Method for shaping and deoxidizing titanium powder through one-step method
By combining ball milling shaping and mechanical alloying, low-temperature deoxidation and morphology optimization of titanium powder were achieved, solving the problem of simultaneous deoxidation and shaping in existing technologies, improving the performance and application efficiency of titanium powder, and making it suitable for the preparation of titanium alloy materials.
Patent Information
- Application Number
- CN202411022713.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing technologies have not yet achieved simultaneous deoxidation and shaping of titanium powder, which limits the development of titanium powder in high-performance applications, and most of them rely on high-temperature processes.
A combination of ball milling shaping and mechanical alloying was used to mix ball milling balls, hydrogenated dehydrogenated titanium powder, and metal reducing agent in an inert atmosphere. Subsequently, the reducing agent was oxidized in air and then acid-washed and water-washed to achieve low-temperature deoxidation and morphology optimization of the titanium powder.
The deoxidation and morphology optimization of titanium powder at low temperature were achieved, reducing the oxygen content to below 1000ppm and changing the morphology to near-spherical or ellipsoidal, which improved the fluidity and forming performance, reduced energy consumption and cost, and is suitable for the preparation of titanium alloy materials.
Smart Images

Figure CN118989315A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium alloy material preparation, and particularly relates to a one-step method for shaping and deoxidizing titanium powder. Background Art
[0002] Titanium alloys are widely used in aerospace, medical devices, and 3C industries due to their excellent mechanical properties and corrosion resistance. As a key raw material for the preparation of titanium alloys, the oxygen content and morphology of titanium powder directly affect the performance of the final product. At present, titanium powder deoxidation technologies mainly include calcium reduction, sodium reduction, and magnesium reduction. However, most of these technologies rely on high-temperature processes, and there have been no reports on low-temperature deoxidation technologies. At the same time, the existing technology has not yet achieved the simultaneous deoxidation and shaping of titanium powder, which limits the further development of titanium powder in high-performance applications. Summary of the invention
[0003] Based on this, the purpose of the present invention is to provide a one-step method for shaping and deoxidizing titanium powder, which realizes deoxidation and morphology optimization of titanium powder by combining ball milling shaping and mechanical alloying. The method of the present invention has the advantages of low-temperature deoxidation, low energy consumption, low cost, high efficiency, etc. The prepared titanium powder is suitable for the preparation of titanium alloy materials.
[0004] The technical solution of the present invention is as follows:
[0005] A one-step method for shaping and deoxidizing titanium powder, the method comprising:
[0006] (1) In an inert atmosphere, ball milling balls, hydrogenated dehydrogenated titanium powder and a metal reducing agent are mixed and ball milled.
[0007] According to an embodiment of the present invention, step (1) further comprises separating ball milling balls.
[0008] According to an embodiment of the present invention, titanium powder and a metal reducing agent with low oxygen content are obtained in step (1). Preferably, the oxygen content of the titanium powder is less than 1000 ppm.
[0009] According to an embodiment of the present invention, the method further comprises:
[0010] (2) placing the titanium powder with low oxygen content obtained in step (1) and the metal reducing agent in air to oxidize the reducing agent to obtain a mixed powder.
[0011] According to an embodiment of the present invention, the method further comprises:
[0012] (3) The mixed powder obtained in step (2) is subjected to acid washing, and after the acid washing is completed, the solution is separated from the powder.
[0013] According to an embodiment of the present invention, the method further comprises:
[0014] (4) The powder obtained in step (3) is washed and dried to obtain titanium powder with low oxygen content.
[0015] According to an embodiment of the present invention, in step (1), the hydrogenated dehydrogenated titanium powder is non-spherical or non-ellipsoidal, for example, has an irregular shape with sharp corners. Preferably, the particle size of the hydrogenated dehydrogenated titanium powder is 5-150 μm.
[0016] According to an embodiment of the present invention, in step (1), the metal reducing agent may be calcium and / or magnesium. Preferably, the metal reducing agent may be in the form of granules or powder. Preferably, the metal reducing agent may be calcium granules and / or magnesium powder. Preferably, the particle size of the metal reducing agent is 0.1-3 mm.
[0017] According to an embodiment of the present invention, in step (1), the mass ratio of hydrogenated dehydrogenated titanium powder, metal reducing agent and ball milling balls is 1:(0.03-0.3):(1-10), preferably 1:(0.05-0.2):(1-6).
[0018] According to an embodiment of the present invention, in step (1), the temperature during ball milling is 15-50 degrees Celsius; the time of ball milling is 2-8 hours, and the speed of ball milling is 200-600 rpm.
[0019] According to an embodiment of the present invention, in step (1), the ball milling balls can be separated by screening.
[0020] According to an embodiment of the present invention, in step (1), the ball milling balls are made of agate balls or titanium alloy balls.
[0021] According to an embodiment of the present invention, in step (2), the time for which the titanium powder with low oxygen content and the metal reducing agent obtained in step (1) are placed in the air is not particularly limited, as long as the metal reducing agent is completely oxidized. For example, the time for which the titanium powder with low oxygen content and the metal reducing agent are placed in the air is 1-3 days.
[0022] Preferably, the metal reducing agent is oxidized in air to metal oxides, illustratively to calcium oxide and / or magnesium oxide.
[0023] According to an embodiment of the present invention, in step (3), the mixed powder obtained in step (2) is mixed with an acid for pickling. The acid is, for example, hydrochloric acid. The concentration and content of the acid are not particularly limited, as long as the pH value of the system after the mixed powder and the acid are mixed is not higher than 5.
[0024] According to an embodiment of the present invention, in step (3), after the acid washing is completed, the obtained mixed solution can be separated from the powder by sedimentation separation or centrifuge separation.
[0025] According to an embodiment of the present invention, in step (4), water is used for washing. Specifically, water is used for washing until the pH value of the mixed solution reaches 7.
[0026] According to the embodiment of the present invention, in step (4), the drying time and temperature are not particularly limited, and the drying time and temperature are sufficient to dry the moisture in the titanium powder.
[0027] According to an embodiment of the present invention, in step (4), the titanium powder is nearly spherical or ellipsoidal.
[0028] According to an embodiment of the present invention, in step (4), the oxygen content in the titanium powder is less than 1000 ppm.
[0029] As an exemplary embodiment of the present invention, the method specifically comprises the following steps:
[0030] 1) mixing and ball milling balls, hydrogenated dehydrogenated titanium powder and a metal reducing agent, and separating the ball milling balls to obtain titanium powder with low oxygen content and residual metal reducing agent;
[0031] 2) placing the titanium powder with low oxygen content obtained in step 1) and the residual metal reducing agent in a material tray, and exposing them to air for 1-2 days until the metal reducing agent is oxidized in the air to generate metal oxides (such as calcium oxide and / or magnesium oxide), thereby obtaining a mixed powder;
[0032] 3) pouring the mixed powder obtained in step 2) into a dilute hydrochloric acid solution for pickling, pouring the mixed powder in batches while stirring the solution, and after the pickling is completed, separating the solution from the powder by sedimentation separation or centrifuge separation, and washing the obtained powder with water until the pH value of the mixed solution is neutral;
[0033] 4) The washed titanium powder in step 3) is placed in a vacuum dryer for drying for 12-72 hours to obtain titanium powder with low oxygen content.
[0034] Beneficial effects of the present invention:
[0035] (1) The method of the present invention subjects hydrogenated dehydrogenated titanium powder to ball milling with a metal reducing agent and ball milling balls (the three are subjected to intense impact and collision), causing the atoms in the powder particles to diffuse, and the metal reducing agent to undergo an in-situ reduction reaction with the oxide film on the surface of the hydrogenated dehydrogenated titanium powder. The hydrogenated dehydrogenated titanium powder is reduced to titanium by the metal reducing agent, thereby achieving the effect of reducing the oxygen content of the titanium powder.
[0036] (2) During the ball milling process, the hydrogenated dehydrogenated titanium powder of the present invention is subjected to centrifugal force and impact energy, so that the hydrogenated dehydrogenated titanium powder undergoes collision, compression and shearing forces, thereby achieving sphericalization of the powder and ultimately controlling its particle size and morphology.
[0037] (3) The method of the present invention achieves deoxidation and morphology optimization of titanium powder at a relatively low temperature, with low energy consumption and low cost; the powder shaping and deoxidation processes are carried out in one step with high efficiency, thus reducing the time and cost consumption caused by multi-step operations.
[0038] (4) The oxygen content of the titanium powder treated by the method of the present invention is significantly reduced (for example, not higher than 1000 ppm), and the morphology is optimized to be nearly spherical or ellipsoidal, which improves the fluidity and molding performance of the titanium powder, and is suitable for the needs of the metal injection molding (MIM) and 3D printing industries.
[0039] In summary, the present invention achieves deoxidation and morphology optimization of titanium powder by combining ball milling and mechanical alloying, has the advantages of low-temperature deoxidation, low energy consumption, low cost, high efficiency, etc., and is suitable for the preparation of titanium alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is the SEM image of the raw material hydrogenated dehydrogenated titanium powder of Example 1.
[0041] Figure 2 This is the SEM image of the titanium powder after ball milling in Example 1. DETAILED DESCRIPTION
[0042] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0043] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0044] Example 1
[0045] 1. Mix hydrogenated dehydrogenated titanium powder (with an irregular sharp-angled shape), calcium particles with a particle size of 1-3 mm, and ball milling balls (such as agate balls or titanium alloy balls) in a weight ratio of 1:0.1:5 and put them into a ball mill.
[0046] 2. Introduce argon gas into the ball mill, set the ball mill speed to 300 rpm, the ball milling time to 4 hours, and perform ball milling at room temperature.
[0047] 3. After the ball milling is completed, the material is poured out into a glove box protected by argon gas, and the grinding balls are sieved and separated to obtain titanium powder with low oxygen content and residual calcium particles.
[0048] 4. Spread the titanium powder with low oxygen content and the remaining calcium particles in a tray and expose them to the air for 1 day until the calcium particles are oxidized to form calcium oxide to obtain a mixed powder.
[0049] 5. Slowly pour the mixed powder into a container filled with dilute hydrochloric acid solution, pour the mixed powder in batches while stirring the solution until the calcium oxide completely reacts with the hydrochloric acid to form calcium chloride, and keep the pH value of the solution between 3-4.
[0050] 6. After the pickling is completed, the solution is separated from the powder by a centrifuge, and deionized water is added to the pickling container to wash the powder. The number of washes is 5 times until the pH value of the water reaches 7.
[0051] 7. The thoroughly washed titanium powder is placed in a feed tray and placed in a vacuum dryer for 24 hours.
[0052] 8. The oxygen content of the titanium powder after drying is less than 1000ppm, and the morphology of the titanium powder changes from an irregular sharp-angled morphology to a nearly spherical morphology.
[0053] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A one-step method for shaping and deoxidizing titanium powder, characterized in that: The method comprises: (1) In an inert atmosphere, ball milling balls, hydrogenated dehydrogenated titanium powder and a metal reducing agent are mixed and ball milled.
2. The method according to claim 1, characterized in that: The method further comprises: (2) placing the titanium powder with low oxygen content obtained in step (1) and the residual metal reducing agent in air to oxidize the reducing agent to obtain a mixed powder.
3. The method according to claim 2, characterized in that The method further comprises: (3) The mixed powder obtained in step (2) is subjected to acid washing, and after the acid washing is completed, the solution is separated from the powder.
4. The method according to claim 3, characterized in that The method further comprises: (4) The powder obtained in step (3) is washed and dried to obtain titanium powder with low oxygen content.
5. The method according to claim 1, characterized in that In step (1), the metal reducing agent is calcium and / or magnesium.
6. The method according to claim 1, characterized in that In step (1), the mass ratio of hydrogenated dehydrogenated titanium powder, metal reducing agent and ball milling balls is 1:(0.03-0.3):(1-10).
7. The method according to claim 1, characterized in that In step (1), the temperature during ball milling is 15-50 degrees Celsius; the ball milling time is 2-8 hours, and the ball milling speed is 200-600 rpm.
8. The method according to claim 4, characterized in that In step (4), the titanium powder with low oxygen content is nearly spherical or ellipsoidal.
9. The method according to claim 4, characterized in that In step (4), the oxygen content in the titanium powder with low oxygen content is less than 1000 ppm.
Citation Information
Patent Citations
Method for producing low oxygen hydrogenated dehydrogenated titanium powder
CN109202090A
Spherical titanium powder and preparation method thereof as well as 3D printing product
CN109604617A
Titanium powder for 3D printing and preparation method and device thereof
CN115026292A
Titanium alloy material for 3D printing and preparation method thereof
CN116393705A
Pure titanium powder, method for preparing pure titanium powder from titanium waste and application of pure titanium powder
CN117921015A
Cited By
Preparation method of low-oxygen titanium-containing powder
CN119819922A
A method for preparing a low-oxygen titanium-containing powder
CN119819922B