Hydrogen permeation resistant composite resin coating as well as preparation method and application thereof

By modifying the combination of two-dimensional inorganic composite filler and epoxy resin, a composite coating with low hydrogen permeability and strong binding force is prepared, which solves the problem of hydrogen embrittlement caused by easy hydrogen permeability and improves hydrogen energy storage and transportation Security.

CN118995007AActive Publication Date: 2024-11-22DALIAN UNIV OF TECH

Patent Information

Application Number
CN202411261045.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-22
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Hydrogen easily penetrates into metals and leads to hydrogen embrittlement effects, reducing metal strength and increasing the risk of hydrogen leakage, hindering the widespread application of hydrogen energy.

Method used

The modified two-dimensional inorganic composite filler f-MOx@LM was mixed with epoxy resin to prepare a hydrogen permeability composite coating. By peeling off layered materials such as kaolin and growing metal oxides in situ, it formed a two-dimensional high aspect ratio. Structure and hydrogen traps work together to reduce hydrogen permeability.

Benefits of technology

It has achieved a composite coating with extremely low hydrogen permeability, strong binding force, excellent anti-corrosion performance, and simple and controllable preparation process, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995007A_ABST
    Figure CN118995007A_ABST
Patent Text Reader

Abstract

The invention discloses a hydrogen permeation resisting composite resin coating as well as a preparation method and application thereof, and belongs to the technical field of hydrogen permeation resisting. The preparation method of the composite coating mainly comprises the following steps: stripping a layered material (LM) into a single layer / few layers, growing a metal oxide (MOx) on the surface of the stripped LM material in situ, modifying a two-dimensional inorganic composite filler (MOx (at) LM), uniformly dispersing the two-dimensional inorganic composite filler (MOx (at) LM) to epoxy resin (EP), and the like, so as to finally prepare the composite coating, and coating the surface of a base material with the composite coating to form the hydrogen barrier composite coating. The coating can achieve a synergistic effect from the two aspects of structural hydrogen resistance and hydrogen trap hydrogen resistance so as to reduce the hydrogen permeability to the maximum extent. The composite coating is high in binding force with a base material, excellent in hydrogen permeation resistance and corrosion resistance, and the preparation process is simple, convenient, controllable, healthy, environmentally friendly and suitable for large-scale production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a hydrogen permeation-resistant composite resin coating and a preparation method and application thereof, which belongs to the technical field of hydrogen permeation resistance. Background Art

[0002] In order to cope with the energy crisis and environmental problems, it is crucial to promote the development of renewable green energy. Hydrogen energy has become a highly anticipated potential alternative energy source due to its high energy density and emission-free characteristics. However, due to the extremely low diffusion coefficient of hydrogen, it can easily penetrate into metals and induce hydrogen embrittlement, resulting in challenges in the safety of hydrogen storage and transportation. The hydrogen embrittlement effect weakens the strength of metals and increases the risk of hydrogen leakage, which poses an obstacle to the widespread application of hydrogen energy. Therefore, it is necessary to develop new materials and improve surface treatment technologies to ensure the reliability of hydrogen storage and transportation and promote the practical application of hydrogen energy.

[0003] Polymer composite coating is an effective technical means to deal with hydrogen embrittlement. By introducing functional fillers into the polymer matrix, the hydrogen barrier performance of the coating can be significantly improved, thereby effectively slowing down the occurrence of hydrogen embrittlement. This makes polymer composite coatings have important application potential in hydrogen storage equipment and transportation systems, providing a reliable solution to ensure the safe storage and transportation of hydrogen energy. With the development of technology, optimizing the material composition and preparation process of polymer composite coatings will further improve their performance and enable them to play a greater role in the field of hydrogen energy. Summary of the invention

[0004] The purpose of the present invention is to provide a composite coating with excellent hydrogen permeation resistance and a preparation method thereof, so that the prepared composite coating has strong bonding with the substrate, excellent hydrogen permeation resistance, and anti-corrosion performance, and the preparation process is simple and controllable, healthy and environmentally friendly, and suitable for large-scale production and application.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A composite resin coating for preventing hydrogen penetration, the coating is composed of a modified two-dimensional inorganic composite filler f-MO x @LM is mixed with epoxy resin and then cured. The modified two-dimensional inorganic composite filler f-MO x @The weight ratio of LM to epoxy resin EP is 1:19~1:2;

[0007] Two-dimensional inorganic composite filler MO x @LM by MO x Metal oxides are in situ grown on the surface of the exfoliated LM layered materials. xThe weight ratio to LM is 1:100~1:1; the LM layered material after peeling is a single-layer or few-layer material, and the few-layer means that the number of material layers after peeling will be reduced compared with the material before peeling, thereby obtaining a high aspect ratio two-dimensional structure and improving the ability to resist hydrogen penetration.

[0008] The MO x Metal oxides are Al2O3, TiO2, ZnO, Cr2O3, NiO, MgO;

[0009] The LM layered material is a layered non-metallic material, selected from one or more of kaolin, montmorillonite, graphite, sericite, muscovite, boron nitride and hydrotalcite.

[0010] A method for preparing a composite resin coating that blocks hydrogen penetration comprises the following steps:

[0011] S1. The LM layered material is peeled off to obtain a peeled LM layered material;

[0012] S2.MO x Metal oxides are in situ grown on the surface of the exfoliated LM layered material to obtain a two-dimensional inorganic composite filler MO. x @LM;

[0013] S3. Modification of two-dimensional inorganic composite filler MOx@LM;

[0014] S4. Modified two-dimensional inorganic composite filler MO x @LM is dispersed into epoxy resin and coated on the substrate to form a hydrogen permeation barrier coating.

[0015] Furthermore, step S1 specifically includes the following steps:

[0016] (1) Pretreatment: The LM layered material is calcined at high temperature in a muffle furnace, refluxed in a nitric acid solution, filtered, and then stirred in a saturated sodium chloride solution to obtain a pretreated LM layered material;

[0017] (2) Intercalation: Disperse the pretreated LM layered material in deionized water, heat and add the intercalation agent, stir, and wash with water to obtain the intercalated LM layered material;

[0018] (3) The intercalated LM layered material is dispersed in a specific solvent, subjected to ultrasound and centrifugal separation, and an upper clear liquid containing single-layer / few-layer LM nanosheets is obtained at a speed of 900×g-1000×g; the upper clear liquid is then centrifuged at a speed above 10380×g, filtered and washed with water to obtain the LM layered material peeled off into a single-layer / few-layer LM nanosheet.

[0019] Further, the intercalant is one or more of hexadecyltrimethylammonium bromide, N-methylformamide, hydrazine hydrate, urea, lithium borohydride, tetramethylammonium ion, tetraethylammonium ion, tetrapropylammonium ion, tetrabutylammonium ion, sulfate ion, and propylamine;

[0020] The solvent is one or more of ethanol, isopropanol and N,N-dimethylformamide.

[0021] Furthermore, step S2 specifically includes the following steps:

[0022] (1) preparing a precursor solution containing M metal, adding a dispersant or a hydrolysis inhibitor, and then pouring the single-layer / few-layer LM layered material into it and mixing it thoroughly to obtain a solution A;

[0023] (2) Under stirring, add solution B containing a precipitant or hydrolyzing agent, and solution A gradually forms a sol, and metal M grows in situ on a single layer / few layers of LM layered material, and then continue to stir until the sol completely turns into a gel; after drying, calcining and grinding, a two-dimensional inorganic composite filler MO is obtained. x @LM.

[0024] Furthermore, the solute in the precursor solution containing the M metal is an inorganic salt containing the M metal or an organic compound containing the M metal, and the M metal is Al, Ti, Zn, Cr, Ni, or Mg;

[0025] The dispersant or hydrolysis inhibitor is one or more of polyethylene glycol, polypropylene glycol, citric acid, glacial acetic acid, formic acid, anhydrous ethanol, diethanolamine, and acetylacetone.

[0026] The precipitant or hydrolyzing agent is one or more of NaOH, KOH, Na2CO3, K2CO3, (NH4)2CO3, ammonia water, urea, glacial acetic acid, nitric acid and hydrochloric acid.

[0027] Further, step S3 includes the following steps:

[0028] Add the modifier to water or weak acid solution and stir; add two-dimensional inorganic composite filler MO x @LM, stirred, filtered, washed with water, and dried to obtain the modified two-dimensional inorganic composite filler f-MO x @LM.

[0029] Furthermore, the modifier is one or more of 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, and 3-glycidyloxypropylmethyldimethoxysilane.

[0030] Further, step S4 is specifically: the modified two-dimensional inorganic composite filler f-MO x @LM is stirred and mixed with epoxy resin, and then a curing agent is added, and the mixture is evenly mixed in a vacuum degassing mixer to obtain a solvent-free composite coating. The composite coating is coated on a substrate through a wet film preparation device and cured at room temperature to obtain a composite resin coating;

[0031] Furthermore, the epoxy resin is one of glycidyl ether epoxy resin and glycidyl amine epoxy resin; the curing agent is aliphatic amine, alicyclic amine, aromatic amine, phenolic amine or polyamide.

[0032] The invention discloses an application of a composite resin coating that blocks hydrogen penetration, wherein the coating is applied to hydrogen transmission pipelines and hydrogen cylinders.

[0033] Furthermore, the coating thickness is between 5 and 150 μm.

[0034] The composite coating has good hydrogen permeation resistance, mainly due to the selection of one or more of kaolin, montmorillonite, graphite, sericite, muscovite, boron nitride, and hydrotalcite with a layered structure as the lamellar skeleton structure to increase the hydrogen permeation path.

[0035] In order to obtain the maximum path for hydrogen permeation, the original LM layered material is stripped into a single layer / few layers by stripping technology, and the steps are as follows: first, it is calcined at high temperature in a muffle furnace, refluxed at 95°C in a nitric acid solution, and stirred at 95°C in a saturated sodium chloride solution for 3 hours, and then dispersed in deionized water, an intercalation agent is added, and the intercalation treatment is completed by stirring for 24 hours; after the intercalation is completed, it is dispersed in ethanol for further ultrasonic dispersion, and the supernatant containing the single layer / few layers of LM nanosheets is separated at a low speed (940×g), and then the supernatant is centrifuged at a higher speed (greater than 10380×g) for 10~30min, filtered and washed with water to obtain the LM layered material stripped into a single layer / few layers.

[0036] Furthermore, MO grown in situ on the layered material is selected x The metal oxide is one or more of Al2O3, TiO2, ZnO, Cr2O3, NiO, and MgO that contain abundant hydrogen traps (such as irreversible lattice defects), and is in-situ grown and highly dispersed on the surface of the sheet material, further greatly increasing the hydrogen permeation resistance.

[0037] Furthermore, MO x The in-situ growth of metal oxides on the surface of the stripped LM layered material mainly includes the following steps: preparing a precursor solution containing M metal, adding a certain amount of dispersant or hydrolysis inhibitor, and then pouring the stripped LM layered material into it and mixing it thoroughly to obtain a solution A; under vigorous stirring, adding a solution B containing a precipitant or a hydrolyzing agent dropwise, the A solution gradually forms a sol, and the M metal grows in situ on the single-layer / few-layer LM layered material, and then continuing to stir until the sol completely turns into a gel; after drying, calcining at 500°C in a muffle furnace to obtain a two-dimensional inorganic composite filler MO x @LM. This preparation method belongs to the sol-gel method. The prepared metal oxide particles are small and uniform, which can significantly improve MO x The uniformity of metal oxides on the surface of LM layered materials greatly improves the hydrogen penetration resistance of composite fillers.

[0038] Furthermore, in order to achieve the compatibility of the two-dimensional inorganic composite filler with the epoxy resin and to achieve the close bonding of the composite coating on the substrate, the present invention performs surface modification on the above-mentioned two-dimensional inorganic composite filler by the following steps: firstly, a certain amount of modifier is added to water or weak acid solution and stirred for 0.5 to 2 hours; then, MO is added x @LM two-dimensional inorganic composite filler was fully stirred for 2-6 hours, then filtered and washed with water, and dried at 110°C to obtain the modified two-dimensional inorganic composite filler f-MO x @LM. Finally, a certain amount of epoxy resin and modified two-dimensional inorganic composite filler f-MO were weighed according to a certain ratio. x @LM, fully mix in a vacuum degassing mixer, then add a certain amount of curing agent and mix evenly under vacuum stirring conditions to obtain a composite coating that can be used for coating.

[0039] Compared with existing technologies, MO x @LM can play a dual role of structural hydrogen barrier and hydrogen trap barrier. Among them, the LM peeled off as a single layer / few layers is a high aspect ratio two-dimensional structure. When it is added into epoxy resin, it greatly increases the hydrogen permeation path and reduces the hydrogen permeation factor; MO x Irreversible defect sites (such as oxygen vacancies) are provided, which can adsorb and anchor hydrogen, i.e., hydrogen traps to block hydrogen. The coating can synergistically reduce hydrogen permeability from the perspectives of structural hydrogen blocking and hydrogen trap blocking. The hydrogen permeation blocking composite coating of the present invention has the following advantages:

[0040] 1. The obtained composite coating has excellent hydrogen permeation resistance. A single layer / few layers of nano two-dimensional materials are obtained by exfoliation using a unique process, and highly uniformly dispersed nano metal oxides are grown in situ on them, thereby obtaining a two-dimensional inorganic composite filler with excellent hydrogen resistance. The composite filler has a synergistic effect from the two aspects of structural hydrogen resistance and hydrogen trap hydrogen resistance, which makes the hydrogen permeability of the coating extremely low.

[0041] 2. The composite coating has strong bonding strength with the substrate and has anti-corrosion performance. The selected epoxy resin itself has excellent bonding and anti-corrosion properties, and the modified two-dimensional inorganic composite filler has good compatibility with the epoxy resin. After coating, the coating is dense and defect-free.

[0042] 3. The preparation process adopted is simple and controllable, healthy and environmentally friendly, and suitable for large-scale production and application. The preparation process of the two-dimensional inorganic composite filler with excellent hydrogen barrier performance of the present invention is simple and controllable, the selected epoxy resin system is a solvent-free resin system, which is green and environmentally friendly, and the two can be independently stored for a long time. The composite coating can be prepared on demand and is suitable for large-scale mass production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification, but shall not be construed as limiting the present invention.

[0044] Figure 1 SEM images of the unpeeled mica in Comparative Example 2 at different magnifications.

[0045] Figure 2 SEM images of the peeled mica in Comparative Example 3 at different magnifications.

[0046] Figure 3 TEM images of 0.2TiO2@EMF at different magnifications in Example 1. DETAILED DESCRIPTION

[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Comparative Example 1

[0049] Preparation of epoxy resin EP coating without inorganic filler

[0050] (1) Weigh 1.50 g of bisphenol A epoxy resin E51 and 1.58 g of phenolic amine epoxy curing agent MD550 respectively, place them in a vacuum degassing mixer and mix them evenly for 5 min (1500 rpm) to obtain a solvent-free composite coating.

[0051] (2) The prepared coating is coated on the substrate through a wet film preparation device, and the coating is cured at room temperature for 24 hours to finally obtain an EP coating.

[0052] Comparative Example 2

[0053] Preparation of f-MF / EP coating with only mica powder (not stripped) + epoxy resin

[0054] (1) Measure 25 mL of acetic acid solution (pH = 4), add 0.05 g of modifier 3-glycidyloxypropyltrimethoxysilane SCA-E87M, and stir for 0.5 h; then weigh and add 5 g of mica powder (unpeeled, 6000 mesh), and stir for 24 h;

[0055] (2) Filter and wash with water 3 to 4 times, then dry at 110°C for 2 hours, grind and set aside, and the modified mica inorganic filler is obtained;

[0056] (3) Weigh 1.50 g of E51 resin and 0.31 g of modified mica (accounting for 10% of the total weight of the resin and curing agent), place them in a vacuum degassing mixer and mix them evenly for 5 min (1500 rpm);

[0057] (4) Weigh 1.58 g of MD550 curing agent and add it to the mixed solution (3) above. Then place the mixture in a vacuum degassing mixer and mix it evenly for 5 min (1500 rpm) to obtain a solvent-free composite coating.

[0058] (5) The prepared composite coating is coated on the substrate through a wet film preparation device, and the composite coating is cured at room temperature for 24 hours to finally obtain the f-MF / EP coating.

[0059] Comparative Example 3

[0060] Preparation of f-EMF / EP coating of mica powder (peeled off) + epoxy resin

[0061] 1. Preparation of Mica Nanosheets by Exfoliation:

[0062] (1) Pretreatment: calcine the mica powder at 850°C in a muffle furnace for 3 h, then take 6 g of the mica powder and reflux it in 200 mL of nitric acid solution (5 mol / L) at 95°C for 6 h, filter it, and then stir it in 200 mL of saturated sodium chloride solution at 95°C for 3 h;

[0063] (2) Intercalation: 500 mL of deionized water was measured and heated to 80 °C. The pretreated mica powder and 18.4 g of hexadecyltrimethylammonium bromide (CTAB) were added and stirred for 24 h. The mixture was then filtered and washed with water several times.

[0064] (3) Stripping: The intercalated mica powder filter cake was dispersed in 150 mL of anhydrous ethanol, ultrasonicated for 0.5 h (840 W power), and then centrifuged at 940 × g to obtain the supernatant containing mica nanosheets; then, the supernatant was centrifuged at 10380 × g for 15 min, filtered and washed with alcohol several times to obtain the stripped mica nanosheets (EMF), which were then stored in an appropriate amount of ethanol. The SEM image of the stripped mica nanosheets is shown in the figure. Figure 2 As shown, compared Figure 1 From the SEM image of the unpeeled mica powder, it can be seen that the number of mica flakes is significantly reduced after peeling, indicating that the mica flakes are successfully peeled and a flake material with a higher aspect ratio is obtained.

[0065] 2. Modification of mica nanosheets:

[0066] (1) Measure 25 mL of acetic acid solution (pH = 4), add 0.05 g of modifier SCA-E87M, and stir for 0.5 h; then weigh and add 5 g of mica nanosheets and stir for 24 h;

[0067] (2) Filter and wash with water for 3 to 4 times, then dry at 110 °C for 2 h, grind and set aside, and the modified mica nanosheets (f-EMF) are obtained;

[0068] 3. Preparation of modified mica nanosheet / epoxy resin composite coating:

[0069] (1) Weigh 1.50 g of E51 resin and 0.31 g of the above f-EMF filler (accounting for 10% of the total weight of the resin and curing agent), place in a vacuum degassing mixer and mix evenly for 5 min (1500 rpm);

[0070] (2) Weigh 1.58 g of MD550 curing agent and add it to the mixed solution (1) above. Then place the mixture in a vacuum degassing mixer and mix it evenly for 5 min (1500 rpm) to obtain a solvent-free composite coating.

[0071] (3) The prepared composite coating is coated on the substrate through a wet film preparation device, and the composite coating is cured at room temperature for 24 hours to finally obtain the f-EMF / EP coating.

[0072] Example 1

[0073] Preparation of f-0.2TiO2@EMF / EP composite coating

[0074] 1. Preparation of Mica Nanosheets by Exfoliation:

[0075] (1) Pretreatment: calcine the mica powder at 850°C in a muffle furnace for 3 h, then take 6 g of the mica powder and reflux it in 200 mL of nitric acid solution (5 mol / L) at 95°C for 6 h, filter it, and then stir it in 200 mL of saturated sodium chloride solution at 95°C for 3 h;

[0076] (2) Intercalation: 500 mL of deionized water was measured and heated to 80 °C. The pretreated mica powder and 18.4 g of CTAB were added and stirred for 24 h. The mixture was then filtered and washed several times.

[0077] (3) Stripping: The intercalated mica powder filter cake was dispersed in 150 mL of anhydrous ethanol, ultrasonicated for 0.5 h (840 W power), and then centrifuged at 940 × g to obtain the supernatant containing mica nanosheets; then, the supernatant was centrifuged at 10380 × g for 15 min, filtered and washed with alcohol several times to obtain the stripped mica nanosheets (EMF), which were then preserved with an appropriate amount of ethanol.

[0078] 2.0.2 Preparation of TiO2@EMF composite filler:

[0079] (1) Prepare Ti precursor solution: weigh 12.96 g of anhydrous ethanol, 0.20 g of glacial acetic acid, and 5.32 g of tetrabutyl titanate in a beaker and stir for 10 min. This is referred to as solution A.

[0080] (2) Weigh 5 g (dry weight) of the exfoliated mica nanosheets, pour them into solution A, and stir for 2 h to fully mix and disperse them;

[0081] (3) Under vigorous stirring, add 0.40 g of nitric acid solution (5 mol / L) dropwise to solution A, and then slowly add deionized water at a rate of about 3 s / drop. A total of 1.12 g is added. Solution A gradually becomes viscous and jelly-like. After about 30 minutes, the solution turns into a gel.

[0082] (4) Place the gel in a water bath at 80°C and evaporate to dryness for about 6 hours until nearly dry, then take it out and grind it;

[0083] (5) Calcination in a muffle furnace at 500°C for 3 h to obtain a 0.2TiO2@EMF composite filler with a TiO2 to EMF weight ratio of 1:4, which was ball-milled and bottled for later use. Figure 3 As shown, wrinkle-like lines can be seen on the mica surface at low magnification, and nanoparticle aggregates can be seen at high magnification. According to the captured HRTEM image, ordered lattice fringes can be clearly observed, and the plane spacing calculated by Gatan Digital Micrograph is 0.354nm, which is consistent with the lattice spacing of anatase titanium dioxide, indicating that anatase titanium dioxide is in situ grown on the mica surface.

[0084] 3.0.2 Modification of TiO2@EMF composite filler:

[0085] (1) Measure 25 mL of acetic acid solution (pH = 4), add 0.05 g of modifier SCA-E87M, and stir for 0.5 h; then weigh and add 5 g of 0.2 TiO2@EMF composite filler and stir for 24 h;

[0086] (2) Filter and wash with water for 3 to 4 times, then dry at 110°C for 2 h, grind and set aside to obtain f-0.2TiO2@EMF composite filler.

[0087] 4. Preparation of f-0.2TiO2@EMF / EP composite coating:

[0088] (1) Weigh 1.50 g of E51 resin and 0.31 g of f-0.2TiO2@EMF composite filler (accounting for 10% of the total weight of the resin and curing agent), place in a vacuum degassing mixer and mix evenly for 5 min (1500 rpm);

[0089] (2) Weigh 1.58 g of MD550 curing agent and add it to the mixed solution (1) above. Then place the mixture in a vacuum degassing mixer and mix it evenly for 5 min (1500 rpm) to obtain a solvent-free composite coating.

[0090] (3) The prepared composite coating is coated on the substrate through a wet film preparation device, and the composite coating is cured at room temperature for 24 hours to finally obtain the f-0.2TiO2@EMF / EP coating.

[0091] Example 2

[0092] Preparation of f-0.5TiO2@EMF / EP composite coating

[0093] 1. Preparation of Mica Nanosheets by Exfoliation:

[0094] The preparation method is the same as the exfoliation preparation of mica nanosheets in Example 1.

[0095] 2.0.5 Preparation of TiO2@EMF composite filler:

[0096] (1) Prepare Ti precursor solution: weigh 12.96 g of anhydrous ethanol, 0.20 g of glacial acetic acid, and 21.30 g of tetrabutyl titanate in a beaker and stir for 10 min. This is referred to as solution A.

[0097] (2) Weigh 5 g (dry weight) of the exfoliated mica nanosheets, pour them into solution A, and stir for 2 h to fully mix and disperse them;

[0098] (3) Under vigorous stirring, add 12 drops (0.40 g) of nitric acid solution (5 mol / L) to solution A drop by drop, and then slowly add deionized water at a rate of about 3 s / drop. A total of 1.12 g is added. Solution A gradually becomes viscous and becomes a gel. After about 30 minutes, the solution turns into a gel.

[0099] (4) Place the gel in a water bath at 80°C and evaporate to dryness for about 6 hours until nearly dry, then take it out and grind it;

[0100] (5) Calcinate at 500 °C in a muffle furnace for 3 h to obtain 0.5TiO2@EMF composite filler, which is then ball-milled and bottled for later use.

[0101] 3.0.2 Modification of TiO2@EMF composite filler:

[0102] (1) Measure 25 mL of acetic acid solution (pH = 4), add 0.05 g of modifier SCA-E87M, and stir for 0.5 h; then weigh and add 5 g of 0.5 TiO2@EMF composite filler and stir for 24 h;

[0103] (2) Filter and wash with water for 3 to 4 times, then dry at 110°C for 2 h, grind and set aside to obtain f-0.5TiO2@EMF composite filler.

[0104] 4. Preparation of f-0.5TiO2@EMF / EP composite coating:

[0105] (1) Weigh 1.50 g of E51 resin and 0.31 g of f-0.5TiO2@EMF composite filler (accounting for 10% of the total weight of the resin and curing agent), place in a vacuum degassing mixer and mix evenly for 5 min (1500 rpm);

[0106] (2) Weigh 1.58 g of MD550 curing agent and add it to the mixed solution (1) above. Then place the mixture in a vacuum degassing mixer and mix it evenly for 5 min (1500 rpm) to obtain a solvent-free composite coating.

[0107] (3) The prepared composite coating is coated on the substrate through a wet film preparation device, and the composite coating is cured at room temperature for 24 hours to finally obtain the f-0.5TiO2@EMF / EP coating.

[0108] Example 3

[0109] f-0.2Al2O3@EMF / EP coating

[0110] 1. Preparation of Mica Nanosheets by Exfoliation:

[0111] The preparation method is the same as the exfoliation preparation of mica nanosheets in Example 1.

[0112] 2.0.2 Preparation of Al2O3@EMF composite filler:

[0113] (1) Prepare Al precursor solution: weigh 2.19 g of aluminum nitrate into a beaker, add 2-3 drops of acetic acid solution (pH=3), then pour in 10 mL of deionized water and stir for 10 min. This is referred to as solution A.

[0114] (2) Weigh 5 g (dry weight) of the exfoliated mica nanosheets, pour them into solution A, and stir for 2 h to fully mix and disperse them;

[0115] (3) Under vigorous stirring, the water bath temperature was raised to 60°C, and 2.1 g of ammonia solution (5 mol / L) was added dropwise to solution A at a rate of about 1 s / drop. Solution A gradually became gelatinous and was allowed to stand for about 60 min.

[0116] (4) Place it in a water bath at 80°C and evaporate to dryness. The sol will gradually gel. It will take about 12 hours to evaporate until it is nearly dry. Then take it out and grind it.

[0117] (5) Calcinate at 500 °C in a muffle furnace for 3 h to obtain 0.2Al2O3@EMF composite filler, which is then ball-milled and bottled for later use.

[0118] 3.0.2 Modification of Al2O3@EMF composite filler:

[0119] (1) Measure 25 mL of acetic acid solution (pH = 3), add 0.10 g of modifier SCA-E87T, and stir for 1 h; then weigh and add 5 g of 0.2 Al2O3@EMF composite filler and stir for 24 h;

[0120] (2) Filter and wash with water for 5 times, then dry at 110℃ for 2h, grind and set aside to obtain f-0.2Al2O3@EMF composite filler.

[0121] 4.0.2 Preparation of Al2O3@EMF / EP composite coating:

[0122] (1) Weigh 1.50 g of E51 resin and 0.31 g of f-0.2Al2O3@EMF composite filler (accounting for 10% of the total weight of the resin and curing agent), place them in a vacuum degassing mixer and mix them evenly for 5 min (1500 rpm);

[0123] (2) Weigh 1.58 g of MD550 curing agent and add it to the mixed solution (1) above. Then place the mixture in a vacuum degassing mixer and mix it evenly for 5 min (1500 rpm) to obtain a solvent-free composite coating.

[0124] (3) The prepared composite coating is coated on the substrate through a wet film preparation device, and the composite coating is cured at room temperature for 24 hours to finally obtain the f-0.2Al2O3@EMF / EP coating.

[0125] Example 4

[0126] The test method for the hydrogen permeation resistance effect is as follows: the H2 permeability (H2GTR) of the composite coating is measured at 25°C and 0.1MPa using an SMT-275 membrane separation test analyzer. The permeability coefficient P is the product of the permeability and the coating thickness. The hydrogen permeation resistance performance of the composite coatings of the comparative examples and embodiments is shown in Table 1.

[0127] Table 1 Comparison of hydrogen permeation resistance of various composite coatings.

[0128] Serial number Coating name Coating thickness (μm) Transmittance* Transmission coefficient** Drop rate Comparative Example 1 EP 106 221.406 23.469 Reference Comparative Example 2 f-MF / EP 110 144.561 15.902 32.2% Comparative Example 3 f-EMF / EP 57 41.841 2.385 89.8% Example 1 <![CDATA[f-0.2TiO2@EMF / EP]]> 64 2.387 0.153 99.3% Example 2 <![CDATA[f-0.5TiO2@EMF / EP]]> 65 1.021 0.067 99.7% Example 3 <![CDATA[f-0.2Al2O3@EMF / EP]]> 75 2.257 0.169 99.3%

[0129] *: The unit of transmittance is cm 3 / m 2 / 24h / 0.1MPa.

[0130] **: The unit of permeability is cm 3 .mm / m 2 / 24h / 0.1MPa.

[0131] As shown in Table 1, the hydrogen permeability coefficient of pure epoxy resin (EP) is 23.469 cm 3 .mm / m 2 / 24h / 0.1MPa (Comparative Example 1), indicating that the resin system itself has a high cross-linking density and a small free volume, and thus has good hydrogen barrier properties;

[0132] After adding modified mica filler, the hydrogen permeability coefficient of the coating (f-MF / EP) was reduced to 15.902 cm 3 .mm / m 2 / 24h / 0.1MPa (Comparative Example 2), indicating that the two-dimensional sheet structure of mica can extend the hydrogen permeation path. This "maze effect" reduces hydrogen permeation, and the hydrogen permeation resistance is improved by 32.2%; the mica is peeled off to create a more complex "maze effect" to further reduce the hydrogen permeability of the coating (Comparative Example 3), and the hydrogen permeation resistance of the obtained coating (f-EMF / EP) is further improved by 85.0% (83.1% compared to the EP coating);

[0133] More importantly, the metal oxide (TiO2, Al2O3) modified on the surface of the stripped mica (Examples 1-3) can further capture and anchor hydrogen in the oxygen vacancies in the metal oxide, thereby significantly reducing the hydrogen permeability coefficient of the coating, and promoting its hydrogen permeation resistance to jump by 93.6%, 97.2%, and 93.0%, respectively (compared with the EP coating, it increased by 99.3%, 99.7%, and 99.3%, respectively). The content of the metal oxide modified on the surface of the stripped mica has a great influence on the hydrogen resistance. On the premise of ensuring the coating effect, the more the amount added, the better the hydrogen resistance, such as No. 5 The composite coating, whose TiO2 addition amount is 50%, has a 56.2% improvement in hydrogen barrier performance compared with the composite filler coating with 20% TiO2 addition. This also shows that the patent of the present invention has a wide hydrogen barrier performance control window, which can be controlled by the metal oxide content in the composite filler.

[0134] The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions also belong to the scope of the present invention. The patent protection scope of the present invention should be defined by the claims.

Claims

1. A composite resin coating that blocks hydrogen penetration, characterized in that: The coating is composed of a modified two-dimensional inorganic composite filler f-MO x @LM is mixed with epoxy resin and then cured. The modified two-dimensional inorganic composite filler f-MO x @The weight ratio of LM to epoxy resin EP is 1:19~1:2; Two-dimensional inorganic composite filler MO x @LM by MO x Metal oxides are in situ grown on the surface of the exfoliated LM layered materials. x The weight ratio with LM is 1:100~1:1; The MO x Metal oxides are Al2O3, TiO2, ZnO, Cr2O3, NiO, MgO; The LM layered material is a layered non-metallic material, selected from one or more of kaolin, montmorillonite, graphite, sericite, muscovite, boron nitride and hydrotalcite.

2. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 1, characterized in that: The following steps are involved: S1. Peeling off the LM layered material to obtain the peeled LM layered material; S2.MO x Metal oxides are in situ grown on the surface of the exfoliated LM layered material to obtain a two-dimensional inorganic composite filler MO. x @LM; S3. Modification of two-dimensional inorganic composite filler MOx@LM; S4. Modified two-dimensional inorganic composite filler f-MO x @LM is dispersed into epoxy resin and coated on the substrate to form a hydrogen permeation barrier coating.

3. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 2, characterized in that: The step S1 specifically includes the following steps: (1) Pretreatment: The LM layered material is calcined at high temperature in a muffle furnace, refluxed in a nitric acid solution, filtered, and then stirred in a saturated sodium chloride solution to obtain a pretreated LM layered material; (2) Intercalation: Disperse the pretreated LM layered material in deionized water, heat and add the intercalation agent, stir, and wash with water to obtain the intercalated LM layered material; (3) The intercalated LM layered material is dispersed in a solvent, subjected to ultrasound, and centrifuged to obtain a supernatant containing the exfoliated LM nanosheets at a speed of 900×g-1000×g; the supernatant is then centrifuged at a speed of more than 10380×g, filtered, and washed with water to obtain the exfoliated LM layered material.

4. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 3, characterized in that: The intercalant is one or more of hexadecyltrimethylammonium bromide, N-methylformamide, hydrazine hydrate, urea, lithium borohydride, tetramethylammonium ion, tetraethylammonium ion, tetrapropylammonium ion, tetrabutylammonium ion, sulfate ion, and propylamine; The solvent is one or more of ethanol, isopropanol and N,N-dimethylformamide.

5. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 2, characterized in that: The step S2 specifically includes the following steps: (1) preparing a precursor solution containing M metal, adding a dispersant or a hydrolysis inhibitor, and then pouring the exfoliated LM layered material into it and mixing it thoroughly to obtain a solution A; (2) Under stirring, add solution B containing a precipitant or hydrolyzing agent, and solution A gradually forms a sol, and metal M grows in situ on the peeled LM layered material, and then continue to stir until the sol completely turns into a gel; after drying, calcination and grinding, a two-dimensional inorganic composite filler MO is obtained. x @LM.

6. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 5, characterized in that: The solute in the precursor solution containing the M metal is an inorganic salt containing the M metal or an organic compound containing the M metal, and the M metal is Al, Ti, Zn, Cr, Ni, or Mg; The dispersant or hydrolysis inhibitor is one or more of polyethylene glycol, polypropylene glycol, citric acid, glacial acetic acid, formic acid, anhydrous ethanol, diethanolamine, and acetylacetone; The precipitant or hydrolyzing agent is one or more of NaOH, KOH, Na2CO3, K2CO3, (NH4)2CO3, ammonia water, urea, glacial acetic acid, nitric acid and hydrochloric acid.

7. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 2, characterized in that: The step S3 comprises the following steps: Add the modifier to water or weak acid solution and stir; add two-dimensional inorganic composite filler MO x @LM, stirred, filtered, washed with water, and dried to obtain the modified two-dimensional inorganic composite filler f-MO x @LM.

8. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 7, characterized in that: The modifier is one or more of 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane and 3-glycidyloxypropylmethyldimethoxysilane.

9. The method for preparing a composite resin coating that blocks hydrogen penetration according to claim 2, characterized in that: The step S4 specifically comprises: treating the modified two-dimensional inorganic composite filler f-MO x @LM is stirred and mixed with epoxy resin, and then a curing agent is added, and the mixture is evenly mixed in a vacuum degassing mixer to obtain a solvent-free composite coating. The composite coating is coated on a substrate through a wet film preparation device and cured at room temperature to obtain a composite resin coating; The epoxy resin is one of glycidyl ether epoxy resin and glycidyl amine epoxy resin; the curing agent is aliphatic amine, alicyclic amine, aromatic amine, phenolic amine or polyamide.

10. The use of a composite resin coating for preventing hydrogen penetration according to claim 1, characterized in that: The coating is used in hydrogen transmission pipelines and hydrogen cylinders.

Citation Information

Patent Citations

  • Alumina / montmorillonite / epoxy resin nano-composite material

    CN109721950A

  • Oxide ceramic and two-dimensional material composite hydrogen-resistant coating and preparation method thereof

    CN115044868A

  • Hydrogen-permeation-resistant coating, preparation method thereof and application of hydrogen-permeation-resistant coating on stainless steel surface

    CN117887293A

  • Composite coating for hydrogen pipeline and preparation method of composite coating

    CN117965074A

  • Producing method of carbon-nanosheets composits

    KR1020110016289A

Cited By

  • High-hydrophobicity coating for fan blade and preparation method of high-hydrophobicity coating

    CN119410259A

  • Odor-free latex for high-brightness labor protection gloves and preparation method of odor-free latex

    CN120699194A

  • A method for preparing, products and applications of composite coatings based on modified two-dimensional MOFs

    CN123107505A