Continuous casting production method for large-specification round billet of power station boiler tube billet steel
By using small taper crystallizer and optimizing process parameters during the continuous casting of SA-335P92 round billet, the problems of open-polluted steel, longitudinal cracks and tail billets are solved, and the ultra-supercritical power plant boiler tube billet steel is realized Stable production and high-quality finished products.
Patent Information
- Application Number
- CN202411146582.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
During the continuous casting of the SA-335P92 round billet for boiler tube steel of ultra-supercritical power station, problems such as open-cast steel, longitudinal cracks on the surface of the casting billet and upturning of the tail billet, resulting in low yield and difficult to achieve stable production.
Use small taper crystallizer and upper and lower plum petal crystallizer to optimize the pouring process parameters, including adjusting liquid level, vibration, water flow and pulling machine pressure, use special protective slag and covering agent to control overheat and pulling speed, and ensure blowing Argon protection and cutting process, extending slow cooling time to resolve surface defects of the casting billet.
The stable production of SA-335P92 round billet continuous casting has been achieved, and the problems of open-poured steel, longitudinal cracks and tail billets have been solved, the yield rate and economic benefits have been improved, and the product quality has been ensured.
Abstract
Description
Technical Field
[0001] The invention relates to a large-size round billet continuous casting production method for power station boiler tube billet steel, in particular to a φ690 size production process of SA-335P92 round billet continuous casting production process for ultra-supercritical power station boiler tube billet steel. Background Art
[0002] SA-335P92 is a steel for ultra-supercritical power plant boilers. It belongs to the new heat-resistant steel series and is used to manufacture heat-receiving tubes such as high-pressure boiler reheaters and superheaters, boiler headers with metal wall temperatures ≤600℃, steam pipes, etc. It is widely used in power plant boilers, petroleum and petrochemical industries. Its use environment is harsh, and it has high requirements for the content of non-metallic inclusions and ultrasonic flaw detection of finished products. The lower the oxygen content, the better. The production process is difficult, and large-section round billet continuous casting is a problem in the steel industry. Our factory's SA-335P92 steel grade originally used die casting technology, and the billet formation rate was low. In March 2015, the round billet continuous casting was completed and put into production. The conditions for continuous casting production of SA-335P92 have been met, and the trial of SA-335P92 conversion to continuous casting production has begun.
[0003] The purpose of the present invention is to realize the stable production of φ690 round billet continuous casting of power station boiler tube billet steel SA-335P92, solve the problem of steel leakage in the middle ladle during continuous casting production, eliminate the problems of longitudinal crack defects on the surface of the casting billet, upturned tail billet, etc., open up the SA-335P92 slow cooling process route, and solve the problem of normal production organization affected by the constraints of heat treatment process. Summary of the invention
[0004] The purpose of the present invention is to solve the above problems and provide a method for continuously casting large-sized round billets of boiler tube steel for power station.
[0005] The object of the present invention is achieved as follows: A method for continuous casting of large-size round billets of boiler tube steel for power station, comprising the following aspects: (1) replacing the crystallizer before production, using a small-taper crystallizer for the crystallizer, and using an upper and lower plum petal crystallizer for the crystallizer copper tube; (2) material preparation, preparing special materials before production; (3) setting the pouring process parameters; (4) ingot plugging: optimizing the ingot plugging method, placing the cold material, placing the pouring cup in the center of the crystallizer, filling the ingot head groove connecting claw with steel bars, filling the outer arc side of the ingot head groove with springs, placing two circles of short springs around the spring fixing iron ring, and requiring 35-45kg of springs and short springs. After the ingot plugging is completed, lubricating oil is applied to the inner wall of the crystallizer copper tube. It is required to apply enough and evenly to ensure the lubrication effect of the billet shell; (5 ) Operation of ladle pouring: After the ladle molten steel arrives at the station, quickly organize the tundish to stop the fire, drive the tundish car to the casting position, hang the ladle long nozzle and start blowing argon protection, the flow rate is 80-120L / min, the sealing gasket of the ladle long nozzle is replaced every furnace, before the tundish pouring, ensure the argon blowing time is 2-3 minutes, and blow argon to protect the casting during the whole casting process. The argon flow rate on both sides is 250-350L / min, and operate the ladle pouring; (6) After the ladle pouring, wait until the molten steel volume in the tundish is ≥25t, organize the tundish pouring, control the tundish pouring emergence time, and control the emergence time within 60-90 seconds. It is required to flow in the first 60 seconds, and the flow rate is controlled at 7-8kg / s. The molten steel covers the head of the ingot head, and then reduce the flow to 4-5kg / s; (7) Tundish superheat and casting speed control. The overheat of SA-335P92 tundish is controlled at 30-40℃, which is 5℃ higher than other steel grades, and the target pulling speed is 0.22-0.24m / min. (8) Adjust the pressing parameters of the straightening machine, increase the pressing force of the billet tail, keep the tail billet pressure of the 1st to 5th group of straightening machines unchanged, maintain 500-550kN, and adjust the tail billet pressure of the 6th to 11th group of straightening machines to 1000-1200kN. After cutting the tail to the 7th group, cancel the tracking of the straightening machine, keep all straightening machines in the pressing state, and do not lift automatically. After the tail is cut and leaves the 11th group of straightening machines, the tail billet pressure value is adjusted back to the normal value of 500-550kN; (9) Adjust the cutting parameters: Before cutting, the cutting carbon equivalent parameter is set to a constant of 1.0-1.5 to ensure that iron powder is sprayed throughout the cutting process. The cutting length setting tolerance is set to a positive tolerance of 100-150mm; (10) Before cutting, the frequency of the dust removal fan of the flame cutting machine is set to 40-50Hz, and then adjusted back to 30-40Hz after cutting; (11) Slow cooling process: The hot billet is put into the pit for slow cooling after it comes off the line. The slow cooling time is ≥36h. At the same time, it is required to be slowly cooled to a surface temperature of <150℃ before leaving the pit.
[0006] (3) The process parameters for pouring are as follows: ① Lower the liquid level in the crystallizer to 54-56%; ② Adjust the vibration parameters of the crystallizer to a frequency of 290-300spm / m and an amplitude of 3.3-3.5mm; ③ Reduce the water flow rate in the crystallizer to 3650-3750L / min; ④ Reduce the starting speed of pouring, the starting speed of the straightening machine is 0.11m / min, and the starting acceleration is 0.01-0.02m / min 2 , the casting speed of the billet at the beginning is 0.11m / min; ⑤Electromagnetic stirring setting, the electromagnetic stirring current of the casting strand is 230-250A, the frequency is 2.0-2.5Hz, and the switching time is 10-20s, the electromagnetic stirring current of the secondary cooling is 90-110A, the frequency is 1.8-2.2Hz, and the switching time is 10-20s, and the terminal electromagnetic stirring current is 380-410A, the frequency is 1.0-1.2Hz, and the switching time is 10-20s.
[0007] The beneficial effects of the present invention are as follows: through the above continuous casting process control operation method, SA-335P92 steel for ultra-supercritical power station boiler tube billets can be smoothly cast into large-size round billets, and the number of continuous casting furnaces can reach 4. The problem of steel leakage during continuous casting is solved. The problem of longitudinal cracks on the surface of the billet is solved by optimizing process parameters and using special protective slag. The problem of tail billet warping is solved by adjusting the pressing force of the straightening machine. The billet slow cooling process route is opened up, stable continuous casting production is achieved, the problem of large core defects is solved, and economic benefits are improved. DETAILED DESCRIPTION
[0008] A method for continuous casting of large-size round billets for boiler tube steel for power stations, comprising: (1) replacing a crystallizer before production, using a small-taper crystallizer with a taper of 1.82%, and using an upper and lower plum petal crystallizer for the crystallizer copper tube; (2) preparing materials, preparing special materials before production, using SA-335P92 special materials, using Xibao special protective slag with fast melting speed and low viscosity for crystallizer protection slag, and using Luoyang Kefeng T-FZK13HB middle-package covering agent with low melting point for middle-package covering agent.
[0009] (3) The process parameters for pouring are as follows: ① Lower the liquid level in the crystallizer to 54-56%; ② Adjust the vibration parameters of the crystallizer to a frequency of 290-300spm / m and an amplitude of 3.3-3.5mm; ③ Reduce the water flow rate in the crystallizer to 3650-3750L / min; ④ Reduce the starting speed of pouring, the starting speed of the straightening machine is 0.11m / min, and the starting acceleration is 0.01-0.02m / min 2, the casting speed of the billet at the beginning is 0.11m / min; ⑤Electromagnetic stirring setting, the electromagnetic stirring current of the casting strand is 230-250A, the frequency is 2.0-2.5Hz, and the switching time is 20s, the electromagnetic stirring current of the secondary cooling is 90-110A, the frequency is 1.8-2.2Hz, and the switching time is 20s, and the terminal electromagnetic stirring current is 380-410A, the frequency is 1.0-1.2Hz, and the switching time is 20s.
[0010] (4) Ingot plugging: Optimize the ingot plugging method, place the cold material, place the pouring cup in the center of the crystallizer, fill the connecting claws of the ingot head groove with steel bars, fill the outer arc side of the south end of the ingot head groove with springs, and place two circles of short springs around the spring fixing iron ring. The springs and short springs require a total of 35 kg to ensure the cooling effect. After the ingot plugging is completed, apply lubricating oil on the inner wall of the crystallizer copper tube. Apply enough and even oil to ensure the lubrication effect of the billet shell.
[0011] (5) Operation of ladle pouring: After the ladle molten steel arrives at the station, quickly organize the tundish to stop the fire, drive the tundish car to the casting position, hang the ladle long nozzle and start blowing argon protection, the flow rate is 80-120L / min, the sealing gasket of the ladle long nozzle is replaced every furnace, the argon blowing time is guaranteed to be 2-3 minutes before the tundish is poured, and argon is blown to protect the casting throughout the casting process. The argon flow rate on both sides is 250-350L / min, and the ladle is operated to start pouring; (6) After the ladle is poured, wait until the amount of molten steel in the tundish is ≥25t, organize the tundish to pour, control the time of the tundish to pour, and the time of the germination is controlled within 60 to 90 seconds. The flow rate is controlled at 7-8kg / s in the first 60 seconds, and the molten steel covers the head of the ingot head, and then the flow is reduced to 4-5kg / s.
[0012] (7) Tundish superheat and drawing speed control. The tundish superheat of SA-335P92 is controlled at 30-40℃, which is 5℃ higher than other steel grades. The target drawing speed is 0.22-0.24m / min.
[0013] (8) Adjust the pressing parameters of the straightening machine, increase the pressing force of the billet tail, keep the tail billet pressure of the 1st to 5th group of straightening machines unchanged, maintain 500-550kN, and adjust the tail billet pressure of the 6th to 11th group of straightening machines to 1000-1200kN. After the tail is cut to the 7th group, cancel the tracking of the straightening machine, keep all the straightening machines in the pressing state, and do not lift automatically. After the tail is cut and leaves the 11th group of straightening machines, the tail billet pressure value is adjusted back to the normal value of 500-550kN. (9) Adjust cutting parameters: Before cutting, set the cutting carbon equivalent parameter to a constant of 1.0-1.5 to ensure that iron powder is sprayed throughout the cutting process. The cutting length setting tolerance is set to a positive tolerance of 100-150mm.
[0014] (10) Before cutting, set the dust removal fan frequency of the flame cutting machine to 45Hz, and adjust it back to 40Hz after cutting.
[0015] (11) Slow cooling process: The hot billet is put into the pit for slow cooling. The slow cooling time is ≥36h. At the same time, it is required to be slowly cooled to a surface temperature of <150℃ before leaving the pit.
[0016] The specific implementation of the method of the present invention is described in detail below in conjunction with examples, but the specific implementation of the present invention is not limited to the following implementation cases.
[0017] 1. Replace the crystallizer before production. Use a small taper crystallizer with a taper of 1.82%, and use an upper and lower plum petal crystallizer for the crystallizer copper tube.
[0018] 2. Optimize the pouring process parameters as follows: (1) Lower the mold liquid level setting from the normal setting value of 59-61% to 54-56%.
[0019] (2) Adjust the vibration parameters of the crystallizer: the frequency is adjusted from 330-350spm / m to 290-300spm / m, and the amplitude is adjusted from 2.8-3.1mm to 3.3-3.5mm.
[0020] (3) Reduce the crystallizer water flow rate from the normal 3950-4050 L / min to 3650-3750 L / min.
[0021] (4) Reduce the starting pouring speed. The starting speed of the straightening machine remains unchanged at 0.11m / min, and the starting acceleration is 0.01-0.02m / min 2 , the initial casting speed of the billet was reduced from 0.12m / min to 0.11m / min.
[0022] (5) Optimize the method of plugging the ingot. Place the cold material and the pouring cup in the center of the crystallizer. Fill the connecting claws of the ingot head groove with steel bars. Fill the outer arc side of the south end of the ingot head groove with springs. Place two circles of short springs around the spring fixing iron ring. A total of 35 kg of springs are required to ensure the cooling effect. After the ingot is plugged, apply lubricating oil on the inner wall of the copper tube of the crystallizer. Apply enough and even oil.
[0023] (6) Control the time for the tundish to start pouring and seedling emergence. The seedling emergence time is controlled within 60 to 90 seconds. The flow rate is required to be controlled at 7-8 kg / s in the first 60 seconds, and the molten steel covers the head of the ingot starter. Then the flow rate is reduced to 4-5 kg / s. (7) Adjust the pressing parameters of the straightening machine, increase the pressing force on the billet tail, keep the tail billet pressure of the 1st to 5th group of straightening machines unchanged, maintain 500-550kN, and adjust the tail billet pressure of the 6th to 11th group of straightening machines to 1000-1200kN. After the tail is cut to the 7th group, cancel the tracking of the straightening machine, keep all the straightening machines in the pressing state, and do not lift automatically. After the tail is cut and leaves the 11th group of straightening machines, the tail billet pressure value is adjusted back to the normal value of 500-550kN; (8) Adjust cutting parameters. Before cutting, set the cutting carbon equivalent parameter to a constant of 1.0-1.5 to ensure that iron powder is sprayed throughout the cutting process. Set the cutting length tolerance to +100-150mm to ensure the fixed length.
[0024] (9) Before cutting begins, set the frequency of the dust removal fan of the flame cutting machine to 45Hz, and adjust it back to 40Hz after cutting to improve the dust removal system's collection effect on smoke. After cutting, adjust it back to normal. This flexible operation protects the environment, protects on-site workers, and saves energy consumption.
[0025] 3. Material preparation: prepare special materials before production. Use SA-335P92 special material. Select Xibao special protective slag with fast melting speed and low viscosity for crystallizer protection slag. Select Luoyang Kefeng T-FZK13HB tundish covering agent with low melting point to prevent carbon increase in the tundish.
[0026] 4. Tundish superheat and drawing speed control. The tundish superheat of SA-335P92 is controlled at 30-40℃, which is 5℃ higher than other steel grades, and the target drawing speed is 0.22-0.24m / min.
[0027] 5. Electromagnetic stirring settings: casting electromagnetic stirring current 230-250A, frequency 2.0-2.5Hz, reversing time 20s, secondary cooling electromagnetic stirring current 90-110A, frequency 1.8-2.2Hz, reversing time 20s, end electromagnetic stirring current 380-410A, frequency 1.0-1.2Hz, reversing time 20s.
[0028] On March 2, 2024, the Φ690 specification single package 4 continuous casting SA-335P92 was organized. The material preparation, process parameter setting, and process control before pouring were strictly implemented. The pouring process was normal, the casting process was normal, and the billet cutting process was normal. The low-power inspection results of the billet met the requirements.
[0029] Through the above measures, a total of 6 castings of SA-335P92 production were organized from March to July 2024, with a total of 24 furnaces produced and a qualified output of 1,700 tons. The casting and production processes were all normal, the product quality was qualified, and SA-335P92 steel for power station boilers was mass-produced.
[0030] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.
Claims
1. A method for continuous casting of large-size round billets of boiler tube steel for power station, characterized in that: These include: (1) Replace the crystallizer before production. Use a small-taper crystallizer and an upper and lower plum petal crystallizer for the crystallizer copper tube; (2) Material preparation: prepare special materials before production; (3) Setting of pouring process parameters; (4) Ingot plugging: Optimize the ingot plugging method, place the cold material, place the pouring cup in the center of the crystallizer, fill the connecting claws of the ingot head groove with steel bars, fill the outer arc side of the ingot head groove with springs, and place two circles of short springs around the spring fixing iron ring. The springs and short springs require a total of 35-45kg. After the ingot plugging is completed, apply lubricating oil on the inner wall of the crystallizer copper tube. Apply enough and even oil to ensure the lubrication effect of the billet shell; (5) Operation of ladle pouring: After the ladle molten steel arrives at the station, quickly organize the tundish to stop the fire, drive the tundish car to the casting position, hang the ladle long nozzle and start blowing argon protection, the flow rate is 80-120L / min, the sealing gasket of the ladle long nozzle is replaced every furnace, the argon blowing time is guaranteed to be 2-3 minutes before the tundish is poured, and argon is blown to protect the casting throughout the casting process. The argon flow rate on both sides is 250-350L / min, and the ladle is operated to start pouring; (6) After the ladle is poured, wait until the amount of molten steel in the tundish is ≥25t, organize the tundish to pour, control the time of the tundish to pour and the time of the seedlings to emerge, which should be controlled within 60 to 90 seconds. The flow rate should be controlled at 7-8kg / s in the first 60 seconds, and the molten steel should cover the head of the ingot head, and then reduce the flow rate to 4-5kg / s; (7) Tundish superheat and drawing speed control. The tundish superheat of SA-335P92 is controlled at 30-40℃, which is 5℃ higher than other steel grades, and the target drawing speed is 0.22-0.24m / min; (8) Adjust the pressing parameters of the straightening machine, increase the pressing force of the billet tail, keep the tail billet pressure of the 1st to 5th group of straightening machines unchanged, maintain 500-550kN, and adjust the tail billet pressure of the 6th to 11th group of straightening machines to 1000-1200kN. After the tail is cut to the 7th group, cancel the tracking of the straightening machine, keep all the straightening machines in the pressing state, and do not lift automatically. After the tail is cut and leaves the 11th group of straightening machines, the tail billet pressure value is adjusted back to the normal value of 500-550kN; (9) Adjust cutting parameters: Before cutting, set the cutting carbon equivalent parameter to a constant of 1.0-1.5 to ensure that iron powder is sprayed throughout the cutting process, and set the cutting length tolerance to a positive tolerance of 100-150mm; (10) Before cutting, set the dust removal fan frequency of the flame cutting machine to 40-50Hz, and adjust it back to 30-40Hz after cutting; (11) Slow cooling process: The hot billet is put into the pit for slow cooling. The slow cooling time is ≥36h. At the same time, it is required to be slowly cooled to a surface temperature of <150℃ before leaving the pit.
2. The method for continuous casting of large-size round billets of boiler tube steel for power station according to claim 1, characterized in that: (3) The process parameters for pouring are as follows: ① Lower the liquid level in the crystallizer to 54-56%; ② Adjust the vibration parameters of the crystallizer to a frequency of 290-300spm / m and an amplitude of 3.3-3.5mm; ③ Reduce the water flow rate in the crystallizer to 3650-3750L / min; ④ Reduce the starting speed of pouring, the starting speed of the straightening machine is 0.11m / min, and the starting acceleration is 0.01-0.02m / min 2 , the casting speed of the billet at the beginning is 0.11m / min; ⑤Electromagnetic stirring setting, the electromagnetic stirring current of the casting strand is 230-250A, the frequency is 2.0-2.5Hz, and the switching time is 10-20s, the electromagnetic stirring current of the secondary cooling is 90-110A, the frequency is 1.8-2.2Hz, and the switching time is 10-20s, and the terminal electromagnetic stirring current is 380-410A, the frequency is 1.0-1.2Hz, and the switching time is 10-20s.
Citation Information
Patent Citations
Method for increasing flaw detection yield of continuous casting sheet head billet and tail billet
CN103586433A
Continuous open casting technique of high alloy stainless steel
CN103600048A
Flame-preheated cutting method for steel plate with high-carbon equivalent thickness of smaller than 30mm
CN104759733A
Casting-on device and method for ultra-large-specification continuous casting round billet
CN115055655A
Continuous casting method for large round billet of tungsten-containing heat-resistant steel
CN115074607A
Cited By
High-pressure-resistant heat-resistant round steel and preparation method thereof
CN120350318A
High-pressure heat-resistant round steel and preparation method thereof
CN120350318B