention can effectively reduce nitrous oxide and nitric oxide from a gas containing water and / or sulfur oxides, nitrous oxide and nitric oxide. The present invention can be appropriately used for the purification treatment of exhaust gas from catalyst-fired coal-fired fluidized bed boilers, exhaust gas from ammonia-fueled ship engines, exhaust gas from ammonia-fueled gas turbines, and exhaust gas from nitrification processes or denitrification processes in water treatment, which contain a large amount of water and / or sulfur oxides. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] Figure 1 FIG. 1 is a diagram showing an example of an ammonia co-firing engine equipped with an exhaust gas treatment system.
[0064] Figure 2 FIG. 1 is a diagram showing an example of an ammonia co-firing engine equipped with an exhaust gas treatment system.
[0065] Figure 3 It is a graph showing TPD spectra of catalysts A to F.
[0066] Figure 4 This is a graph showing the N2O decomposition rate with respect to the temperature for catalysts A to F.
[0067] Figure 5 This is a graph showing the NO decomposition rate with respect to temperature for catalysts A to F.
[0068] Figure 6 It is a graph showing the catalytic reaction rate of N2O relative to the pyridine desorption amount w at 150-450°C.
[0069] Figure 7 It is a diagram showing TPD spectra of catalysts G, H, and J to N.
[0070] Figure 8 This is a graph showing the N2O decomposition rate with respect to temperature for catalysts G, H, and J to N.
[0071] Fig. 9 This is a graph showing the NO decomposition rate with respect to temperature for catalysts G, H, and J to N.
[0072] Fig.10 It is a graph showing the N2O decomposition rate with respect to the temperature of the catalysts J2 and G2.
[0073] Fig.11 It is a graph showing the NO decomposition rate with respect to the temperature of the catalysts J2 and G2.
[0074] Fig.12 It means that for catalyst J, J H , K, K H , G, and G H Plot of N2O decomposition rate as a function of temperature.
[0075] Fig.13 It means that for catalyst J, J H , K, K H , G, and G H A graph of the NO decomposition rate as a function of temperature.
[0076] Fig.14 It is a graph showing the N2O decomposition rate with respect to the temperature for the catalysts O, P, Q, R, and S.
[0077] Fig.15 It is a graph showing the NO decomposition rate with respect to the temperature for the catalysts O, P, Q, R, and S. DETAILED DESCRIPTION
[0078] The N2O decomposition catalyst of the present invention contains a carrier containing SiO2 and Al2O3 and an iron element supported on the carrier.
[0079] In the carrier, SiO 2 and Al 2 O 3 may be contained as a mixture or as a composite.
[0080] Examples of the complex of SiO2 and Al2O3 include aluminosilicate (xM2O·yAl2O3·zSiO2·nH2O) and the like.
[0081] Specific examples of aluminosilicates include mullite (3Al2O3·2SiO2 to 2Al2O3·SiO2); kaolinite (Al4Si4O 10 (OH)8); illite ((K,H3O)(Al,Mg,Fe)2(Si,Al)4O10 [(OH)2,(H2O)]); zeolite; feldspars such as sodium aluminosilicate, potassium aluminosilicate, calcium aluminosilicate ((Na,K,Ca,Ba)Al(Al,Si)Si2O8), etc.
[0082] Examples of the zeolite include amicisite, analcime, barrerite, bellbergite, bikitaite, boggsite, brewsterite, brewsterite-Sr, brewsterite-Ba, chabazite, chabazite-Ca, chabazite-Na, chabazite-K, chabazite-Sr, chabazite-Ba ...Ba, chabazite-Ca, chabazite-Na, chabazite-K, chabazite-Sr, chabazite-Ba, chabazite-Ba, chabazite-Ca, chabazite-Na, chabazite-K, chabazite-Sr, chabazite-Ba, chabazite-Ba, chabazite-Ca, chabazite-Na, chabazite-K, chabazite-Sr, chabazite-Ba, chabazite-Ba, chabazite-Ca, chabaz iavennite), clinoptilolite, clinoptilolite-K, clinoptilolite-Na, clinoptilolite-Ca, cowlesite, dachiardite, dachiardite-Ca, dachiardite-Na, edingtonite, epistilbite, erionite, erionite-Na te-Na), erionite-K, erionite-Ca, faujasite, faujasite-Na, faujasite-Ca, faujasite-Mg, ferrierite, ferrierite-Mg, ferrierite-K, ferrierite-Na, garronite, gaultite, gismondite ine), gmelinite, gmelinite-Na, gmelinite-Ca, gmelinite-K, gobbinsite, gonnardite, goosecreekite, gottardiite, harmome, heulandite, heulandite-Ca, heulandite-Sr, heulandite-Na,heulandite-K, hsianghualite, kalborsite, laumontite, levyne, levyne-Ca, levyne-Na, lovdarite, maricopaite, mazzite, merlinoite, mesolite, montesommaite, mordenite, mutinite aite), natrolite, offretite, pahasapaite, partheite, paulingite, paulingite-Na, paulingite-K, paulingite-Ca, perlialite, phillipsite, phillipsite-Na, phillipsite-K, phillipsite-Ca -Ca), pollucite, roggianite, scolecite, stellerite, stilbite, stilbite-Ca, stilbite-Na, terranovaite, thomsonite, tschernichite, tschortnerite, wairakite, weinebeneite, willhenite natural zeolites such as dersonite), yugawaralite, etc.; A-type (LTA-type) zeolite, X-type (FAU-type) zeolite, LSX-type (FAU-type) zeolite, β-type (BEA-type) zeolite, ZSM-5-type (MFI-type) zeolite, ferrierite-type (FER-type) zeolite, mordenite-type (MOR-type) zeolite, L-type (LTL-type) zeolite, Y-type (FAU-type) zeolite, MCM-22-type (MWW-type) zeolite, offretite / erionite-type (O / E-type) zeolite, AEI-type zeolite, AEL-type zeolite, AFT-type zeolite, AFX-type zeolite, CHA-type zeolite, EAB-type zeolite, ERI-type zeolite, KFI-type zeolite, LEV-type zeolite, LTN-type zeolite,Synthetic zeolites such as MSO zeolite, RHO zeolite, SAS zeolite, SAT zeolite, SAV zeolite, SFW zeolite, TON zeolite, and TSC zeolite.
[0083] Among these, the carrier used in the present invention is preferably zeolite, more preferably synthetic zeolite, and still more preferably BEA-type zeolite.
[0084] The ratio of SiO2 to Al2O3 (SiO2 / Al2O3 molar ratio) is preferably greater than 1, more preferably greater than 5, further preferably greater than 10, and further preferably greater than 20. The greater the ratio of SiO2, the higher the durability of the catalyst tends to be. Therefore, the upper limit of the SiO2 / Al2O3 molar ratio is not particularly limited as long as it can be manufactured. For example, it is preferably 100, more preferably 60, and further preferably 55.
[0085] Synthetic zeolite can be obtained, for example, by mixing a silica source, an alumina source, an alkali source, a solvent, an organic structure-directing agent (OSDA), a surfactant, etc. to obtain a starting reaction mixture, and subjecting the starting reaction mixture to a hydrothermal reaction at high temperature and high pressure in an autoclave. The synthetic zeolite obtained by this method contains an organic component derived from OSDA. However, it seems that the organic component can be removed by subsequent calcination.
[0086] Certain types of synthetic zeolites can be obtained by hydrothermal reaction without using OSDA. Furthermore, certain types of synthetic zeolites can be obtained by mechanochemical treatment and steam synthesis without using OSDA. Synthetic zeolites obtained without using OSDA (hereinafter sometimes referred to as OSDA-free zeolites) do not contain organic components from OSDA. In the present invention, OSDA-free zeolites can be appropriately used. The SiO2 / Al2O3 molar ratio in the OSDA-free zeolite is preferably greater than 1, more preferably greater than 5, and further preferably greater than 8. The upper limit of the SiO2 / Al2O3 molar ratio in the OSDA-free zeolite is, for example, preferably 50, more preferably 45, and further preferably 40.
[0087] The iron element is carried on the carrier in the form of Fe, Fe(III), Fe(II), Fe(II,III) and the like. Fe(III), Fe(II), Fe(II,III) can be in the form of iron oxide, iron oxyhydroxide, iron hydroxide and the like. The carrying can be in the form of iron particles or iron compound (such as iron oxide, etc.) particles attached to the carrier, or in the form of cations of the elements constituting the carrier exchanging with iron cations (ion exchange). In the decomposition reaction of N2O, the carried iron element can be in the form of high-valent iron such as Fe(IV), Fe(V), Fe(VI) and the like.
[0088] The amount of iron element loaded, in terms of Fe2O3 conversion, is preferably 0.1% by weight or more, more preferably 1% by weight or more, more preferably 2% by weight or more, and further preferably 3% by weight or more, relative to the carrier. The upper limit of the amount of iron element loaded is not particularly limited as long as it is an amount that can be loaded, for example, in terms of Fe2O3 conversion, it is preferably 10% by weight, more preferably 7% by weight, relative to the carrier. The method of loading is not particularly limited, for example, it can be loaded by impregnating an aqueous solution or suspension of an iron compound into the carrier, followed by drying / calcining.
[0089] The N2O decomposition catalyst of the present invention may, as required, carry other metal elements on the aforementioned carrier, and / or may further include a carrier in which other metal elements are carried on another carrier.
[0090] As other metal elements, there can be mentioned copper group elements (Cu, Ag, Au), platinum group elements (Pt, Rh, Pd, Ru, etc.), transition metal elements (Co, Ni, etc., excluding Fe), base metal elements (V, Mo, W, etc.), etc., which can be expected to promote the decomposition reaction of N2O or promote the decomposition reaction of N2O and the decomposition reaction of NO. As other carriers carrying other metal elements, there can be mentioned carriers containing SiO2, Al2O3, SiO2-Al2O3, ZrO2, TiO2, TiO2-SiO2, SiC, etc.
[0091] The N2O decomposition catalyst of the present invention has an acid site derived from an OH group or the like. The properties of the acid site can generally be observed by a method known as the pyridine-TPD method. In the pyridine-TPD method, for example, a flame ionization detector (FID) can be used as a detector. Pyridine will adsorb on the acid site. Pyridine can adsorb on the acid sites on the outer surface of the pores of the catalyst and on the acid sites on the inner surface of the pores. It is generally understood that the higher the desorption temperature of the adsorbed pyridine, the stronger the acid strength of the acid site. In addition, it is also believed that the pyridine desorbed at a high temperature is from the acid site affected by diffusion, that is, the pyridine present on the acid site on the inner surface of the pore (Nakano et al. "Determination of the Acid Properties of Zeolites by the Temperature Desorption Method" Toyo Soda Research Report Vol. 29 No. 1 (1985), pp3-11). The effective molecular diameter of pyridine is considered to be (Refer to Anderson et al. J. Catal., 58, 114 (1979)). Moreover, the total amount of acid sites can be determined by the saturated adsorption amount of pyridine. When pyridine is adsorbed and then the temperature is raised at a certain rate (20°C / min), the acid strength distribution of the acid sites can be determined by the distribution of the amount of pyridine released at each temperature (this distribution is sometimes referred to as a TPD spectrum). In addition, in the present invention, the adsorption of pyridine can be carried out at room temperature to 150°C, preferably at 150°C.
[0092] In the N2O decomposition catalyst of the present invention, in the TPD spectrum, the ratio of the total amount of pyridine released in the range of 150°C to less than 450°C to the total amount of pyridine released in the range of 450°C to 800°C is preferably 0.9 or more, more preferably 0.98 or more, further preferably 1 or more, and further preferably 1.1 or more. The upper limit of the ratio of the total amount of pyridine released in the range of 150°C to less than 450°C to the total amount of pyridine released in the range of 450°C to 800°C is not particularly limited as long as it can be manufactured.
[0093] In the N2O decomposition catalyst of the present invention, in the TPD spectrum, the total amount of pyridine released in the range of 150°C to less than 450°C is preferably 100 μmol or more, more preferably 200 μmol or more, further preferably 250 μmol or more, and further preferably 300 μmol or more relative to 1 g of the catalyst. The upper limit of the total amount of pyridine released in the range of 150°C to less than 450°C is not particularly limited as long as it can be manufactured.
[0094] In the N2O decomposition catalyst of the present invention, in the TPD spectrum, the total amount of pyridine released in the range of 450°C to 800°C is preferably 1000 μmol or less, more preferably 800 μmol or less, and further preferably 500 μmol or less relative to 1 g of the catalyst. The lower limit of the total amount of pyridine released in the range of 450°C to 800°C is not particularly limited as long as it can be manufactured.
[0095] In the N2O decomposition catalyst of the present invention, in the TPD spectrum, the value of the L peak (the amount of pyridine removed from the maximum peak top in the range of 150°C or more and less than 450°C) is greater than the value of the H peak (the amount of pyridine removed from the maximum peak top in the range of 450°C or more and 800°C or less). That is, the ratio of the value of the L peak to the value of the H peak is preferably greater than 1, more preferably greater than 1.12, further preferably greater than 1.2, further preferably greater than 1.4, and most preferably greater than 1.6. The upper limit of the ratio of the value of the L peak to the value of the H peak is not particularly limited as long as it can be manufactured.
[0096] In the N2O decomposition catalyst of the present invention, in the TPD spectrum, the lower limit of the temperature at which the H peak appears (the temperature of the maximum peak top in the range of not less than 450°C and not more than 800°C) is preferably 490°C, more preferably 510°C, and further preferably 530°C, and the upper limit is preferably 650°C, more preferably 620°C, further preferably 600°C, and further preferably 580°C.
[0097] The N2O decomposition catalyst of the present invention is preferably a catalyst having a large saturated adsorption amount of pyridine. The saturated adsorption amount of pyridine in the N2O decomposition catalyst of the present invention is preferably 100 μmol or more, more preferably 200 μmol or more, further preferably 500 μmol or more, and further preferably 700 μmol or more, relative to 1 g of the catalyst. The upper limit of the saturated adsorption amount of pyridine in the N2O decomposition catalyst of the present invention is not particularly limited as long as it can be manufactured. For example, it is preferably 2000 μmol, more preferably 1500 μmol, relative to 1 g of the catalyst. The saturated adsorption amount of pyridine can be measured at 150°C.
[0098] The N2O decomposition catalyst of the present invention is preferably a catalyst with a larger crystallite size. The crystallite size in the N2O decomposition catalyst of the present invention is preferably 5 nm or more, more preferably 10 nm or more, further preferably 20 nm or more, and further preferably 30 nm or more. The upper limit of the crystallite size of the N2O decomposition catalyst of the present invention is not particularly limited as long as it can be manufactured, for example, it is preferably 100 nm, and more preferably 80 nm. The crystallite size can be measured by X-ray diffraction (for example, refer to JIS H 7805 or JIS R 7651).
[0099] The N2O decomposition catalyst of the present invention is preferably a catalyst in which the NO2 decomposition rate and the NO decomposition rate are still high even after being exposed to a 530°C gas containing 20% H2O and 20ppm SO2 for 70 hours. The N2O decomposition catalyst of the present invention is preferably a catalyst in which the NO2 decomposition rate is still 60% or more and the NO decomposition rate is still 90% or more under the condition of 450°C even after being exposed to a 530°C gas containing 20% H2O and 20ppm SO2 for 70 hours.
[0100] The catalyst of the present invention having such pyridine adsorption characteristics is excellent in water resistance and / or sulfur oxide resistance, and is excellent in the effect of promoting the decomposition reaction of N2O or promoting the decomposition reaction of N2O and NO.
[0101] The N2O decomposition catalyst of the present invention can promote not only the reduction reaction of N2O contained in the gas alone, but also the reduction reaction of NO or NO2. The N2O decomposition catalyst of the present invention can be used in combination or in admixture with a known catalyst (denitrification catalyst) configured in a manner capable of reducing NO or NO2. By using the N2O decomposition catalyst of the present invention in combination or in admixture with a denitrification catalyst, nitrogen oxides (NO, NO2, N2O) contained in the exhaust gas can be more effectively reduced.
[0102] As an example of the reduction reaction of NO or NO 2 by ammonia, the one represented by the following formula can be cited.
[0103] 4NO+4NH3+O2→4N2+6H2O
[0104] NO+NO2+2NH3→2N2+3H2O
[0105] 6NO2+8NH3→7N2+12H2O
[0106] As an example of the reduction reaction of nitrous oxide by ammonia, the one represented by the following formula can be mentioned.
[0107] 3N2O+2NH3→4N2+3H2O
[0108] The N2O decomposition catalyst of the present invention can be formed into balls, Raschig rings, Bell saddle packings, Pall rings, honeycombs, plates, corrugations, etc. by known forming methods. In addition, it can also be made into a catalyst element, which contains a substrate of a desired shape and the N2O decomposition catalyst of the present invention coated with the substrate. Examples of the substrate include honeycomb substrates, corrugated substrates, lath substrates (mesh metal, punched metal plate, wire mesh, etc.), etc.
[0109] The exhaust gas treatment device of the present invention comprises: a reactor containing the N2O decomposition catalyst or catalyst element of the present invention; a first supply pipeline configured to allow the treated gas to flow into the reactor; a second supply pipeline configured to allow the reducing agent to flow into the reactor; and an exhaust pipeline configured to allow the gas to flow out of the reactor. The N2O decomposition catalyst or catalyst element of the present invention can be accommodated in the reactor in a manner to form a fixed layer, a fluidized layer, or a moving layer. In the exhaust gas treatment device of the present invention, the treated gas is a gas containing at least one selected from water and sulfur oxides and nitrous oxide, or a gas containing at least one selected from water and sulfur oxides, nitrous oxide, and nitric oxide. In the treated gas, the water content is preferably 10% or more and / or the sulfur oxide content is 15 ppm or more.
[0110] As the treated gas used in the present invention, for example, there can be cited exhaust gas from coal-fired fluidized bed boilers, exhaust gas from ammonia fueled ship engines, exhaust gas from ammonia fueled gas turbines, etc. The treated gas used in the present invention may further contain nitrogen dioxide, carbon monoxide, carbon dioxide, hydrogen, hydrocarbons, oxygen, nitrogen, etc. in addition to sulfur oxides (SOx) and / or water (H2O) and nitrous oxide and / or nitric oxide.
[0111] Figure 1 This is a diagram showing an example of an ammonia fuel engine having an exhaust gas treatment device of the present invention. A reducing agent (such as ammonia or urea) 6 is added together with dilution air (not shown) and the like to the gas exhausted from the cylinder 1 of the ammonia co-firing engine (ammonia fuel engine) through the exhaust manifold 5. The mixed gas of the exhaust gas and the reducing agent flows into a catalytic reactor 2 having a fixed layer 8 filled with the N2O decomposition catalyst of the present invention. In the fixed layer 8 filled with the N2O decomposition catalyst, mainly N2O and NOx are decomposed and chemically changed into N2 and H2O. The gas exhausted from the catalytic reactor drives the turbine 12 in the turbocharger, flows out of the turbocharger and is discharged to the outside of the system through the exhaust pipe 15. The rotation of the turbine 12 causes a compressor 13 disposed in the turbocharger and coaxial with the turbine 12 to rotate. The compressor 13 compresses the inhaled air 3. The compressed air is supplied to the cylinder 1 via the intake manifold 14 of the ammonia co-firing engine. The fuel 4 is combusted in the cylinder. In addition, Figure 1 In the conventional turbocharger, fuel is mixed with compressed air and then supplied to the cylinder. However, in the case of a diesel engine, fuel can be injected into the cylinder.
[0112] Figure 2This is a diagram showing another example of an ammonia fuel engine having an exhaust gas treatment device of the present invention. The gas exhausted from the cylinder 1 of the ammonia co-firing engine (ammonia fuel engine) via the exhaust manifold 5 drives the turbine 12 in the turbocharger. The rotation of the turbine 12 causes the compressor 13, which is arranged in the turbocharger and is coaxial with the turbine 12, to rotate. The compressor 13 compresses the sucked air 3. The compressed air is supplied to the cylinder 1 via the intake manifold 14 of the ammonia co-firing engine. The fuel 4 is burned in the cylinder. In addition, Figure 2 Although the fuel is mixed with compressed air and then supplied to the cylinder, in the case of a diesel engine, the fuel can be injected into the cylinder. The reducing agent (such as ammonia or urea) 6 is added to the gas flowing out of the turbocharger together with the dilution air (not shown). The mixed gas of the exhaust gas and the reducing agent flows into the catalytic reactor 2 having a fixed layer 8 filled with the N2O decomposition catalyst of the present invention. In the fixed layer 8 filled with the N2O decomposition catalyst, mainly N2O and NOx are decomposed and chemically changed into N2 and H2O. The gas exhausted from the catalytic reactor is discharged to the outside of the system via the exhaust pipe 15.
[0113] The method of the present invention is used to reduce nitrous oxide or nitrous oxide and nitric oxide from a treated gas. The method of the present invention comprises: decomposing nitrous oxide or nitrous oxide and nitric oxide by contacting the catalyst or catalyst element of the present invention with the treated gas and a reducing agent. From the viewpoint of catalyst life, the less the water content in the treated gas, the better, and more preferably less than 30%. The method of the present invention is effective even for a treated gas with a high water content, such as a treated gas with a water content of more than 1% and a treated gas with a water content of more than 10%. From the viewpoint of catalyst life, the less the sulfur oxide (SOx) content in the treated gas, the better, and more preferably less than 300ppm, and further preferably less than 250ppm. The method of the present invention is effective even for a treated gas with a high SOx content, such as a treated gas with a SOx content of more than 1ppm, a treated gas with a SOx content of more than 5ppm, and a treated gas with a SOx content of more than 15ppm.
[0114] The content of nitrous oxide in the treated gas is not particularly limited, and is preferably 1 ppm or more and 1000 ppm or less, more preferably 10 ppm or more and 500 ppm or less. The content of nitric oxide in the treated gas is not particularly limited, and is preferably 1 ppm or more and 1000 ppm or less, more preferably 5 ppm or more and 500 ppm or less. In the treated gas, the content of water and / or the content of sulfur oxides is preferably 15 ppm or more.
[0115] Although sulfur dioxide (SO2) easily causes the side reaction listed in the following formula, the N2O decomposition catalyst of the present invention can suppress the progress of the side reaction (this property is referred to as sulfur oxide resistance in this application).
[0116] 2SO2+O2→2SO3
[0117] Water (H2O) is also generated by the reduction reaction of nitrogen oxides. If a large amount of water is present in the system, the dealumination of the carrier is likely to proceed, but the N2O decomposition catalyst of the present invention can suppress the progress of dealumination (this property is referred to as water resistance in this application).
[0118] In the method of the present invention, the contact between the treated gas and the reducing agent and the N2O decomposition catalyst or catalyst element can be carried out by a known method, for example, using a fixed bed reactor, a fluidized bed reactor, a moving bed reactor, a simulated moving bed reactor, etc.
[0119] The temperature during contact is preferably 200 to 950° C., more preferably 300 to 700° C., and further preferably 400 to 500° C. The pressure during contact may be the same as atmospheric pressure or higher than atmospheric pressure. If a higher pressure is used, it is expected that the frequency (adsorption rate) of contact between the catalyst and nitrous oxide, nitric oxide, and the reducing agent will increase.
[0120] As the reducing agent used in the present invention, there can be mentioned: nitrogen-based reducing agents such as ammonia and urea; hydrocarbon-based reducing agents such as methane, ethane, propane, propylene, methanol, and dimethyl ether; hydrogen; carbon monoxide, etc. Among these, nitrogen-based reducing agents are preferred, and ammonia or urea is more preferred. Regarding the amount of reducing agent, there is no particular limitation as long as it is an amount that can fully decompose the dinitrogen monoxide or dinitrogen monoxide and nitric oxide contained in the gas. For example, in the case of ammonia, the amount of reducing agent is preferably 0.67 to 1.2 moles relative to 1 mole of the total amount of dinitrogen monoxide and nitric oxide. The reducing agent can be added to the treated gas and mixed using a known gasifier, injector, etc. In the combustion exhaust gas of ammonia fuel, the amount of ammonia remaining in the combustion exhaust gas can also be set by adjusting the combustion rate of the ammonia fuel.
[0121] The present invention will be described in more detail below. Note that these examples are merely examples of the present invention, and the scope of the present invention is not limited thereto.
[0122] Catalyst Preparation Example 1
[0123] (Supporting step <ion exchange>)
[0124] 60 g of BEA type zeolite (SiO2 / Al2O3 ratio = 25) was placed in 2000 ml of an aqueous solution containing 13.2 g of iron (III) nitrate nonahydrate (Fe2(NO3)3·9H2O) heated to 80°C, and then stirred for 3 hours while maintaining the temperature at 80°C to obtain a slurry. The slurry was dehydrated using a suction funnel equipped with filter paper (No.5C). A specified amount of pure water was injected into the filter cake on the filter paper for washing. The washed filter cake was dried at 110°C for 12 hours and calcined at 500°C for 5 hours. The calcined product was crushed using a planetary ball mill to obtain a powdered Fe-loaded zeolite catalyst A.
[0125] (Pyridine-TPD method)
[0126] Fill the adsorption tube with a specified amount (12.5 mg) of catalyst. As a pretreatment, helium is introduced at 30 cc / min, and the catalyst layer temperature is maintained at 450°C for 1 hour. The catalyst layer temperature is lowered to below 100°C. Next, helium is introduced at 10 cc / min, and pyridine is injected into the catalyst layer inlet side of the adsorption tube while maintaining the catalyst layer temperature at 150°C. GC-FID is used to quantify the pyridine at the catalyst layer outlet side. If the amount of pyridine does not change (regarded as saturated adsorption at 150°C), the injection of pyridine is stopped. After 30 minutes have passed since the injection of pyridine was stopped, the catalyst layer temperature was raised at 20°C / min. GC-FID is used to quantify the pyridine at the catalyst layer outlet side between 150°C and 800°C, and the TPD spectrum is recorded. The TPD spectrum and pyridine detachment amount of Fe-loaded zeolite catalyst A are shown in Figure 3 and in Table 1. The crystallite size of the Fe-supported zeolite catalyst A was 14.8 nm.
[0127] (Coating process)
[0128] The Fe-loaded zeolite catalyst A was added to pure water and then stirred to obtain a catalyst slurry. The catalyst slurry was added to a coating amount of 70 g / m 2 The catalyst was applied onto a honeycomb substrate, dried at 120°C for 2 hours, and then calcined at 500°C for 2 hours to obtain a honeycomb catalyst A.
[0129] Catalyst Preparation Example 2
[0130] Powdered Fe-supported zeolite catalyst B and honeycomb catalyst B were obtained by the same method as in Catalyst Preparation Example 1 except that BEA-type zeolite (SiO2 / Al2O3 ratio = 28) was used instead of BEA-type zeolite (SiO2 / Al2O3 ratio = 25). The TPD spectrum and pyridine desorption amount of Fe-supported zeolite catalyst B are shown in Figure 3 And Table 1.
[0131] Catalyst Preparation Example 3
[0132] Powdered Fe-supported zeolite catalyst C and honeycomb catalyst C were obtained by the same method as in Catalyst Preparation Example 1 except that BEA-type zeolite (SiO2 / Al2O3 ratio = 7.5) was used instead of BEA-type zeolite (SiO2 / Al2O3 ratio = 25). The TPD spectrum and pyridine desorption amount of Fe-supported zeolite catalyst C are shown in Figure 3 And Table 1.
[0133] Catalyst Preparation Example 4
[0134] 60 g of CHA-type zeolite (SiO2 / Al2O3 ratio = 24) was placed in 2000 ml of an aqueous solution containing 13.2 g of iron (III) nitrate nonahydrate (Fe2(NO3)3·9H2O) heated to 80°C, and then stirred for 3 hours while maintaining the temperature at 80°C to obtain a slurry. The slurry was filtered through a suction funnel equipped with filter paper (No.5C). A specified amount of pure water was injected into the filter cake on the filter paper for washing. The washed filter cake was dried at 110°C for 12 hours and calcined at 500°C for 5 hours. The calcined product was crushed using a planetary ball mill to obtain a powder.
[0135] The powder was added to 2000 ml of an aqueous solution containing 13.2 g of iron (III) nitrate nonahydrate (Fe2(NO3)3·9H2O), and the above operation was further performed twice (a total of three ion exchange steps) to obtain a powdered Fe-supported zeolite catalyst D. The TPD spectrum and pyridine desorption amount of the Fe-supported zeolite catalyst D are shown in Figure 3 And Table 1.
[0136] A honeycomb catalyst D was obtained by the same method as in Catalyst Preparation Example 1 except that the Fe-supporting zeolite catalyst D was used instead of the Fe-supporting zeolite catalyst A.
[0137] Catalyst Preparation Example 5
[0138] Powdered Fe-supported zeolite catalyst E and honeycomb catalyst E were obtained by the same method as in Catalyst Preparation Example 1 except that MFI zeolite (SiO2 / Al2O3 ratio = 30) was used instead of BEA zeolite (SiO2 / Al2O3 ratio = 25). The TPD spectrum and pyridine desorption amount of Fe-supported zeolite catalyst E are shown in Figure 3 And Table 1.
[0139] Catalyst Preparation Example 6
[0140] Powdered Fe-supported zeolite catalyst F and honeycomb catalyst F were obtained by the same method as in Catalyst Preparation Example 1 except that BEA-type zeolite (SiO2 / Al2O3 ratio = 24) was used instead of BEA-type zeolite (SiO2 / Al2O3 ratio = 25). The TPD spectrum and pyridine desorption amount of Fe-supported zeolite catalyst F are shown in Figure 3 And Table 1.
[0141] [Table 1]
[0142]
[0143] Test Example 1
[0144] The honeycomb catalysts A to F were installed on the reaction tubes. Simulated gases with the composition ratio shown in Table 2 were flowed into the reaction tubes at AV = gas volume / geometric surface area of the catalyst = 25 Nm / hr, and the reaction tubes were set to 400 ° C, 450 ° C and 500 ° C. The N2O decomposition rate and NO decomposition rate at each temperature were measured. The results are shown in Figure 4 and Figure 5 In particular, catalysts A and B have high N2O decomposition rates and NO decomposition rates at 400-500°C.
[0145] [Table 2]
[0146] Composition ratio of simulated gas
[0147]
[0148] Test Example 2
[0149] The same method as in Catalyst Preparation Example 1 was used to obtain various powdered Fe-loaded zeolite catalysts and honeycomb catalysts, except for changing the type of carrier, loading amount, calcination temperature, calcination time, catalyst promoter addition, SiO2 / Al2O3 ratio, etc. The amount of pyridine released in the range of 150°C to less than 450°C was measured by the aforementioned pyridine-TPD method. The N2O decomposition rate was measured in the same manner as in Test Example 1. Based on the measurement results, the catalyst reaction rate was calculated assuming that the N2O decomposition rate at 500°C was a single reaction. The results are shown in Figure 6 It can be seen that the greater the amount of pyridine released in the range of 150°C or more and less than 450°C, the higher the catalyst reaction rate (Nm / hr) tends to be.
[0150] Catalyst Preparation Example 7
[0151] 60 g of BEA type zeolite (SiO2 / Al2O3 ratio = 25) was added to 2000 ml of an aqueous solution containing 9.1 g of iron (II) sulfate heptahydrate (FeSO4·7H2O) heated to 80°C, and then stirred for 3 hours while maintaining the temperature at 80°C to obtain a slurry. The slurry was dehydrated using a suction funnel equipped with filter paper (No.5C). A specified amount of pure water was injected into the filter cake on the filter paper for cleaning. The cleaned filter cake was dried at 110°C for 12 hours and calcined at 500°C for 5 hours. The calcined product was crushed using a planetary ball mill to obtain a powdered Fe-loaded zeolite catalyst G. The TPD spectrum, pyridine desorption amount, crystallite size, etc. of the Fe-loaded zeolite catalyst G are shown in Figure 7 And Table 3.
[0152] The Fe-supported zeolite catalyst G was added to pure water and then stirred to obtain a catalyst slurry. The catalyst slurry was added to a coating amount of 70 g / m 2 The resultant was applied onto a honeycomb substrate, dried at 120°C for 2 hours, and then calcined at 500°C for 2 hours to obtain a honeycomb catalyst G.
[0153] Catalyst Preparation Example 8
[0154] The powdered Fe-supported zeolite catalyst H was obtained by the same method as in Catalyst Preparation Example 7, except that 13.2 g of iron nitrate (III) nonahydrate (Fe2(NO3)3·9H2O) was replaced by 9.1 g of iron (II) sulfate heptahydrate (FeSO4·7H2O) and the calcination temperature was changed from 500°C to 600°C. The TPD spectrum, pyridine desorption amount, crystallite size, etc. of the Fe-supported zeolite catalyst H are shown in Figure 7 And Table 3.
[0155] A honeycomb catalyst H was obtained by the same method as in Catalyst Preparation Example 7 except that the Fe-supporting zeolite catalyst H was used instead of the Fe-supporting zeolite catalyst G.
[0156] Catalyst Preparation Example 9
[0157] 60 g of BEA-type zeolite (SiO2 / Al2O3 ratio = 10) with a larger crystallite size is added to 2000 ml of an aqueous solution containing 26.4 g of iron (III) nitrate nonahydrate (Fe2(NO3)3·9H2O) heated to 80°C, and then stirred for 3 hours while maintaining the temperature at 80°C to obtain a slurry. The slurry is dehydrated using a suction funnel equipped with filter paper (No.5C). A specified amount of pure water is injected into the filter cake on the filter paper for cleaning. The cleaned filter cake is dried at 110°C for 12 hours and calcined at 600°C for 5 hours. The calcined product is crushed using a planetary ball mill to obtain a powdered Fe-loaded zeolite catalyst J. The TPD spectrum, pyridine release amount, crystallite size, etc. of the Fe-loaded zeolite catalyst J are shown in Figure 7 And Table 3.
[0158] The Fe-supported zeolite catalyst J was added to pure water and then stirred to obtain a catalyst slurry. The catalyst slurry was added to a coating amount of 70 g / m 2 The catalyst was applied onto a honeycomb substrate, dried at 120°C for 2 hours, and then calcined at 500°C for 2 hours to obtain a honeycomb catalyst J.
[0159] Catalyst Preparation Example 10
[0160] The same method as in Catalyst Preparation Example 9 was used to obtain powdered Fe-supported zeolite catalyst K and honeycomb catalyst K, except that BEA-type zeolite (SiO2 / Al2O3 ratio = 12) with a larger crystallite size was used instead of BEA-type zeolite (SiO2 / Al2O3 ratio = 10). The TPD spectrum, pyridine desorption amount, crystallite size, etc. of Fe-supported zeolite catalyst K are shown in Figure 7 And Table 3.
[0161] Catalyst Preparation Example 11
[0162] The powdered Fe-supported zeolite catalyst L was obtained by the same method as in Catalyst Preparation Example 9, except that 26.4 g of iron nitrate (III) nonahydrate (Fe2(NO3)3·9H2O) was replaced by 18.2 g of iron (II) sulfate heptahydrate (FeSO4·7H2O) and the calcination temperature was changed from 600°C to 500°C. The TPD spectrum, pyridine desorption amount, crystallite size, etc. of the Fe-supported zeolite catalyst L are shown in Figure 7 And Table 3.
[0163] A honeycomb catalyst L was obtained by the same method as in Catalyst Preparation Example 9 except that the Fe-supporting zeolite catalyst L was used instead of the Fe-supporting zeolite catalyst J.
[0164] Catalyst Preparation Example 12
[0165] The same method as in Catalyst Preparation Example 9 was used except that 26.4 g of iron nitrate (III) nonahydrate (Fe2(NO3)3·9H2O) was replaced with 18.2 g of iron sulfate (II) heptahydrate (FeSO4·7H2O) to obtain powdered Fe-supported zeolite catalyst M and honeycomb catalyst M. The TPD spectrum, pyridine desorption amount, crystallite size, etc. of the Fe-supported zeolite catalyst M are shown in Figure 7 And Table 3.
[0166] Catalyst Preparation Example 13
[0167] A powdery Fe-supported zeolite catalyst N was obtained by the same method as in Catalyst Preparation Example 9 except that the calcination temperature was changed from 600°C to 500°C. The TPD spectrum, pyridine desorption amount, crystallite size, etc. of the Fe-supported zeolite catalyst N are shown in Figure 7 And Table 3.
[0168] Honeycomb Catalyst N was obtained by the same method as in Catalyst Preparation Example 9 except that Fe-supporting zeolite Catalyst N was used instead of Fe-supporting zeolite Catalyst J.
[0169] [Table 3]
[0170]
[0171] Test Example 3
[0172] The honeycomb catalysts G, H and J-N were installed on the reaction tubes. AV = gas volume / geometric surface area of catalyst = 25 Nm / hr (SV = gas volume / catalyst volume = 20000 hr -1 ), simulated gases with the composition ratios shown in Table 4 were flowed into these reaction tubes, and the reaction tubes were set to 350°C, 400°C, and 450°C. The N2O decomposition rate and NO decomposition rate at each temperature were measured. The results are shown in Figure 8 and Fig. 9 Compared with honeycomb catalysts G and H, honeycomb catalysts J to N with larger crystallite sizes and greater release amounts w have higher N2O decomposition rates and NO decomposition rates.
[0173] [Table 4]
[0174] Composition ratio of simulated gas
[0175]
[0176] Catalyst Preparation Example 14
[0177] In addition to the coating weight of 70g / m 2 Changed to coating weight 140g / m 2In addition, the same method as in Catalyst Preparation Example 7 was used to obtain a honeycomb catalyst G2.
[0178] Catalyst Preparation Example 15
[0179] In addition to the coating weight of 70g / m 2 Changed to coating weight 140g / m 2 In addition, the same method as in Catalyst Preparation Example 9 was adopted to obtain a honeycomb catalyst J2.
[0180] Test Example 4
[0181] The honeycomb catalysts G2 and J2 were installed on the reaction tubes. Simulated gases with the composition ratios shown in Table 4 were flowed into the reaction tubes at AV = 25 Nm / hr and 8.3 Nm / hr, and the reaction tubes were set to 350°C, 400°C, and 450°C. The N2O decomposition rate and NO decomposition rate were measured at each temperature and flow rate. The results are shown in Fig.10 and Fig.11 The N2O decomposition rate of the honeycomb catalyst J2 at AV = 25 Nm / hr is about the same as the N2O decomposition rate of the honeycomb catalyst G2 at AV = 8.3 Nm / hr. This can be explained by the fact that the N2O decomposition rate constant of the honeycomb catalyst J2 is about 3 times higher than that of the honeycomb catalyst G2.
[0182] Catalyst Preparation Example 16
[0183] The honeycomb catalysts G, J and K were subjected to hydrothermal treatment for 70 hours under the conditions shown in Table 5 to obtain honeycomb catalysts G, J and K, respectively. H , J H and K H .
[0184] Test Example 5 (Evaluation of Water Resistance / SOx Resistance)
[0185] The honeycomb catalysts G, J, K, G H , J H and K H Installed on the reaction tube. Simulated gas with the composition ratio shown in Table 4 was flowed into these reaction tubes at AV = 25Nm / hr, and the reaction tubes were set to 350℃, 400℃ and 450℃. The N2O decomposition rate and NO decomposition rate at each temperature were measured. The results are shown in Fig.12 and Fig.13 It can be seen that even after the hydrothermal treatment, the N2O decomposition rate and NO decomposition rate of the honeycomb catalyst of the present invention do not decrease much and are maintained at more than 60% and more than 90%, that is, the water resistance and sulfur oxide resistance are excellent.
[0186] [Table 5]
[0187] Hydrothermal treatment conditions
[0188]
[0189] Catalyst Preparation Example 17
[0190] 60 g of BEA-type zeolite (SiO2 / Al2O3 ratio = 10) without OSDA is added to 2000 ml of an aqueous solution containing 18.2 g of iron (II) sulfate heptahydrate (FeSO4·7H2O) heated to 80°C, and then stirred for 3 hours while maintaining the temperature at 80°C to obtain a slurry. The slurry is dehydrated by a suction funnel equipped with filter paper (No.5C). A specified amount of pure water is injected into the filter cake on the filter paper for cleaning. The cleaned filter cake is dried at 110°C for 12 hours and calcined at 500°C for 5 hours. The calcined product is crushed using a planetary ball mill and added to pure water, followed by stirring to obtain a catalyst slurry. The catalyst slurry is coated with 70 g / m 2 The catalyst was applied onto a honeycomb substrate. It was dried at 120°C for 2 hours and then calcined at 500°C for 2 hours to obtain a honeycomb catalyst O. The same test as in Test Example 3 was performed on the honeycomb catalyst O. The results are shown in Fig.14 and Fig.15 .
[0191] Catalyst Preparation Example 18
[0192] 60 g of BEA-type zeolite (SiO2 / Al2O3 ratio = 10) without OSDA is added to 2000 ml of an aqueous solution containing 26.4 g of iron (III) nitrate nonahydrate (Fe2(NO3)3·9H2O) heated to 80°C, and then stirred for 3 hours while maintaining the temperature at 80°C to obtain a slurry. The slurry is dehydrated by a suction funnel equipped with filter paper (No.5C). A specified amount of pure water is injected into the filter cake on the filter paper for cleaning. The cleaned filter cake is dried at 110°C for 12 hours and calcined at 600°C for 5 hours. The calcined product is crushed using a planetary ball mill and added to pure water, followed by stirring to obtain a catalyst slurry. The catalyst slurry is coated with 70 g / m 2 The catalyst was applied on a honeycomb substrate. It was dried at 120°C for 2 hours and then calcined at 500°C for 2 hours to obtain a honeycomb catalyst P. The same test as in Test Example 3 was conducted on the honeycomb catalyst P. The results are shown in Fig.14 and Fig.15 .
[0193] Catalyst Preparation Example 19
[0194] The same method as in Catalyst Preparation Example 18 was used except that the calcination temperature was changed from 600°C to 500°C to obtain a powdered Fe-supported zeolite catalyst Q. The same method as in Catalyst Preparation Example 18 was used except that the Fe-supported zeolite catalyst Q was used instead of the Fe-supported zeolite catalyst P. The same test as in Test Example 3 was performed on the honeycomb catalyst Q. The results are shown in Fig.14 and Fig.15 .
[0195] Catalyst Preparation Example 20
[0196] The same method as in Catalyst Preparation Example 18 was used to obtain powdered Fe-supported zeolite catalyst R and honeycomb catalyst R, except that BEA zeolite (SiO2 / Al2O3 ratio = 12) was used instead of BEA zeolite (SiO2 / Al2O3 ratio = 10) not containing OSDA. The same test as in Test Example 3 was performed on the honeycomb catalyst R. The results are shown in Fig.14 and Fig.15 .
[0197] Catalyst Preparation Example 21
[0198] The same method as in Catalyst Preparation Example 18 was used to obtain powdered Fe-supported zeolite catalyst S and honeycomb catalyst S, except that 26.4 g of iron nitrate (III) nonahydrate (Fe2(NO3)3·9H2O) was replaced with 18.2 g of iron sulfate (II) heptahydrate (FeSO4·7H2O). The same test as in Test Example 3 was performed on the honeycomb catalyst S. The results are shown in Fig.14 and Fig.15 .
[0199] Catalyst Preparation Example 22
[0200] In addition to the coating weight of 70g / m 2 Changed to coating weight 140g / m 2 In addition, the same method as in Catalyst Manufacturing Example 18 was used to obtain a honeycomb catalyst P2. The same test as in Test Example 4 was performed on the honeycomb catalyst P2. The N2O decomposition rate of the honeycomb catalyst P2 at AV = 25 Nm / hr was about the same as the N2O decomposition rate of the honeycomb catalyst G2 at AV = 8.3 Nm / hr. This can be explained by the fact that the N2O decomposition rate constant of the honeycomb catalyst P2 is about 3 times higher than that of the honeycomb catalyst G2.
[0201] Catalyst Preparation Example 23
[0202] The honeycomb catalyst P was subjected to hydrothermal treatment for 70 hours under the conditions shown in Table 5 to obtain a honeycomb catalyst P. H For Honeycomb Catalyst PH The same test as in Test Example 5 was carried out. Even after the hydrothermal treatment (honeycomb catalyst P H ), the N2O decomposition rate and NO decomposition rate of the honeycomb catalyst P did not decrease much and were maintained at more than 60% and more than 90%. That is, the water resistance and sulfur oxide resistance were excellent.
[0203] Explanation of symbols
[0204] 1-engine cylinder, 2-catalytic reactor, 3-air, 4-fuel, 5-exhaust manifold, 6-reductant, 7-temperature regulator, 8-N2O decomposition catalyst fixed layer, 12-turbine, 13-compressor, 14-intake manifold, 15-exhaust pipe.
Claims
1. A catalyst, which is configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein: The catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and In the TPD spectrum, the total amount of pyridine desorbed in the range of 150° C. or higher and lower than 450° C. was 100 μmol or more per 1 g of the catalyst.
2. A catalyst, which is configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein: The catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and In the TPD spectrum, the ratio of the pyridine desorption amount at the maximum peak top in the range of 150°C to less than 450°C to the pyridine desorption amount at the maximum peak top in the range of 450°C to 800°C is larger than 1.
3. A catalyst, which is configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein: The catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and In the TPD spectrum, the ratio of the total amount of pyridine released in the range of 150° C. to less than 450° C. to the total amount of pyridine released in the range of 450° C. to 800° C. is 0.9 or more.
4. A catalyst, which is configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein: The catalyst contains a carrier including SiO2 and Al2O3 and an iron element supported on the carrier, and in a TPD spectrum, a maximum peak top temperature in a range of 450°C to 800°C is 490°C to 650°C.
5. A catalyst, which is configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein: The catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and The saturated adsorption amount of pyridine is 100 μmol or more based on 1 g of the catalyst.
6. A catalyst, which is configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein: The catalyst comprises a carrier comprising SiO2 and Al2O3 and an iron element supported on the carrier, and The crystallite size is 20 nm or more.
7. A catalyst configured to promote the decomposition reaction of nitrous oxide or the decomposition reaction of nitrous oxide and nitric oxide, wherein: The catalyst contains zeolite without an organic structure directing agent (OSDA) and iron element supported on the zeolite.
8. The catalyst according to any one of claims 1 to 7, wherein Even after exposure to a 530°C gas containing 20% H2O and 20 ppm SO2 for 70 hours, the NO2 decomposition rate was still above 60% at 450°C, and the NO decomposition rate was still above 90%. 9 . A catalyst element comprising a substrate and the catalyst according to claim 1 covering the substrate.
10. A method for reducing nitrous oxide or nitrous oxide and nitric oxide from a gas containing at least one selected from water and sulfur oxides and nitrous oxide, or from a gas containing at least one selected from water and sulfur oxides, nitrous oxide and nitric oxide, comprising the following steps: Nitrous oxide or nitrous oxide and nitric oxide are decomposed by bringing a gas containing at least one selected from water and sulfur oxides and nitrous oxide, or a gas containing at least one selected from water and sulfur oxides, nitrous oxide and nitric oxide, and a reducing agent into contact with the catalyst described in any one of claims 1 to 8 or the catalyst element described in claim 9.
11. The method according to claim 10, wherein: The gas has a water content of 10% or more and a sulfur oxide content of 15 ppm or more.
12. An exhaust gas treatment device, comprising: A reactor containing the catalyst according to claims 1 to 8 or the catalyst element according to claim 9; a first supply pipeline configured to allow the processed gas to flow into the reactor; a second supply pipeline configured to allow the reducing agent to flow into the reactor; and an exhaust line configured to allow gas to flow from the reactor, The treated gas is a gas containing at least one selected from water and sulfur oxides and nitrous oxide, or a gas containing at least one selected from water and sulfur oxides, nitrous oxide and nitric oxide.
13. The exhaust gas treatment device according to claim 12, wherein: The gas to be treated has a water content of 10% or more and a sulfur oxide content of 15 ppm or more.
14. An ammonia fuel engine comprising the exhaust gas treatment device according to claim 12 or 13.
Citation Information
Patent Citations
Denitrification catalyst for high temperature waste gas
JP1991296436A
Method for removing nitrous oxide in exhaust gas and catalyst for removing the same
JP1996057262A
A zeolite catalyst supported with iron ions, a method for producing the same, and a method for reducing nitrous oxide alone or both nitrous oxide and nitric oxide simultaneously using an ammonia reducing agent with the catalyst.
JP2012521288A
Organotemplate-free synthetic process for production of zeolitic material
JP2013049624A
Nitrous oxide treatment catalyst and purification method of exhaust gas using the nitrous oxide treatment catalyst
JP2014176808A
Cited By
Multifunctional catalyst for purifying N2O, NOx and NH3 as well as preparation method and application of multifunctional catalyst