Hydraulic shotcrete containing aldehyde modified polymer and construction process
By using aldehyde-based modified polymer admixtures and improved construction technology in hydraulic spray concrete, the durability and strength of hydraulic spray concrete in complex geological environments are solved, and crack resistance, impact wear and resistance are improved. The seepage performance ensures construction safety and surrounding rock stability.
Patent Information
- Application Number
- CN202411099740.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-19
AI Technical Summary
Hydraulic sprayed concrete is prone to bubble, peeling, falling off, large rebound, low early strength, late strength attenuation and poor durability in complex geological environments, making it difficult to meet the construction needs of hydraulic buildings.
Aldehyde-containing modified polymers are used as admixtures, and surface modification is modified through molecular design, combined with improved spray concrete mix ratio and construction technology, including the use of silicate cement with strength grades above 42.5R and specific proportions of aggregates Aldehyde-based modified polymer admixtures form a cross-linking network and a three-dimensional framework to improve crack resistance, impact wear and permeability resistance.
Effectively improve the crack resistance, impact wear and permeability of hydraulic sprayed concrete, and is suitable for complex environments such as surrounding rock alteration, dry and wet circulation, water-rich, etc., extends service life, reduces construction difficulty and maintenance requirements, and ensures The stability of surrounding rocks and construction safety.
Smart Images

Figure CN118978371A_ABST
Abstract
Description
Technical Field
[0001] The invention provides a hydraulic sprayed concrete containing formaldehyde-modified polymer and a construction process, belonging to the technical field of hydraulic construction materials. Background Art
[0002] During the excavation and construction of hydraulic tunnels, shotcrete is used as a temporary support technology. It uses compressed air to spray a mixture of cement, aggregate, water and admixtures onto the designed surface to make it gel into a concrete support measure. The supporting function of shotcrete is to reinforce the rock layer in time, prevent the loosening, peeling and falling of rock blocks, and enhance the stability of the rock mass. Since shotcrete is tightly bonded to the rock layer, it can evenly distribute the load transmitted by the surrounding rock, so as to make full use of the resistance of the rock layer. The rock interface of hydraulic tunnels is often in a humid state, and is greatly affected by complex environmental factors such as dry-wet cycles, water erosion, and ion erosion. It is prone to bubbling, peeling and shedding, resulting in poor durability of concrete, which is difficult to meet the construction needs of hydraulic structures.
[0003] At present, the use of high-grade cement, high-strength aggregate, addition of silica powder, addition of fiber, etc., and modification or optimization of the concrete material composition are common measures to improve the impermeability, abrasion resistance and crack resistance of hydraulic sprayed concrete. The addition of silica powder, expansion agent and other admixtures increases the material cost of high-strength crack-resistant and abrasion-resistant concrete, increases its construction difficulty, maintenance requirements and early cracking risk, and does not fundamentally solve the contradiction between high strength and high crack resistance. CN111320416A discloses a low-rebound high-strength sprayed concrete strengthening agent, which improves the performance of compression, impermeability, wear resistance, etc., but it also exposes many problems in the actual application process. It cannot adapt to the complex geological environment such as surrounding rock alteration, dry-wet cycle, and water-rich, which directly affects the performance and even forms a hidden danger to the service life. Summary of the invention
[0004] The invention provides a hydraulic sprayed concrete containing an aldehyde-modified polymer and a construction process, the purpose of which is to obtain a hydraulic sprayed concrete admixture material through molecular design surface modification, and to improve the mix ratio and construction process of the sprayed concrete, so as to solve the problems of low early strength and poor durability of the hydraulic sprayed concrete in the prior art.
[0005] The technical solution of the present invention: A hydraulic sprayed concrete containing formaldehyde-modified polymer has a strength grade of C25. The raw material components mainly include cementitious materials, aggregates, water and formaldehyde-modified polymer admixtures. The amount of cementitious materials is 420-440 kg / m³, the water-cement ratio is 0.44-0.45, the sand ratio is 58%, and the admixture dosage is 10% of the total amount of cementitious materials.
[0006] Furthermore, the cementitious material is silicate cement with a strength grade of 42.5R or above.
[0007] Furthermore, the aggregate can be coarse aggregate and fine aggregate, and the weight ratio of coarse aggregate to fine aggregate is 1.38:1; the coarse aggregate is 5-15 mm pebbles, with a crushing index of ≤8%, a total content of needle- and flake-like particles ≤4%, a mud content ≤0.5%, and a tight void ratio ≤40%; the fine aggregate is medium-coarse river sand with a fineness modulus of 2.7-3.2, a mud content ≤2.0%, and a mud block content ≤0.5%.
[0008] Furthermore, the aldehyde-modified polymer admixture comprises the following components in parts by mass: Dispersant: 5-20 parts; Modified nanocellulose-based composite hydrogel: 10-20 parts; Nano-silicon calcium oxide: 2-5 parts; Accessories: 2-10 parts; Solvent water: 45-80 parts.
[0009] Furthermore, the dispersant comprises 80-95 parts of a comb-like polymer dispersant and 5-20 parts of a small material. The comb-like polymer dispersant is a six-carbon comb-like polymer super-strong liquid dispersant, the monomer is a polyether, and the molecular weight is greater than 4000. The small material is one or more of polyethylene glycol, 2-acrylamide-2-methylpropane sulfonic acid, sodium methyl allyl sulfonate, β-mercaptopropionic acid, thioglycolic acid, persulfate, azobisisobutyronitrile, diacyl peroxide, and sodium gluconate.
[0010] Further, the nano-silicon calcium oxide is an oxide particle with a particle size of less than 250 nm, preferably an oxide particle with a particle size of less than 200 nm, and more preferably an oxide particle with a particle size of less than 100 nm. The chemical formula of the nano-silicon calcium oxide can be expressed as xCaO·SiO2·yH2O+zCa(OH)2 or xCaO·SiO2·yH2O+zSi(OH)4, wherein x=0.8~2.0, y=4~12, and z=0~2.2, and the value depends on the total ratio of calcium element to silicon element.
[0011] Furthermore, the auxiliary material is one or more of sodium chloride, sodium nitrate, sodium nitrite, sodium sulfate, sodium gluconate, potassium chloride, potassium nitrate, potassium nitrite, and potassium sulfate.
[0012] A construction process for hydraulic sprayed concrete containing formaldehyde-modified polymers comprises the following steps: 1) Construction preparation: Check the size of the excavation section, pry off the loose soil and under-excavated parts on the surface, remove the scum, clean the sprayed surface, drive short steel bars into the rock surface, and mark the scale; when there is a large amount of water on the excavation surface, drain the water in a centralized manner; 2) Preparation of aldehyde-modified polymer admixtures; 3) Shotcrete mixing: The cementitious materials, aggregates and water are matched according to the mix ratio requirements and mixed centrally at a mixing station outside the tunnel. The slump of the mortar is controlled at 100-120 mm and transported to the tunnel by a concrete tank truck; 4) Spraying: Use wet spraying technology. Add formaldehyde-modified polymer admixture to the mortar prepared in step 3) in proportion before spraying and mix thoroughly. First spray 3 cm thick concrete to seal the soil surface, set up steel frames, hang steel mesh, install locking anchor rods, clean the initial sprayed soil surface and then spray again to the designed thickness. 5) Concrete curing: Use a sprayer to cure for more than 7 days 24 hours after final setting.
[0013] Furthermore, the preparation of the aldehyde-modified polymer admixture in step 2) comprises the following steps: S1: Prepare the dispersant; mix the components of the dispersant according to the proportion, stir evenly, heat to 60°C, and cool for later use; S2: Preparation of modified nanocellulose-based composite hydrogels; S3: fully mixing the dispersant with the modified nanocellulose-based composite hydrogel to obtain a dispersion; S4: Preparation of nano-silicon calcium oxide: Add calcium nitrate solution and sodium silicate solution to the dispersion in S3 at the same time, and stir continuously to generate nano-silicon calcium oxide, add auxiliary materials, stir continuously for 24 hours and age, and obtain aldehyde-modified polymer admixture.
[0014] Furthermore, the spraying operation in step 4) is carried out in layers, sections and pieces in a continuous order from bottom to top. First, the low-lying areas are roughly sprayed flat, and then the layers are sprayed back and forth in sequence. When spraying in layers, the thickness of each layer of the top arch is about 5 to 8 cm, and the thickness of each layer of the side wall is 8 to 15 cm, and the thickness of the spray layer is kept uniform; the length of the section should not be greater than 6m; the piecewise spraying should be carried out from bottom to top and the concrete between the steel frame and the soil surface should be sprayed first, and then the concrete between the two steel frames should be sprayed. The side wall spraying concrete should be sprayed upward from the arch foot (wall foot) to prevent the upper spray material from covering the arch foot (corner) without being dense and insufficient in strength, causing the arch foot (corner) to become unstable.
[0015] Furthermore, in step 4), the distance between the nozzle and the sprayed surface is maintained at 0.8 to 1.2 m, and the spray angle is as close to 90° as possible; the spray speed should be appropriate during spraying, which is conducive to the compaction of concrete. If the wind pressure is too high, the rebound will increase; if the wind pressure is too low, the spray speed is too low, the compaction force is small, and it is easy to block the pipe and affect the strength of concrete. The general working wind pressure of the spraying equipment is 0.6 MPa. The wind pressure is adjusted according to the nozzle discharge situation to obtain maximum compaction and minimum rebound.
[0016] Beneficial effects of the present invention: 1) The benzene rings on the modified nanocellulose form a cross-linked network with the polymer quaternary ammonium salt through the cation-π bond, and cooperate with the nano-silicon calcium oxide particles to accelerate hydration, thus ensuring the crack resistance and abrasion resistance of the concrete; 2) Nanocellulose and dispersant jointly construct a three-dimensional skeleton, and the pore points are modified with nano-silicon calcium oxide particles to produce a steric hindrance effect, thereby improving the corrosion resistance coefficient of hydraulic concrete and reducing the shrinkage caused by the carbonization process; 3) Molecular design of nanocellulose, using cationic-aromatic hydrophobic modification, tightly adhering to the negative surface layer while making the hydraulic concrete impermeability grade greater than P12; 4) The product can be applied to shotcrete construction under complex geological conditions such as surrounding rock alteration, low strength, dry-wet cycle, and water-rich conditions. It can effectively solve the problems of conventional shotcrete, such as bubbling, peeling, shedding, large rebound, large cement consumption, low early strength, late strength attenuation, strong corrosion, and poor durability. It is economically friendly, green and environmentally friendly, and improves construction efficiency. After the shotcrete is applied, it can ensure the stability of the surrounding rock and ensure the safety of hydraulic tunnel excavation construction. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them: Figure 1 The present invention is a construction process flow chart of hydraulic sprayed concrete containing formaldehyde-modified polymer. DETAILED DESCRIPTION
[0018] The preparation method of the aldehyde-modified polymer additive comprises the following steps: S1: Prepare dispersant; mix the components of the dispersant in proportion, stir evenly, heat to 60°C, and cool for standby use; wherein the weight proportions of the dispersant are: 80-95 parts of comb polymer dispersant and 5-20 parts of small materials. The comb polymer dispersant is a six-carbon comb polymer super liquid dispersant. The small materials are one or more of polyethylene glycol, 2-acrylamide-2-methylpropane sulfonic acid, sodium methyl allyl sulfonate, β-mercaptopropionic acid, thioglycolic acid, persulfate, azobisisobutyronitrile, diacyl peroxide, and sodium gluconate.
[0019] S2: The preparation of modified nanocellulose-based composite hydrogel is specifically carried out in the following steps: S21: Mixing a cellulose raw material and periodate for oxidation at 65°C for 5 hours, washing and dialyzing the product to obtain formaldehyded nanocellulose, wherein the molar ratio of periodate to cellulose repeating units is 3:1; the cellulose raw material is bleached coniferous wood pulp or pine wood pulp; and the periodate is sodium periodate; S22: Under anaerobic conditions, the aldehyde-modified nanocellulose and the aniline derivative are mixed and reacted for 6 hours, and the product is washed, dialyzed and dried to obtain hydrophobically modified nanocellulose, wherein the molar ratio of aniline to the repeating unit of the aldehyde-modified nanocellulose is (0.5-3):1, preferably (1-2):1; the aniline derivative is aniline hydrochloride; and the drying is vacuum freeze drying at a drying temperature of -30 to -40°C for 24 to 48 hours; S23: Under anaerobic conditions at room temperature, the hydrophobically modified nanocellulose and the propylene quaternary ammonium salt are dissolved in a solvent and fully mixed, and then an ultraviolet initiator and a chemical crosslinking agent are added and stirred to obtain a mixed solution, and the mixed solution is irradiated with a 365nm ultraviolet lamp for 11 hours to initiate a polymerization reaction to obtain a modified nanocellulose-based composite hydrogel. Among them, the molar ratio of the hydrophobically modified nanocellulose repeating unit to the propylene quaternary ammonium salt is (0.5-2):1; the molar ratio of the ultraviolet initiator to the propylene quaternary ammonium salt is 0.25:1, and the molar ratio of the chemical crosslinking agent to the propylene quaternary ammonium salt is (0.1-0.15):1; the solvent is dimethyl sulfoxide, the propylene quaternary ammonium salt is (3-acrylamidopropyl) trimethylammonium chloride or (methacryloyloxyethyl) trimethylammonium chloride, the ultraviolet initiator is ketoglutaric acid, and the chemical crosslinking agent is N,N'-methylenebisacrylamide.
[0020] S3: fully mixing the dispersant with the modified nanocellulose-based composite hydrogel to obtain a dispersion; S4: Preparation of nano-silicon calcium oxide: Add calcium nitrate solution and sodium silicate solution to the dispersion in step 3) at the same time, and stir continuously to generate nano-silicon calcium oxide, add auxiliary materials, stir continuously for 24 hours and age, and obtain aldehyde-modified polymer admixture.
[0021] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0023] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0024] The processability test of the present invention uses common commercially available raw materials unless otherwise specified: ① The cement used is P·O 42.5R produced by Sichuan Erlangshan Labahe Cement Co., Ltd.; ② Fine and coarse aggregates are produced by China Hydropower No. 10 Engineering Bureau Co., Ltd.; ③ The water used is drinking water from the Mozigou surface; ④ The admixture is the formaldehyde-modified polymer prepared by the present method. The admixtures in Comparative Examples 1-3 are commercially available admixtures, with a water reducer content of 1.0% and an accelerator content of 8.0%.
[0025] The performance of the material prepared in the embodiment of the present invention was tested as follows: A 100×100×100mm specimen was cut from a large plate at the test site for compression testing. The strength of the concrete was evaluated by comparing the strength of the large plate cut specimens at 8h, 16h, 24h, 3d, and 28d. The test method was based on the standard cube compression test method for concrete in the "Testing Procedures for Hydraulic Concrete" (DL / T5150-2017), and the compression test was carried out using a WBS-1000 universal material testing machine.
[0026] The test hydraulic sprayed concrete mix ratio is as follows:
[0027] A 100×100×100mm specimen was cut from a large plate at the test site for compression testing. The strength of the concrete was evaluated by comparing the strength of the large plate cut specimen at 8h, 16h, 24h, 3d, and 28d. The rebound rate of the shotcrete was evaluated based on the average rebound rate of the on-site shotcrete test. The comparison data are as follows:
[0028] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A hydraulic sprayed concrete containing an aldehyde-modified polymer, with a strength grade of C25, Features The raw material components mainly include cementitious materials, aggregates, water and formaldehyde-modified polymer admixtures; The amount of the cementitious material is 420-440 kg / m³, the water-cement ratio is 0.44-0.45, the sand ratio is 58%, and the amount of the formaldehyde-modified polymer admixture is 10% of the total amount of the cementitious material.
2. The hydraulic sprayed concrete containing the aldehyde-modified polymer according to claim 1, Features The cementitious material is silicate cement with a strength grade of 42.5R or above; the aggregate includes one or more of coarse aggregate and fine aggregate, and the weight ratio of the coarse aggregate to the fine aggregate is 1.38:1; the coarse aggregate is 5-15 mm pebbles, with a crushing index of ≤8%, a total content of needle- and flake-like particles of ≤4%, a mud content of ≤0.5%, and a tight void ratio of ≤40%; the fine aggregate is medium-coarse river sand with a fineness modulus of 2.7-3.2, a mud content of ≤2.0%, and a mud block content of ≤0.5%.
3. The hydraulic sprayed concrete containing formaldehyde-modified polymer according to claim 1, Features The aldehyde-modified polymer admixture comprises the following components in parts by mass: Dispersant: 5-20 parts; Modified nanocellulose-based composite hydrogel: 10-20 parts; Nano-silicon calcium oxide: 2-5 parts; Accessories: 2-10 parts; Solvent water: 45-80 parts.
4. The hydraulic sprayed concrete containing the formaldehyde-modified polymer according to claim 3, Features The dispersant comprises 80-95 parts of a comb polymer dispersant and 5-20 parts of a small material; The comb-like polymer dispersant is a six-carbon comb-like polymer super-strong liquid dispersant, the monomer is a polyether, and the molecular weight is greater than 4000; The small material is one or more of polyethylene glycol, 2-acrylamide-2-methylpropane sulfonic acid, sodium methyl allyl sulfonate, β-mercaptopropionic acid, thioglycolic acid, persulfate, azobisisobutyronitrile, diacyl peroxide, and sodium gluconate; The nano-silicon calcium oxide is an oxide particle with a particle size less than 250 nm; The auxiliary material is one or more of sodium chloride, sodium nitrate, sodium nitrite, sodium sulfate, sodium gluconate, potassium chloride, potassium nitrate, potassium nitrite and potassium sulfate.
5. A construction process for hydraulic sprayed concrete containing formaldehyde-modified polymers, Features The following steps are involved: 1) Construction preparation: Check the size of the excavation section, pry off the loose soil and under-excavated parts on the surface, remove the scum and the sprayed surface, drive short steel bars into the rock surface, and mark the scale; if there is a large amount of water on the excavation surface, drain the water in a centralized manner; 2) Preparation of aldehyde-modified polymer admixtures; 3) Shotcrete mixing: The cementitious materials, aggregates and water are matched according to the mix ratio requirements provided in claims 1 and 2, and are centrally mixed at a mixing station outside the tunnel. The slump is controlled at 100-120 mm, and then transported to the tunnel by concrete tank trucks; 4) Spraying: Use wet spraying technology. Add formaldehyde-modified polymer admixture to the mortar prepared in step 3) in proportion before spraying and mix thoroughly. First spray 3 cm thick concrete to seal the soil surface, set up steel frames, hang steel mesh, install locking anchor rods, clean the initial sprayed soil surface and then spray again to the designed thickness. 5) Concrete curing: Use a sprayer to cure for more than 7 days 24 hours after final setting.
6. A construction process for hydraulic sprayed concrete containing formaldehyde-modified polymer according to claim 5, Features Step 2) The preparation of the aldehyde-modified polymer admixture comprises the following steps: S1: Mix the components of the dispersant according to claim 4 in proportion, stir evenly, heat to 60° C., and cool for later use; S2: preparing the modified nanocellulose-based composite hydrogel according to claim 3; S3: fully mixing the dispersant with the modified nanocellulose-based composite hydrogel to obtain a dispersion; S4: simultaneously dripping calcium nitrate solution and sodium silicate solution into the dispersion liquid described in S3, and continuously stirring to generate nano-silicon calcium oxide, adding the auxiliary material described in claim 4, continuously stirring and aging for 24 hours, and obtaining an aldehyde-modified polymer admixture.
7. A construction process for hydraulic sprayed concrete containing formaldehyde-modified polymer according to claim 6, Features The step of preparing the modified nanocellulose-based composite hydrogel in S2 comprises: S21: oxidizing the cellulose raw material with periodate at 65°C for 5 h, washing and dialyzing the product to obtain aldehyde-modified nanocellulose; S22: under anaerobic conditions, the aldehyde-modified nanocellulose and the aniline derivative are mixed and reacted for 6 hours, and the product is washed, dialyzed and dried to obtain hydrophobically modified nanocellulose; S23: Under anaerobic conditions at room temperature, the hydrophobically modified nanocellulose and propylene quaternary ammonium salt are dissolved in a solvent and fully mixed, and then an ultraviolet initiator and a chemical cross-linking agent are added and stirred evenly to obtain a mixed solution, and the mixed solution is irradiated with an ultraviolet lamp for 11 hours to initiate a polymerization reaction to obtain a modified nanocellulose-based composite hydrogel.
8. A construction process for hydraulic sprayed concrete containing formaldehyde-modified polymer according to claim 7, Features In step S21, the molar ratio of periodate to cellulose repeating units is 3:1; The cellulose raw material is bleached conifer pulp or pine pulp; the periodate is sodium periodate; In the step S22, the molar ratio of the derivative to the aldehyde-modified nanocellulose repeating unit is (0.5-3):1; the aniline derivative is aniline hydrochloride; the drying is vacuum freeze drying, the drying temperature is -30--40°C, and the drying time is 24-48h; In the step S23, the solvent is dimethyl sulfoxide; the molar ratio of the hydrophobically modified nanocellulose repeating unit to the propylene quaternary ammonium salt is (0.5-2):1; the propylene quaternary ammonium salt is one or more of (3-acrylamidopropyl)trimethylammonium chloride or (methacryloyloxyethyl)trimethylammonium chloride; the molar ratio of the ultraviolet initiator, the chemical crosslinker and the propylene quaternary ammonium salt is 0.25:(0.1-0.15):1; the ultraviolet initiator is ketoglutaric acid, and the chemical crosslinker is N,N'-methylenebisacrylamide; the wavelength of the ultraviolet lamp is 365nm.
9. A construction process for hydraulic sprayed concrete containing formaldehyde-modified polymer according to claim 5, Features Step 4) The spraying operation is carried out in layers, sections and slices in a continuous order from bottom to top; first, the low-lying areas are roughly sprayed flat, and then the layers are sprayed back and forth in sequence; During the layered spraying, the thickness of each layer of the top arch is about 5 to 8 cm, and the thickness of each layer of the side wall is 8 to 15 cm, and the thickness of the sprayed layer is kept uniform; the length of the segment is less than 6 m; The piecewise spraying is carried out from bottom to top, first spraying the concrete between the steel frame and the soil surface, and then spraying the concrete between the two steel frames.
10. A construction process for hydraulic sprayed concrete containing formaldehyde-modified polymer according to claim 9, Features During spraying, the nozzle should be kept at a distance of 0.8 to 1.2 m from the sprayed surface, and the spraying angle should be as close to 90° as possible; the working air pressure of the spraying equipment is 0.6 MPa.
Citation Information
Cited By
High-performance sprayed concrete for tunnel and preparation method of high-performance sprayed concrete
CN122059651A
High-performance shotcrete for tunnel and method for preparing the same