Modified inorganic fiber material, preparation method thereof and automobile roof composite material

By distributing porous powder materials and adhesives in the inorganic fiber layer of the car roof material to form modified inorganic fiber materials, the problem of insufficient sound absorption and noise reduction function of existing car roof materials is solved, and significant noise reduction and passenger comfort are achieved promote.

CN118993578APending Publication Date: 2024-11-22SSI NEW MATERIAL (ZHENJIANG) CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310557936.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing car ceiling materials have shortcomings in improving sound absorption and noise reduction functions, and have failed to effectively improve the material level, resulting in poor noise control in the car.

Method used

Using modified inorganic fiber materials, the porous powder material and adhesive are distributed in the three-dimensional network structure of the porous inorganic fiber material surface and internal space to form an efficient sound absorption and noise reduction layer. The specific implementation method includes uniform coating of mixed slurry and vacuum freeze-drying treatment to ensure the acoustic performance and sound absorption of the material.

Benefits of technology

It significantly improves the sound absorption coefficient and provides efficient sound absorption and noise reduction function. It can significantly reduce the noise inside the car without changing the preparation process of the car ceiling composite material and improve passenger comfort. The preparation method is simple and easy to use without special equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993578A_ABST
    Figure CN118993578A_ABST
Patent Text Reader

Abstract

The invention provides a modified inorganic fiber material, a preparation method of the modified inorganic fiber material and an automobile roof composite material, and the modified inorganic fiber material comprises a porous inorganic fiber material and a porous powder material, the porous powder material is distributed on the surface of the porous inorganic fiber material and in the three-dimensional network structure of the internal space of the porous inorganic fiber material through the adhesion of the adhesive; wherein the content of the porous powder material and the adhesive is 10-200g / m < 2 >, the content is equal to (C-B) / A, in the formula, A and B are respectively the surface area and the mass of the porous inorganic fiber material, the unit is m2 and g, C is the total weight of the modified inorganic fiber material, and the unit is g. The sound absorption coefficient of the modified inorganic fiber material is remarkably improved, and the modified inorganic fiber material has efficient sound absorption and noise reduction functions; when the composite material is used as the material of the inorganic fiber material layer in the automobile roof composite material, the sound absorption and noise reduction functions of the automobile roof composite material can be remarkably improved, so that the noise in an automobile can be reduced, and the comfort of passengers in the automobile is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a modified inorganic fiber material and a preparation method thereof and a composite material for automobile roof, belonging to the material field, in particular to the technical field of related materials used in automobiles. Background Art

[0002] At present, with the development and progress of society and the improvement of people's living standards, cars have become common consumer goods in thousands of households. At the same time, consumers are paying more and more attention to and requiring the control level of noise and vibration inside cars. NVH (noise vibration harshness) is the subjective feeling characteristics of passengers in terms of hearing, touch and vision. NVH performance is the most easily perceived car performance by passengers and is an important indicator for measuring car quality.

[0003] The car ceiling is one of the important decorative parts in the car interior. It can not only significantly improve the decorative quality of the car interior, but also has the functions of heat insulation and sound insulation, thereby improving the comfort of passengers in the car. The area of ​​the car ceiling is large, so it has an important influence on the absorption of noise in the car. From this perspective, it can be seen that it is of great significance to develop car ceiling materials with high-efficiency sound absorption and noise reduction functions, significantly reduce the noise in the car, and improve the comfort of passengers in the car.

[0004] Some companies have made some attempts and efforts to enhance and improve the sound absorption and noise reduction function of car roofs, as follows.

[0005] CN103921504A discloses a novel automobile roof and its production process. The novel automobile roof disclosed in the invention is composed of composite knitted fabric, glass fiber felt, foam board, glass fiber felt and bottom non-woven fabric from top to bottom, and each layer is compounded by a film. The process of producing the novel automobile roof as described above combines the advantages of simple process and fast production cycle of the dry molding process, and the product molding performance of the wet molding process is better than that of the dry process ceiling and the product has the advantages of lightweight. The molding process is also a dry wet molding (cold material hot mold) molding process. The prior art reduces the VOC performance of the product and improves the NVH performance of the product, and has the advantages of good product molding performance, lightweight product, improved product production cycle, and less pollution to the production environment.

[0006] CN211417409U discloses a composite material automobile roof, including a carbon fiber composite roof body and a sunroof frame, wherein the left end of the carbon fiber composite roof body is bonded with a front reinforcement, and the right end of the carbon fiber composite roof body is bonded with a rear reinforcement, and the sunroof frame is located inside the left end of the carbon fiber composite roof body. Compared with the existing ordinary automobile roof, the composite material automobile roof can reduce the weight of the automobile, making the automobile lightweight, thereby achieving the effect of energy saving and emission reduction, improving the environmental protection of the automobile roof, and improving the rigidity and aging resistance of the automobile roof, thereby improving the dent resistance and service life of the automobile roof, and also improving the specific modulus of the automobile roof, improving the NVH performance of the roof, and also improving the damping of the automobile roof, and the sound insulation performance of the roof, while adopting a wet molding process.

[0007] However, both of these existing technologies improve the preparation process of the automobile roof, but do not improve the materials used in the automobile roof to enhance the sound absorption and noise reduction function.

[0008] Therefore, providing a novel modified inorganic fiber material and a preparation method thereof, and an automobile roof composite material comprising the modified inorganic fiber material has become a technical problem that needs to be solved urgently in the art. Summary of the invention

[0009] In order to solve the above-mentioned shortcomings and deficiencies, an object of the present invention is to provide a modified inorganic fiber material.

[0010] Another object of the present invention is to provide a method for preparing the modified inorganic fiber material.

[0011] Another object of the present invention is to provide a composite material for automobile ceiling, wherein the inorganic fiber material layer is made of the modified inorganic fiber material described above.

[0012] In order to achieve the above objectives, on the one hand, the present invention provides a modified inorganic fiber material, wherein the modified inorganic fiber material comprises a porous inorganic fiber material and a porous powder material, wherein the porous powder material is distributed in a three-dimensional network structure on the surface of the porous inorganic fiber material and in its internal space through bonding with an adhesive;

[0013] The content of the porous powder material and the adhesive is 10-200 g / m 2 , the content = (CB) / A, where A and B are the surface area and mass of the porous inorganic fiber material, respectively, in units of m 2 and g, C is the total weight of the modified inorganic fiber material, in g.

[0014] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the modified inorganic fiber material is prepared by first mixing a porous powder material, an adhesive, an additive and water evenly to obtain a mixed slurry, then evenly coating the mixed slurry on the surface of the porous inorganic fiber material, and then freeze-molding and vacuum freeze-drying.

[0015] As a specific embodiment of the modified inorganic fiber material of the present invention, the porous inorganic fiber material has a loose porous three-dimensional network structure, a thickness of 80-600 μm, and a gram weight of 20-200 g / m 2 .

[0016] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the porous inorganic fiber material includes glass fiber, ceramic fiber, basalt fiber, carbon fiber, quartz fiber, asbestos fiber, volcanic rock fiber, metal fiber or alumina fiber.

[0017] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the porous powder material is a porous powder material with sound absorption and noise reduction functions, including one or a combination of zeolite molecular sieve, activated silica, activated carbon, surface porous calcium carbonate and surface porous calcium silicate.

[0018] In order to enhance the sound absorption and noise reduction effects of the modified inorganic fiber materials to a greater extent, as a specific embodiment of the modified inorganic fiber materials described above in the present invention, the zeolite molecular sieve comprises one or a combination of several of the MFI structure molecular sieve, FER structure molecular sieve, CHA structure molecular sieve, MEL structure molecular sieve, TON structure molecular sieve and MTT structure molecular sieve.

[0019] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the particle size of the zeolite molecular sieve is 0.5-10 μm.

[0020] As a specific embodiment of the modified inorganic fiber material described above, the zeolite molecular sieve includes micropores with a pore size of 0.3-0.7 nm and mesopores with a pore size of 10-30 nm.

[0021] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the zeolite molecular sieve is ZSM-5 molecular sieve.

[0022] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the adhesive includes an organic adhesive and / or an inorganic adhesive; the organic adhesive includes one or a combination of polyacrylate, acrylic copolymer, polyurethane, polystyrene butadiene emulsion, polystyrene acrylate, polystyrene acetate emulsion, polyvinyl acetate emulsion, silicone resin and polybutadiene rubber emulsion; the inorganic adhesive includes one or a combination of silica sol, aluminum sol, pseudo-boehmite, etc.

[0023] As a specific embodiment of the modified inorganic fiber material described above in the present invention, the thickness of the modified inorganic fiber material is determined by the porous inorganic fiber material, and thus the thickness range is also 80-600 μm.

[0024] On the other hand, the present invention also provides a method for preparing the modified inorganic fiber material described above, wherein the preparation method comprises:

[0025] (1) mixing the porous powder material, adhesive, additive and water to obtain a mixed slurry;

[0026] (2) uniformly coating the mixed slurry on the surface of a porous inorganic fiber material;

[0027] (3) Drying the product obtained in step (2) to obtain the modified inorganic fiber material.

[0028] In step (2) of the preparation method of the modified inorganic fiber material described above, the mixed slurry can be evenly coated on one side of the porous inorganic fiber material, and after coating, the mixed slurry will enter the interior of the porous inorganic fiber material and then diffuse to the other side of the porous inorganic fiber material. The mixed slurry can also be evenly coated on both sides of the porous inorganic fiber material at the same time, and after coating, the mixed slurry will enter the interior of the porous inorganic fiber material. In addition, under the premise that the coating amount, that is, the mass of the absolute dry coating (porous powder material and adhesive in the present invention) per unit area is the same, the effects of these two coating methods are the same. It can be seen that no matter which coating method is used, both sides of the inorganic fiber material are modified.

[0029] As a specific embodiment of the preparation method described above in the present invention, the mass ratio of the porous powder material, adhesive, water and additive is 100:4-10:1-159:1-159, preferably 100:5-8.5:5-95:5-95, and the amount of the porous powder material, adhesive and additive is calculated based on the absolute dry mass of the active ingredient.

[0030] As a specific embodiment of the preparation method described above of the present invention, the auxiliary agent is a liquid auxiliary agent that can be frozen at -30°C to -50°C and can sublime at a temperature of 60-80°C and a vacuum degree of less than 15Pa.

[0031] As a specific embodiment of the above preparation method of the present invention, wherein, under the condition of a temperature of 20° C., the viscosity of the liquid auxiliary agent is not less than 500 cp.

[0032] As a specific embodiment of the preparation method described above in the present invention, the auxiliary agent includes one or a combination of ethylene glycol (melting point of -13°C, boiling point of 194°C / 760mmHg), 2,3-butanediol (melting point of 18°C, boiling point of 179°C / 760mmHg), 1,4-butanediol, 1,3-butanediol and 1,5-pentanediol.

[0033] The auxiliary agent used in the present invention is a high-viscosity liquid auxiliary agent. By adjusting its added amount, the purpose of adjusting the viscosity of the mixed slurry can be achieved, so that the viscosity of the mixed slurry meets the needs of the coating operation; at the same time, during the molding and drying process of the modified inorganic fiber material, it is easy to separate from the porous inorganic fiber material, the porous powder material and the adhesive, and does not affect the acoustic properties of the modified inorganic fiber material; and for the auxiliary agents commonly used in this field, such as starch, polyvinyl alcohol, carboxymethyl cellulose, and synthetic coating thickeners, although the purpose of adjusting the viscosity of the mixed slurry can also be achieved by adjusting its added amount, these substances do not volatilize during the molding and drying process of the modified inorganic fiber material, and they will be adsorbed by the porous powder material, thereby having a serious negative impact on the acoustic properties and sound absorption and noise reduction performance of the modified inorganic fiber material.

[0034] As a specific embodiment of the above preparation method of the present invention, the viscosity of the mixed slurry is 30-800cp.

[0035] As a specific embodiment of the preparation method described above in the present invention, the water includes one or a combination of deionized water, distilled water, reverse osmosis water, etc.

[0036] As a specific embodiment of the preparation method described above of the present invention, wherein, in step (3), the drying comprises first freeze-forming the product obtained in step (2), and then performing vacuum freeze-drying treatment on the product obtained after freeze-forming;

[0037] Alternatively, the drying includes directly subjecting the product obtained in step (2) to high temperature drying.

[0038] As a specific embodiment of the preparation method described above of the present invention, the freezing molding temperature is not higher than -20°C, preferably -30°C to -50°C, and the freezing molding time is within 60s;

[0039] The vacuum freeze drying process comprises: after freeze molding, the temperature is raised from no higher than -20°C to 60-80°C through a program temperature increase, and the vacuum degree is maintained at less than 15Pa for vacuum freeze drying.

[0040] As a specific embodiment of the preparation method described above of the present invention, wherein the high temperature drying is drying at 85-150° C. for 60-300 min;

[0041] Preferably, the high temperature drying is carried out under reduced pressure or vacuum. Under this high temperature drying condition, water and additives in the mixed slurry will also be removed, while the porous powder material and adhesive continue to be distributed on the surface and the entire internal structure (the three-dimensional network structure of the internal space) of the porous inorganic fiber material, thereby obtaining a modified inorganic fiber material.

[0042] As a specific embodiment of the preparation method described above of the present invention, step (1) specifically comprises:

[0043] Accurately weigh the required porous powder material, adhesive, and additive, and add them to the required amount of water, and then uniformly disperse and mix the porous powder material, adhesive, and additive by conventional stirring, shearing, ultrasonic and other dispersion methods to obtain a uniformly dispersed mixed slurry. It can be seen that the purpose of step (1) is to prepare a uniformly dispersed mixed slurry and make the mixed slurry have a certain viscosity so as to meet the requirements of the coating operation in step (2).

[0044] As a specific embodiment of the preparation method described above of the present invention, step (2) specifically comprises:

[0045] The mixed slurry is uniformly coated on the surface of the porous inorganic fiber material using a conventional rod coater, a blade coater, a film transfer coater (also known as a roller transfer coater), a rod + blade coater, etc.; and during the coating process, the coating amount can be obtained by adjusting the settings of the coater, adjusting the concentration of the porous powder material in the mixed slurry and the viscosity of the mixed slurry, and selecting porous inorganic fiber materials of different thicknesses. 2 The modified inorganic fiber material.

[0046] Since the porous inorganic fiber material selected in the present invention has a loose porous three-dimensional network structure, after coating, the mixed slurry will be uniformly absorbed by the surface and the three-dimensional network structure of the internal space of the porous inorganic fiber material, and thus uniformly distributed on the surface and the entire internal structure (the three-dimensional network structure of the internal space) of the porous inorganic fiber material. This is different from the coating of the currently conventionally used coated paper, which requires the coating to be on the surface of the base paper as much as possible after coating.

[0047] As a specific embodiment of the preparation method described above, the freeze molding in step (3) specifically includes: after the coating operation is completed, the product obtained in step (2) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding.

[0048] As a specific embodiment of the preparation method described above in the present invention, the vacuum freeze-drying treatment in step (3) specifically includes: when the mixed slurry is completely frozen and formed on the surface of the porous planar carrier material and the entire internal structure (the three-dimensional network structure of the internal space), turning on the vacuum pump, setting the temperature rising program of the vacuum freeze dryer, so that the temperature is raised from no higher than -20°C, preferably from -30°C to -50°C to 60-80°C through the program temperature rising, and maintaining the vacuum degree less than 15Pa for vacuum freeze-drying treatment.

[0049] During the operation of the vacuum freeze dryer, the ultimate vacuum degree of the equipment is extremely low, usually less than 15Pa, so the frozen water and additives in the mixed slurry will gradually begin to sublime, while the porous powder material and adhesive continue to be distributed on the surface and the entire internal structure of the porous inorganic fiber material (the three-dimensional network structure of the internal space), thereby obtaining a modified inorganic fiber material. At the same time, the sublimation of water and additives will generate a large number of evenly distributed pores on the surface and inside of the modified inorganic fiber material, which is conducive to the circulation of air and also helps to give full play to the acoustic properties and sound absorption and noise reduction properties of the porous powder material.

[0050] In another aspect, the present invention further provides a composite material for automobile ceiling, comprising a polyurethane layer, an inorganic fiber material layer and a decorative layer respectively arranged on both sides of the polyurethane layer, wherein the inorganic fiber material layer is made of the modified inorganic fiber material described above. The composite material for automobile ceiling provided by the present invention is a composite material for automobile ceiling with high-efficiency sound absorption and noise reduction function.

[0051] The present invention does not make any specific requirements on the preparation method of the automobile roof composite material. The existing conventional method can be used for preparation, and the preparation method can also be reasonably adjusted and improved according to the actual needs of on-site operations, as long as the automobile roof composite material can be obtained.

[0052] Compared with the prior art, the beneficial technical effects that can be achieved by the present invention include:

[0053] 1. The sound absorption coefficient of the modified inorganic fiber material provided by the present invention is significantly improved, and it has a highly efficient sound absorption and noise reduction function;

[0054] 2. The modified inorganic fiber material provided by the present invention is used as the material of the inorganic fiber material layer in the automobile ceiling composite material. Without changing the original preparation process of the automobile ceiling composite material, the sound absorption and noise reduction function of the automobile ceiling composite material can be significantly improved, thereby reducing the noise inside the car and improving the comfort of the passengers in the car;

[0055] 3. The preparation method of the modified inorganic fiber material provided by the present invention is simple and easy, does not require special equipment, and is simple to operate. In addition, since a coating operation is adopted when preparing the modified inorganic fiber material, the present invention can efficiently prepare the modified inorganic fiber material. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0057] Figure 1 The gram weight used in Example 1 of the present invention obtained by using a high-definition digital microscope is 25g / m 2 Schematic diagram of the surface of glass fiber.

[0058] Figure 2 This is a schematic diagram of the surface of the modified glass fiber obtained in Example 1 of the present invention, obtained using a high-definition digital microscope.

[0059] Figure 3 This is a schematic cross-sectional view of the modified glass fiber obtained in Example 1 of the present invention, obtained using a high-definition digital microscope.

[0060] Figure 4 It is a schematic cross-sectional view of the modified glass fiber prepared in Example 3 of the present invention obtained by using a high-definition digital microscope.

[0061] Figure 5 This is a schematic structural diagram of the automobile ceiling composite material provided in Example 4 of the present invention.

[0062] Description of main figures:

[0063] 1. Polyurethane layer;

[0064] 2. Inorganic fiber material layer;

[0065] 3. Decorative layer. DETAILED DESCRIPTION

[0066] It should be noted that the term "comprises" and any variations thereof in the specification and claims of the present invention are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or devices.

[0067] "Scope" disclosed in the present invention is given in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges defined in this way are combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, for a specific parameter, a range of 60-120 and 80-110 is listed, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​listed are 1 and 2, and the maximum range values ​​listed are 3, 4 and 5, then the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.

[0068] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in the present invention, and "0-5" is just an abbreviation of these numerical combinations.

[0069] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned in the present invention can be combined with each other to form a new technical solution.

[0070] In the present invention, unless otherwise specified, all technical features and preferred features mentioned in the present invention can be combined with each other to form a new technical solution.

[0071] In the present invention, if not specifically stated, the term "two" used in this specification means "at least two".

[0072] In the present invention, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0073] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the attached table, drawings and examples. The following described embodiments are some embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0074] Example 1

[0075] This embodiment provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:

[0076] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 85 parts by weight of deionized water, and 5 parts by weight of ethylene glycol, wherein the amounts of ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol are calculated based on the absolute dry weight of the active ingredients. Add ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 52.5 cP;

[0077] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.

[0078] (b) Use a scraper coater to evenly coat the mixed slurry on a surface with a gram weight of 25 g / m 2 Glass fiber (surface diagram as shown Figure 1 shown).

[0079] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding, and the freeze molding temperature is -40°C and the time is 5 seconds.

[0080] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the heating program of the vacuum freeze dryer is set so that the temperature rises from -40°C to 75°C, and the vacuum degree is maintained at less than 15 Pa for vacuum freeze drying treatment. After the treatment, the modified glass fiber material is obtained, which is marked as test sample 1#.

[0081] The surface schematic diagram and cross-sectional schematic diagram of the test sample 1# prepared in this embodiment are shown as follows: Figure 2-Figure 3 As shown, compared Figure 1 and Figure 2 It can be seen that the porous powder material continues to be distributed on the surface and the entire internal structure of the porous glass fiber material (the three-dimensional network structure of the internal space) through the bonding effect of the adhesive, and the sublimation of water and additives causes a large number of evenly distributed pores to be generated on the surface and inside of the modified glass fiber;

[0082] from Figure 3 It can be seen that the average thickness of test sample 1# is 134μm.

[0083] Example 2

[0084] This embodiment provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:

[0085] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 7 parts by weight of polystyrene butadiene adhesive, 95 parts by weight of deionized water, and 20 parts by weight of ethylene glycol, wherein the amounts of ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol are calculated based on the absolute dry weight of the active ingredients. Add ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 60.0 cP;

[0086] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.

[0087] (b) Use a scraper coater to evenly coat the mixed slurry on a surface with a gram weight of 25 g / m 2 on fiberglass material.

[0088] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding, and the freeze molding temperature is -40°C and the time is 8 seconds.

[0089] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the temperature rising program of the vacuum freeze dryer is set so that the temperature rises from -40°C to 75°C, and the vacuum degree is maintained at less than 15Pa for vacuum freeze drying treatment. After the treatment, the modified glass fiber material is obtained, which is marked as test sample 2#.

[0090] It can be reasonably expected from the characterization results in Example 1 that in the test sample 2# prepared in this example, the porous powder material continues to be distributed on the surface and in the entire internal structure (the three-dimensional network structure of the internal space) of the porous glass fiber material through the bonding effect of the adhesive, and the sublimation of water and additives also causes a large number of evenly distributed pores to be generated on the surface and inside of the modified glass fiber.

[0091] Example 3

[0092] This embodiment provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:

[0093] (a) Accurately weigh 50 parts by weight of ZSM-5 molecular sieve, 50 parts by weight of Silicalite-1 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 3.5 parts by weight of polyacrylate adhesive, 20 parts by weight of deionized water, and 90 parts by weight of ethylene glycol, wherein ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol are all calculated based on the absolute dry mass of the effective ingredients. Add ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 119 cP;

[0094] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm. The average particle size of the Silicalite-1 molecular sieve porous powder material with sound absorption and noise reduction function is 1.4μm, including micropores with a pore size of 0.60nm and mesopores with a pore size of 11nm.

[0095] (b) Use a scraper coater to evenly coat the mixed slurry on a surface with a gram weight of 50 g / m 2 on fiberglass material.

[0096] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding, and the freeze molding temperature is -40°C and the time is 20 seconds.

[0097] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the temperature rising program of the vacuum freeze dryer is set so that the temperature rises from -40°C to 75°C, and the vacuum degree is maintained at less than 15Pa for vacuum freeze drying treatment. After the treatment, the modified glass fiber material is obtained, which is marked as test sample 3#.

[0098] It can be reasonably expected from the characterization results in Example 1 that in the test sample 3# prepared in this example, the porous powder material continues to be distributed on the surface and in the entire internal structure (the three-dimensional network structure of the internal space) of the porous glass fiber material through the bonding effect of the adhesive, and the sublimation of water and additives also causes a large number of evenly distributed pores to be generated on the surface and inside of the modified glass fiber.

[0099] The cross-sectional schematic diagram of the test sample 3# prepared in this embodiment is as follows Figure 4 As shown, from Figure 4 It can be seen that the average thickness of test sample 3# is 352μm.

[0100] Example 4

[0101] This embodiment provides a modified glass fiber material, which differs from the embodiment 1 only in freeze molding and vacuum freeze drying. The modified glass fiber material is prepared by a preparation method comprising the following specific steps:

[0102] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 85 parts by weight of deionized water, and 5 parts by weight of ethylene glycol, wherein the amounts of ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol are calculated based on the absolute dry weight of the active ingredients. Add ZSM-5 molecular sieve, polystyrene butadiene adhesive, and ethylene glycol to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 52.5 cP;

[0103] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.

[0104] (b) Use a scraper coater to evenly coat the mixed slurry on a surface with a gram weight of 25 g / m 2 on fiberglass material.

[0105] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a 90° C. forced air drying oven for drying. After drying for 60 minutes, the modified glass fiber material is obtained, which is marked as test sample 4#.

[0106] Example 5

[0107] This embodiment provides a series of automobile roof composite materials, and its structural schematic diagram is as follows Figure 5 As shown, it includes a polyurethane layer 1, an inorganic fiber material layer 2 respectively arranged on both sides of the polyurethane layer 1, and a decorative layer 3 arranged on the inorganic fiber material layer 2 and facing the interior of the car, wherein the material of the inorganic fiber material layer 2 is the modified glass fiber material provided in Example 1 to Example 4, namely, test sample 1# to test sample 4#.

[0108] The series of automobile ceiling composite materials provided in this embodiment are all automobile ceiling composite materials with high-efficiency sound absorption and noise reduction functions.

[0109] Comparative Example 1

[0110] This comparative example provides a modified glass fiber material, which differs from Example 1 only in that no ethylene glycol additive is added. The modified glass fiber material is prepared by a preparation method comprising the following specific steps:

[0111] (a) Accurately weigh 100 parts by weight of ZSM-5 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, and 85 parts by weight of deionized water, wherein the amounts of ZSM-5 molecular sieve and polystyrene butadiene adhesive are calculated based on the absolute dry weight of the active ingredients. Add ZSM-5 molecular sieve and polystyrene butadiene adhesive to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 6.25 cP;

[0112] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm.

[0113] (b) Use a scraper coater to evenly coat the mixed slurry on a surface with a gram weight of 25 g / m 2 on fiberglass material.

[0114] Coating results: Since the viscosity of the mixed slurry is particularly low, when it is coated on the glass fiber material, the mixed slurry has too good fluidity, and the glass fiber material absorbs the mixed slurry particularly quickly, resulting in a particularly high coating amount on the modified glass fiber material that cannot be precisely controlled, and the uniformity of the resulting material is also very poor.

[0115] By comparing Example 1 with Comparative Example 1, it can be seen that the viscosity of the mixed slurry is very important for the coating operation. The present invention controls the viscosity of the mixed slurry to 30-800cp by liquid additives to successfully achieve the purpose of preparing a modified glass fiber material with excellent performance.

[0116] Comparative Example 2

[0117] This comparative example provides a modified glass fiber material, which is prepared by a preparation method comprising the following specific steps:

[0118] (a) Accurately weigh 50 parts by weight of ZSM-5 molecular sieve, 50 parts by weight of Silicalite-1 molecular sieve, 5 parts by weight of polystyrene butadiene adhesive, 3.5 parts by weight of polyacrylate adhesive, 20 parts by weight of deionized water, and 90 parts by weight of ethylene glycol, wherein ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol are all calculated based on the absolute dry mass of the effective ingredients. Add ZSM-5 molecular sieve, MFI structure molecular sieve, polystyrene butadiene adhesive, polyacrylate adhesive, and ethylene glycol to deionized water and mix and stir evenly to obtain a mixed slurry. The viscosity of the mixed slurry measured by a digital rotational viscometer is 119 cP;

[0119] Among them, the average particle size of the ZSM-5 molecular sieve porous powder material with sound absorption and noise reduction function is 1.5μm, including micropores with a pore size of 0.55nm and mesopores with a pore size of 20nm. The average particle size of the Silicalite-1 molecular sieve porous powder material with sound absorption and noise reduction function is 1.4μm, including micropores with a pore size of 0.60nm and mesopores with a pore size of 11nm.

[0120] (b) Use a scraper coater to evenly coat the mixed slurry on a surface with a gram weight of 50 g / m 2 on fiberglass material.

[0121] (c) After the coating operation is completed, the product obtained in step (b) is quickly / immediately transferred to a vacuum freeze dryer for rapid freeze molding, and the freeze molding temperature is -40°C and the time is 20 seconds.

[0122] (d) After the mixed slurry is completely frozen and formed on the surface and the entire internal structure of the glass fiber material (the three-dimensional network structure of the internal space), the vacuum pump is turned on, and the heating program of the vacuum freeze dryer is set so that the temperature is raised from -40°C to 75°C, and the vacuum degree is maintained at less than 15Pa for vacuum freeze drying treatment. After the treatment, the modified glass fiber material is obtained, which is marked as reference sample 2#.

[0123] Test Example 1

[0124] In this test example, test samples 1# to 4# and reference sample 2# were first cut into 10×10 mm squares, and the contents of molecular sieve and adhesive therein were calculated according to the parameters in Table 1 according to the following formula 1), and the specific results of the contents are shown in Table 1.

[0125] Content of molecular sieve and adhesive = (CB) / A, unit: g / m 2 , formula 1);

[0126] In formula 1), A and B are the surface area and mass of the porous glass fiber material, respectively, in units of m 2 and g, C is the total weight of the modified glass fiber material, in g.

[0127] Table 1

[0128]

[0129] Test Example 2

[0130] This test example uses a standing wave tube, that is, an impedance tube to measure the modified glass fiber materials provided in Examples 1 to 4 and Comparative Example 2, and the gram weight used in the examples and comparative examples is 25 g / m 2 Glass fiber, weight 50g / m 2 The sound pressure changes of the glass fiber at different frequencies are calculated, and the sound absorption coefficient is calculated based on the sound pressure change data. The experimental results are shown in Table 2 below.

[0131] Table 2

[0132]

[0133]

[0134] From the experimental data in Table 2 above, it can be seen that:

[0135] (1) Untreated weight is 25g / m 2 The sound absorption coefficient of the glass fiber material at different frequencies is significantly lower than the sound absorption coefficient of the modified glass fiber material provided in Example 1, Example 2 and Example 4 at the same frequency, which fully proves that the porous powder material with sound absorption and noise reduction function in the modified glass fiber material provided in the embodiment of the present invention has a very obvious effect on absorbing noise.

[0136] (2) Untreated weight is 50g / m 2The sound absorption coefficient of the glass fiber material at different frequencies is significantly lower than the sound absorption coefficient of the modified glass fiber material provided in Example 3 at the same frequency, which fully proves that the porous powder material with sound absorption and noise reduction function in the modified glass fiber material provided in the embodiment of the present invention has a very obvious effect on absorbing noise.

[0137] (3) By comparing the experimental data of Example 4 and Example 1, it can be seen that the sound absorption coefficient of the modified glass fiber material provided in Example 1 at different frequencies is significantly higher than the sound absorption coefficient of the modified glass fiber material provided in Example 4 at the same frequency, which fully proves the importance of the drying method. Freeze drying is better than high-temperature drying. This is because: during the water volatilization process of high-temperature drying, under the action of surface tension, the particles of the porous powder material with sound absorption and noise reduction functions are close to each other, so that no rich pore structure is formed in the glass fiber material; in addition, the film-forming performance of the adhesive in the high-temperature drying process is better than that in the freeze-drying process. After the adhesive film is formed, the glass fiber material is firmly wrapped, so that the pore structure in the glass fiber material is further reduced.

[0138] (4) By comparing the experimental results data of Example 1 or Example 4, Example 2, and Example 3, it can be seen that as the absolute dry adsorption mass of the porous powder material with sound absorption and noise reduction function in the glass fiber material increases (in the modified glass fiber material provided in Example 1 or Example 4, Example 2, and Example 3, the absolute dry adsorption mass of the porous powder material with sound absorption and noise reduction function in the glass fiber material is 9.62 mg, 12.62 mg, and 17.79 mg, respectively), its sound absorption coefficient also increases accordingly.

[0139] In addition, the experimental results of Example 3 and Comparative Example 2 show that when the coating amount exceeds 200 g / m 2 , the sound absorption and noise reduction performance of the modified glass fiber material obtained is reduced. This is because the coating is dense after drying, the density is high, and the porosity is reduced, thereby reducing the sound absorption and noise reduction effect of the modified glass fiber material.

[0140] In summary, compared with the prior art, the beneficial technical effects that can be achieved by the embodiments of the present invention include:

[0141] 1. The sound absorption coefficient of the modified inorganic fiber material provided in the embodiment of the present invention is significantly improved, and it has a highly efficient sound absorption and noise reduction function;

[0142] 2. The modified inorganic fiber material provided in the embodiment of the present invention is used as the material of the inorganic fiber material layer in the automobile ceiling composite material. Without changing the original preparation process of the automobile ceiling composite material, the sound absorption and noise reduction function of the automobile ceiling composite material can be significantly improved, thereby reducing the noise inside the car and improving the comfort of the passengers in the car;

[0143] 3. The preparation method of the modified inorganic fiber material provided in the embodiment of the present invention is simple and easy, does not require special equipment, and is simple to operate. In addition, since a coating operation is used when preparing the modified inorganic fiber material, the embodiment of the present invention can efficiently prepare the modified inorganic fiber material.

[0144] The above is only a specific embodiment of the present invention, and cannot be used to limit the scope of the invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the protection scope of the patent of the present invention, should still fall within the scope of this patent. In addition, the technical features of the present invention can be freely combined with each other, with each other and with each other, and with each other.

Claims

1. A modified inorganic fiber material, characterized in that: The modified inorganic fiber material includes a porous inorganic fiber material and a porous powder material, wherein the porous powder material is distributed on the surface of the porous inorganic fiber material and in a three-dimensional network structure in its internal space through bonding with an adhesive; The content of the porous powder material and the adhesive is 10-200 g / m 2 , the content = (CB) / A, where A and B are the surface area and mass of the porous inorganic fiber material, respectively, in units of m 2 and g, C is the total weight of the modified inorganic fiber material, in g.

2. The modified inorganic fiber material according to claim 1, characterized in that The porous inorganic fiber material has a loose porous three-dimensional network structure, a thickness of 80-600 μm, and a gram weight of 20-200 g / m 2 .

3. The modified inorganic fiber material according to claim 1 or 2, characterized in that: The porous inorganic fiber material includes glass fiber, ceramic fiber, basalt fiber, carbon fiber, quartz fiber, asbestos fiber, volcanic rock fiber, metal fiber or alumina fiber.

4. The modified inorganic fiber material according to claim 1, characterized in that The porous powder material includes one or a combination of zeolite molecular sieve, activated silicon dioxide, activated carbon, surface porous calcium carbonate and surface porous calcium silicate.

5. The modified inorganic fiber material according to claim 4, characterized in that The zeolite molecular sieve includes one or a combination of MFI structure molecular sieve, FER structure molecular sieve, CHA structure molecular sieve, MEL structure molecular sieve, TON structure molecular sieve and MTT structure molecular sieve.

6. The modified inorganic fiber material according to claim 4, characterized in that The particle size of the zeolite molecular sieve is 0.5-10 μm.

7. The modified inorganic fiber material according to claim 4, characterized in that The zeolite molecular sieve comprises micropores with a pore size of 0.3-0.7 nm and mesopores with a pore size of 10-30 nm.

8. The modified inorganic fiber material according to any one of claims 4 to 7, characterized in that: The zeolite molecular sieve is ZSM-5 molecular sieve.

9. The modified inorganic fiber material according to claim 1, characterized in that: The adhesive includes an organic adhesive and / or an inorganic adhesive; wherein the organic adhesive includes one or a combination of polyacrylate, acrylic copolymer, polyurethane, polystyrene butadiene emulsion, polystyrene acrylate, polystyrene acetate emulsion, polyvinyl acetate emulsion, silicone resin and polybutadiene rubber emulsion; wherein the inorganic adhesive includes one or a combination of silica sol, alumina sol and pseudo-boehmite.

10. The modified inorganic fiber material according to claim 1 or 2, characterized in that: The thickness of the modified inorganic fiber material is 80-600 μm.

11. The method for preparing the modified inorganic fiber material according to any one of claims 1 to 10, characterized in that: The preparation method comprises: (1) mixing the porous powder material, adhesive, additive and water to obtain a mixed slurry; (2) uniformly coating the mixed slurry on the surface of a porous inorganic fiber material; (3) Drying the product obtained in step (2) to obtain the modified inorganic fiber material.

12. The preparation method according to claim 11, characterized in that: The mass ratio of the porous powder material, adhesive, water and auxiliary agent is 100:4-10:1-159:1-159, and the dosage of the porous powder material, adhesive and auxiliary agent is calculated based on the absolute dry weight of the active ingredient.

13. The preparation method according to claim 11, characterized in that: The auxiliary agent is a liquid auxiliary agent that can be frozen at -30°C to -50°C and can sublime at a temperature of 60-80°C and a vacuum degree of less than 15Pa.

14. The preparation method according to claim 13, characterized in that: At a temperature of 20° C., the viscosity of the liquid additive is not less than 500 cp.

15. The preparation method according to any one of claims 11 to 14, characterized in that: The auxiliary agent includes one or a combination of ethylene glycol, 2,3-butanediol, 1,4-butanediol, 1,3-butanediol and 1,5-pentanediol.

16. The preparation method according to any one of claims 11 to 14, characterized in that: The viscosity of the mixed slurry is 30-800cp.

17. The preparation method according to any one of claims 11 to 14, characterized in that: The water includes deionized water, distilled water, reverse osmosis water or a combination of the two.

18. The preparation method according to any one of claims 11 to 14, characterized in that: In step (3), the drying comprises first freeze-forming the product obtained in step (2), and then performing vacuum freeze-drying treatment on the product obtained after freeze-forming; Alternatively, the drying includes directly subjecting the product obtained in step (2) to high temperature drying.

19. The preparation method according to claim 18, characterized in that: The freezing molding temperature is not higher than -20°C, preferably -30°C to -50°C, and the freezing molding time is within 60s; The vacuum freeze drying process comprises: after freeze molding, the temperature is raised from no higher than -20°C to 60-80°C through a program temperature increase, and the vacuum degree is maintained at less than 15Pa for vacuum freeze drying.

20. The preparation method according to claim 18, characterized in that: The high temperature drying is 85-150°C drying for 60-300min; Preferably, the high temperature drying is performed under reduced pressure or vacuum environment.

21. A composite material for automobile ceiling, comprising a polyurethane layer, an inorganic fiber material layer and a decorative layer respectively arranged on both sides of the polyurethane layer, characterized in that: The material of the inorganic fiber material layer is the modified inorganic fiber material according to any one of claims 1-10.

Citation Information

Cited By

  • Wearable electronic equipment with shock absorption and noise reduction structure

    CN223413555U

  • Modified inorganic fiber material and preparation method therefor, automobile roof lining composite material, sound insulation composite material, and vehicle

    EP4714752A1