Method for controlling stability of liquid level of crystallizer in peritectic steel production process

By optimizing the protection slag composition and cooling water flow and adjusting the pulling speed, the problem of unstable crystallizer liquid level during the casting of the continuous casting machine is solved, the quality of the casting billet and the production stability are improved, and the adaptation of industrial applications is achieved. Sexual and economic benefits.

CN119035477APending Publication Date: 2024-11-29SHANDONG IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411213076.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the continuous casting machine, the liquid level of the crystallizer is unstable, resulting in longitudinal cracks, slag inclusions on the surface of the casting billet, which affects the quality of the final rolling material, and there are excessive inclusions in the casting billet and leakage of steel. Vicious production accident.

Method used

By optimizing the composition and cooling water flow of the crystallizer protection slag and adjusting the pulling speed, controlling the stability of the crystallizer liquid level, specifically including increasing the alkalinity of the protection slag and reducing its viscosity, adjusting the water flow and pulling speed, and using non-metallic addition Slag nozzle achieves stability control of liquid level.

Benefits of technology

It effectively improves the surface quality of the casting billet, reduces surface defects, improves the qualification rate of the casting billet, reduces the finishing amount, increases the hot delivery ratio, creates economic benefits, and adapts to industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020768010000121
    Figure BDA0005020768010000121
  • Figure BDA0005020768010000122
    Figure BDA0005020768010000122
  • Figure HDA0005020768030000011
    Figure HDA0005020768030000011
Patent Text Reader

Abstract

The invention provides a method for controlling the stability of the liquid level of a crystallizer in the peritectic steel production process, which comprises the following steps of: reducing the wide-surface water flow and the narrow-surface water flow of an inner cavity of the crystallizer; the alkalinity of the crystallizer peritectic steel casting powder is improved, the viscosity of the crystallizer peritectic steel casting powder is reduced, and the crystallizer peritectic steel casting powder is adjusted to be specific components; controlling the pulling speed of the crystallizer; the stability of the liquid level of the crystallizer is controlled by regulating and controlling the steps in the peritectic steel production process. According to the condition of existing process equipment of a slab continuous casting machine, influence factors of the crystallizer liquid level fluctuation problem in the peritectic steel production process are systematically analyzed, an optimization scheme of casting powder, cooling water, the pulling speed and the like is formulated, the liquid level fluctuation problem is effectively solved, the crystallizer liquid level stability in the peritectic steel pouring process of the continuous casting machine is achieved, and the casting quality is improved. And the surface quality of the casting blank is improved. And existing equipment of the continuous casting machine is not changed, and the method has the advantages of low investment, quick effect and the like and has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparing peritectic steel by pouring with a continuous casting machine, and relates to the application of mold protection slag in improving the stability of the crystallizer liquid level in the peritectic steel production process and a method for controlling the crystallizer liquid level stability in the peritectic steel production process, and in particular to a method for controlling the crystallizer liquid level stability in the peritectic steel production process. Background Art

[0002] In the process of intelligent control of steelmaking continuous casting production line, with the increase of the types of steel produced, the proportion of peritectic steel cast by continuous casting machine gradually increased. In the production process, the problem of unstable liquid level in the crystallizer began to occur frequently, and the fluctuation had a certain periodicity, which was more common when casting peritectic steel. Excessive liquid level fluctuation will first affect the three-layer structure of the crystallizer protective slag, destroy its lubrication and heat transfer balance, and cause surface defects such as longitudinal cracks on the surface of the ingot. Secondly, it will also increase the risk of slag rolling of molten steel in the crystallizer, causing slag rolling on the surface of the ingot, and the inclusion content in the ingot exceeded the standard, which seriously affected the quality of the final rolled product, and even caused vicious production accidents such as longitudinal cracks and steel leakage in the ingot, slag inclusion and steel leakage.

[0003] Therefore, how to find a more suitable way to solve the above-mentioned technical problems existing in the existing process has become one of the urgent problems to be solved by many front-line researchers in the industry. Summary of the invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide an application of mold protection slag in improving the stability of the mold liquid level in the production process of peritectic steel and a method for controlling the stability of the mold liquid level in the production process of peritectic steel. The method provided by the present invention effectively solves the problem of the crystallizer liquid level fluctuation in the current continuous casting machine during the casting of peritectic steel, which is of great significance for improving the surface quality of the continuous casting billet and ensuring stable and smooth production. In addition, the process flow is simple, controllable, and adaptable, and it is more suitable for industrial promotion and application.

[0005] The present invention provides an application of mold protection slag in improving the stability of the mold liquid level in the peritectic steel production process;

[0006] The mold powder, measured by mass content, includes:

[0007] SiO2: 28.45%;

[0008] Al2O3: 3.91%;

[0009] CaO: 40.73%;

[0010] F: 11.57%;

[0011] Na2O: 10.47%;

[0012] C solid: 3.51%.

[0013] Preferably, the moisture content of the mold protection slag is 0.16% by mass;

[0014] The basicity of the mold protection slag is 1.42;

[0015] The mold powder also includes a balance of inevitable impurities.

[0016] Preferably, the melting point of the mold protection slag is 1130°C;

[0017] The viscosity of the mold protection slag is 0.10 Pa.S;

[0018] The application specifically also includes increasing the basicity of the mold protection slag to improve the stability of the mold liquid level during the production of peritectic steel and / or reducing the viscosity of the mold protection slag to improve the stability of the mold liquid level during the production of peritectic steel.

[0019] The present invention also provides a method for controlling the stability of a crystallizer liquid level during the production of peritectic steel, comprising the following steps:

[0020] 1) Reduce the water flow rate on the wide surface and narrow surface of the crystallizer cavity;

[0021] 2) increasing the basicity of the mold peritectic steel protection slag, reducing the viscosity of the mold peritectic steel protection slag, and adjusting the mold peritectic steel protection slag to a specific component;

[0022] 3) Control the pulling speed of the crystallizer;

[0023] By regulating the above steps 1) to 3) during the production of peritectic steel, the stability of the crystallizer liquid level is controlled.

[0024] Preferably, the production specifications of the crystallizer are that the width of the peritectic steel slab is 2330 mm and the thickness is 175 mm; or that the width of the peritectic steel slab is 1663 mm and the thickness is 175 mm;

[0025] The production specification is a crystallizer with a peritectic steel slab length of 2330 mm, a reduced wide surface water flow rate of 4300-4400 L / min, and a narrow surface water flow rate of 340-360 L / min;

[0026] The production specification is a crystallizer with a peritectic steel slab length of 1663 mm, a reduced wide surface water flow rate of 2900-3000 L / min, and a narrow surface water flow rate of 340-360 L / min.

[0027] Preferably, the adjusted mold powder comprises, by mass content:

[0028] SiO2: 28.45%;

[0029] Al2O3: 3.91%;

[0030] CaO: 40.73%;

[0031] F: 11.57%;

[0032] Na2O: 10.47%;

[0033] C solid: 3.51%.

[0034] Preferably, the basicity of the improved mold protection slag is 1.42;

[0035] The adjusted moisture content of the mold protection slag is 0.16% by mass.

[0036] Preferably, the viscosity of the mold protection slag after the reduction is 0.10 Pa.S;

[0037] The step 2) further comprises lowering the melting point of the mold peritectic steel protection slag;

[0038] The melting point of the reduced mold protection slag is 1130°C.

[0039] Preferably, the pulling speed of the crystallizer is 1.25-1.35 m / min;

[0040] The method further comprises adding a slag nozzle to the non-metallic crystallizer.

[0041] Preferably, the crystallizer liquid level stability is controlled within ±1.5m.

[0042] The present invention provides an application of a mold protection slag in improving the stability of a crystallizer liquid level in a peritectic steel production process; the mold protection slag comprises, by mass content: SiO2: 28.45%; Al2O3: 3.91%; CaO: 40.73%; F: 11.57%; Na2O: 10.47%; and C solid: 3.51%. Compared with the prior art, the present invention systematically analyzes the problem of liquid level fluctuation in the crystallizer during the production of peritectic steel, targets a variety of key influencing factors, especially optimizes the protective slag, cooling water, pulling speed, etc., controls the heat transfer performance of the protective slag, enables the primary billet shell to grow evenly, appropriately reduces the flow rate of a cold water and increases the billet pulling speed, and slows down the heat transfer of the crystallizer, which can also promote the uniform growth of the primary billet shell. The evenly grown billet shell is cooled by a second cold water in the fan-shaped segment, and the bulging deformation of the billet between the rollers in the fan-shaped segment is reduced, thereby effectively improving the problem of liquid level fluctuation in the production process of peritectic steel, significantly improving the surface quality of the billet, significantly reducing defects such as surface longitudinal cracks and subcutaneous slag addition, significantly improving the qualified rate of the billet, significantly reducing the amount of finishing, and increasing the proportion of hot delivery, thereby generating good economic benefits.

[0043] The present invention studies the crystallizer liquid level fluctuation control technology for peritectic steel, and proposes a control method for the crystallizer liquid level stability in the peritectic steel production process, which solves the problem of crystallizer liquid level fluctuation in the current continuous casting machine during the casting of peritectic steel, and is of great significance for improving the surface quality of continuous casting billets and ensuring stable and smooth production. The present invention is aimed at the periodic and violent fluctuation of the liquid level caused by the uneven growth of the primary solidified billet shell in the crystallizer during the production of peritectic steel. It is believed that on the one hand, a weak cooling method of the crystallizer can be used to promote the uniform and stable growth of the primary billet shell, and on the other hand, the thickness of the billet shell can be increased by enhancing the secondary cooling strength. The present invention aims to produce a uniform billet shell in a crystallizer. Starting from the aspects of heat transfer performance of protective slag, primary cooling water strength, secondary cooling water strength, pulling speed control model, material and model of automatic slag adding nozzle, etc., the heat flux density in the crystallizer is reduced, heat transfer is slowed down, and normal liquid level fluctuation in the crystallizer during the peritectic steel production process is achieved. Surface cracks, slag inclusions and other defects caused by liquid level fluctuations on the ingot surface are reduced, the qualified rate of the ingot is improved, the finishing caused by ingot surface quality problems is reduced, the heat delivery rate is improved, energy consumption is reduced, and considerable economic benefits are created.

[0044] According to the existing process equipment status of the slab continuous casting machine, the present invention systematically analyzes the influencing factors of the crystallizer liquid level fluctuation problem in the peritectic steel production process, formulates the optimization schemes of protective slag, cooling water, casting speed, etc., effectively improves the liquid level fluctuation problem, achieves the stability of the crystallizer liquid level in the process of casting peritectic steel by the continuous casting machine, and improves the surface quality of the casting. Moreover, the existing equipment of the continuous casting machine is not changed, and improvements and innovations are made according to the characteristics of the existing process equipment, which has the advantages of low investment and quick results, and has broad application prospects.

[0045] The implementation results show that by adopting the control method provided by the present invention, the liquid level fluctuation of the crystallizer of the slab continuous casting machine is stabilized at about ±1.5mm in on-site practice, the cleaning of the fallen ingots and the tracking of the rolled material quality are normal, the use effect is remarkable, the qualified rate of the ingots is increased from 97.55% to more than 99.55%, and the amount of finishing due to unqualified surface quality of the ingots is significantly reduced, the proportion of direct hot delivery of the ingots is increased, and the annual direct economic benefits are considerable. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 A field photo of the liquid level of the crystallizer of the slab continuous casting machine for casting peritectic steel provided by the present invention;

[0047] Figure 2 The historical fluctuation curve of the liquid level of the existing slab continuous casting machine crystallizer (±3mm);

[0048] Figure 3 The method provided by the present invention controls the fluctuation curve (±1.3 mm) of the liquid level of the peritectic steel crystallizer of the slab continuous casting machine;

[0049] Figure 4 The surface quality of the cleaned cast billet in the production of peritectic steel for the slab continuous casting machine provided by the present invention (normal);

[0050] Figure 5 The surface quality of peritectic steel rolled products prepared by the slab continuous casting machine provided by the present invention (normal). DETAILED DESCRIPTION

[0051] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention rather than limiting the patent claims of the present invention.

[0052] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0053] There is no particular restriction on the purity of all raw materials in the present invention. In the present invention, industrial purity or conventional purity in the field of peritectic steel prepared by continuous casting machine casting is preferably used.

[0054] The brands and abbreviations of all raw materials of the present invention are conventional brands and abbreviations in the art. Each brand and abbreviation is clear and definite in the field of its related use. Those skilled in the art can purchase them from the market or prepare them by conventional methods according to the brands, abbreviations and corresponding uses.

[0055] The present invention provides an application of mold protection slag in improving the stability of the mold liquid level in the peritectic steel production process;

[0056] The mold powder, measured by mass content, includes:

[0057] SiO2: 28.45%;

[0058] Al2O3: 3.91%;

[0059] CaO: 40.73%;

[0060] F: 11.57%;

[0061] Na2O: 10.47%;

[0062] C solid: 3.51%.

[0063] In the present invention, the water content of the mold powder is preferably 0.16% by mass.

[0064] In the present invention, the basicity of the mold protection slag is preferably 1.42.

[0065] In the present invention, the mold powder preferably further includes a balance of inevitable impurities.

[0066] In the present invention, the melting point of the mold protection slag is preferably 1130°C.

[0067] In the present invention, the viscosity of the mold protection slag is preferably 0.10 Pa.S.

[0068] In the present invention, the application specifically also preferably includes the application of increasing the basicity of the mold protection slag in improving the stability of the mold liquid level during the peritectic steel production process.

[0069] In the present invention, the application specifically also preferably includes the application of reducing the viscosity of the mold protection slag in improving the stability of the mold liquid level during the peritectic steel production process.

[0070] The present invention provides a method for controlling the liquid level stability of a crystallizer in a peritectic steel production process, comprising the following steps:

[0071] 1) Reduce the water flow rate on the wide surface and narrow surface of the crystallizer cavity;

[0072] 2) increasing the basicity of the mold peritectic steel protection slag, reducing the viscosity of the mold peritectic steel protection slag, and adjusting the mold peritectic steel protection slag to a specific component;

[0073] 3) Control the pulling speed of the crystallizer;

[0074] By regulating the above steps 1) to 3) during the production of peritectic steel, the stability of the crystallizer liquid level is controlled.

[0075] In the present invention, in the control method, steps 1) to 3) have no sequence.

[0076] The present invention firstly reduces the wide surface water flow and the narrow surface water flow of the inner cavity of the crystallizer.

[0077] In the present invention, the production specifications of the crystallizer are preferably that the width of the peritectic steel slab is 2330 mm and the thickness is 175 mm; or that the width of the peritectic steel slab is 1663 mm and the thickness is 175 mm.

[0078] In the present invention, the production specification is preferably a crystallizer with a peritectic steel slab length of 2330 mm, and the water flow rate on the wide side after reduction is preferably 4300-4400 L / min, and the water flow rate on the narrow side is 340-360 L / min, more preferably the water flow rate on the wide side after reduction is 4320-4380 L / min, and the water flow rate on the narrow side is 344-356 L / min, more preferably the water flow rate on the wide side after reduction is 4340-4360 L / min, and the water flow rate on the narrow side is 348-352 L / min.

[0079] In the present invention, the production specification is preferably a crystallizer with a peritectic steel slab length of 1663 mm, and the water flow rate on the wide surface after reduction is preferably 2900-3000 L / min, and the water flow rate on the narrow surface is 340-360 L / min, more preferably the water flow rate on the wide surface after reduction is 2920-2980 L / min, and the water flow rate on the narrow surface is 344-356 L / min, more preferably the water flow rate on the wide surface after reduction is 2940-2960 L / min, and the water flow rate on the narrow surface is 348-352 L / min.

[0080] The invention further improves the basicity of the crystallizer peritectic steel protection slag, reduces the viscosity of the crystallizer peritectic steel protection slag and adjusts the crystallizer peritectic steel protection slag to a specific component.

[0081] In the present invention, the adjusted mold powder preferably comprises, by mass content:

[0082] SiO2: 28.45%;

[0083] Al2O3: 3.91%;

[0084] CaO: 40.73%;

[0085] F: 11.57%;

[0086] Na2O: 10.47%;

[0087] C solid: 3.51%.

[0088] In the present invention, the improved basicity of the mold protection slag is preferably 1.42.

[0089] In the present invention, the moisture content of the adjusted mold powder is preferably 0.16%.

[0090] In the present invention, the reduced viscosity of the mold protection slag is preferably 0.10 Pa.S.

[0091] In the present invention, the step 2) preferably further comprises lowering the melting point of the mold peritectic steel protection slag.

[0092] In the present invention, the melting point of the mold protection slag after the reduction is preferably 1130°C.

[0093] The present invention then controls the pulling speed of the crystallizer.

[0094] In the present invention, the pulling speed of the crystallizer is preferably 1.25-1.35 m / min, more preferably 1.27-1.33 m / min, and more preferably 1.29-1.31 m / min.

[0095] In the present invention, the method preferably further comprises adding a slag nozzle to the non-metallic crystallizer.

[0096] In the present invention, the stability of the liquid level in the crystallizer is controlled within ±1.5 m.

[0097] Finally, the present invention controls the stability of the crystallizer liquid level by regulating the above steps 1) to 3) during the peritectic steel production process.

[0098] The present invention is a complete and detailed overall technical solution, which can better control the stability of the crystallizer liquid level and further improve the qualified rate of the casting of peritectic steel. The application of the above-mentioned crystallizer protection slag in improving the stability of the crystallizer liquid level in the production process of peritectic steel and a method for controlling the stability of the crystallizer liquid level in the production process of peritectic steel can specifically include the following contents:

[0099] See also Figure 1 , Figure 1 This is a field photo of the liquid level in the crystallizer of the slab continuous casting machine for pouring peritectic steel provided by the present invention.

[0100] Cold water cooling intensity (inner cavity water flow)

[0101] From the mechanism of liquid level fluctuation in the crystallizer during the production process of peritectic steel, it can be seen that the uniform and stable growth of the primary solidified shell in the crystallizer is the key to solving the liquid level fluctuation. By gradually reducing the water flow rate on the wide and narrow sides, the liquid level fluctuation changes significantly. When the liquid level fluctuation no longer changes, the appropriate crystallizer water flow rate is determined.

[0102] Weak cooling achieved by reducing the water flow in the crystallizer can effectively suppress the periodic and violent fluctuations of the liquid level.

[0103] Cold water cooling intensity (external spray cooling water)

[0104] In order to suppress the periodic fluctuation of the liquid level caused by the thin shell of the billet after leaving the crystallizer, which is caused by the obvious bulging under the static pressure of the molten steel, the target surface temperature curve of the area above the straightening point in the second cooling zone of the second cooling model was lowered respectively in combination with the actual production on site. It can be seen from the historical trend chart of the liquid level fluctuation that after the second cooling intensity is enhanced, the liquid level fluctuation in the crystallizer is still quite violent. The test shows that adjusting the cooling intensity of the second cooling zone alone has no obvious effect on controlling the periodic violent fluctuation of the crystallizer liquid level.

[0105] Optimizing mold powder performance

[0106] During the casting process, the behavior of the protective slag layer directly affects the lubrication and heat transfer of the crystallizer. Steels of different compositions have different molten steel properties and solidification characteristics, which determines that the requirements for the performance of the crystallizer protective slag are also different. Therefore, special protective slag is needed. For peritectic steel with strong shrinkage, in order to increase the uniformity of the billet shell, the peritectic steel protective slag is required to have a large thermal resistance to achieve a weak cooling effect of the crystallizer. High crystallization temperature and high basicity protective slag are selected to increase the ratio of the solid phase layer and the crystallization phase, slow down heat transfer, and reduce the heat conductivity at the meniscus of the crystallizer, so that the primary billet shell grows uniformly. The melting point and viscosity of the existing protective slag are high, which affects the normal melting and slagging of the protective slag. For this reason, the peritectic steel protective slag is adjusted in two aspects relative to the original slag:

[0107] Increasing the basicity of the original peritectic steel protection slag from 1.24 to 1.42 increases the crystal phase ratio in the protection slag liquid slag, which can slow down the heat transfer in the crystallizer and make the solidification of the primary shell in the crystallizer more uniform.

[0108] The viscosity is reduced from the original 0.18Pa.S to 0.10Pa.S, the F and Na2O content is increased, the viscosity and melting point of the protective slag are reduced, the melting rate of the protective slag is increased, and the lubrication effect of the protective slag is improved. After using the improved protective slag, the fluctuation range of the peritectic steel liquid level is controlled at ±3mm, and the improvement effect is significant.

[0109] Optimizing the casting speed control model

[0110] When casting peritectic steel, the crystallizer liquid level fluctuates violently periodically, and the pulling speed reduction operation has no effect, and may even aggravate the fluctuation. This is mainly because the speed reduction is equivalent to indirectly enhancing the cooling of the crystallizer, but aggravates the peritectic phase transformation reaction of the molten steel solidification process in the crystallizer. When the protective slag is not adjusted, the high viscosity protective slag cannot fill the gaps caused by the peritectic reaction in time, and the heat transfer is uneven, which will aggravate the unevenness of the shell. On the contrary, increasing the pulling speed is more conducive to controlling the liquid level fluctuation, because increasing the pulling speed is equivalent to indirectly reducing the cooling intensity of the crystallizer. It plays the same role as reducing the cooling water flow of the crystallizer. In actual production, the pulling speed is generally controlled in the range of 1.25-1.35m / min.

[0111] Optimize the material and model of automatic slag adding nozzle

[0112] The continuous casting machine adopts an eddy current type tundish stopper rod automatic control system. The electromagnetic signal in the eddy current sensor generates eddy current on the surface of the molten steel, and acts on the sensor to generate induced current. The magnitude of the sensor induced current varies with the distance from the surface of the molten steel to the bottom of the sensor. The secondary instrument filters the sensor induced signal, collects the effective signal, calculates and outputs the voltage and current signal that can represent the liquid level after analog-to-digital conversion, and transmits it to the system PLC. The system PLC acts on the digital driver through comprehensive processing of various information, controls the CNC electric cylinder, and adjusts the stopper rod position. The flow of molten steel injected from the tundish into the crystallizer is adjusted by controlling the stopper rod opening, so as to achieve the purpose of stably controlling the height of the molten steel liquid level in the crystallizer, thereby realizing automatic steel casting with constant drawing speed and constant liquid level.

[0113] In order to improve the stability of the mold slag addition operation, avoid leakage, over-addition, uneven distribution of mold slag, etc., and reduce the labor intensity of employees and improve the automation of the continuous casting process, an automatic slag feeder is used. Due to the poor working environment of the slag nozzle of the automatic slag feeder, the equipment needs to have wear-resistant and high-temperature resistant characteristics, and is currently made of stainless steel. During use, it was found that the liquid level fluctuated regularly, with a fluctuation range of ±3mm, which has reached the upper limit of the on-site control standard. This regular liquid level fluctuation is a major hidden danger to the surface quality of the ingot.

[0114] See also Figure 2 , Figure 2 It is the historical fluctuation curve (±3mm) of the liquid level in the crystallizer of the existing slab continuous casting machine.

[0115] Through on-site tracking, it was found that the slag adding nozzle of the automatic slag adding would pass through the liquid level control system probe during the lateral movement, and the time interval was consistent with the liquid level fluctuation time interval. Therefore, it was inferred that the slag adding nozzle made of stainless steel affected the accuracy of the liquid level control system. After removing the automatic slag feeder, the liquid level fluctuation range was significantly reduced, which verified the above inference again. The liquid level fluctuation of the crystallizer was compared before and after the automatic slag feeder was used, and the liquid level fluctuation was not observed when the automatic slag device was not used. The slag adding nozzle on the side with the liquid control probe can be replaced with a ceramic material, or the external dimensions of the slag adding nozzle can be further optimized to minimize its impact on liquid level automatic control.

[0116] The present invention integrates the above methods, and through on-site practice, the liquid level fluctuation of the crystallizer of the slab continuous casting machine is stabilized at about ±1.5mm, and the cleaning of the fallen ingots and the tracking of the rolled material quality are all normal, with significant use effect.

[0117] The above content of the present invention provides the application of mold protection slag in improving the stability of the crystallizer liquid level in the production process of peritectic steel and a method for controlling the stability of the crystallizer liquid level in the production process of peritectic steel. The present invention systematically analyzes the problem of crystallizer liquid level fluctuation in the production process of peritectic steel, optimizes the protection slag, cooling water, drawing speed, etc. in particular, targets multiple key influencing factors, controls the heat transfer performance of the protection slag, enables the primary billet shell to grow uniformly, appropriately reduces the flow rate of a cold water and increases the billet drawing speed, slows down the heat transfer of the crystallizer, and can also promote the uniform growth of the primary billet shell. The uniformly grown billet shell is cooled by a second cold water in the fan-shaped section, and the bulging deformation of the billet between the rollers in the fan-shaped section is reduced, thereby effectively improving the problem of liquid level fluctuation in the production process of peritectic steel, significantly improving the surface quality of the billet, significantly reducing defects such as surface longitudinal cracks and subcutaneous slag addition, significantly improving the qualified rate of the billet, significantly reducing the finishing amount, and increasing the hot delivery ratio, resulting in good economic benefits.

[0118] The present invention studies the crystallizer liquid level fluctuation control technology for peritectic steel, and proposes a control method for the crystallizer liquid level stability in the peritectic steel production process, which solves the problem of crystallizer liquid level fluctuation in the current continuous casting machine during the casting of peritectic steel, and is of great significance for improving the surface quality of continuous casting billets and ensuring stable and smooth production. The present invention is aimed at the periodic and violent fluctuation of the liquid level caused by the uneven growth of the primary solidified billet shell in the crystallizer during the production of peritectic steel. It is believed that on the one hand, a weak cooling method of the crystallizer can be used to promote the uniform and stable growth of the primary billet shell, and on the other hand, the thickness of the billet shell can be increased by enhancing the secondary cooling strength. The present invention aims to produce a uniform billet shell in a crystallizer. Starting from the aspects of heat transfer performance of protective slag, primary cooling water strength, secondary cooling water strength, pulling speed control model, material and model of automatic slag adding nozzle, etc., the heat flux density in the crystallizer is reduced, heat transfer is slowed down, and normal liquid level fluctuation in the crystallizer during the peritectic steel production process is achieved. Surface cracks, slag inclusions and other defects caused by liquid level fluctuations on the ingot surface are reduced, the qualified rate of the ingot is improved, the finishing caused by ingot surface quality problems is reduced, the heat delivery rate is improved, energy consumption is reduced, and considerable economic benefits are created.

[0119] According to the existing process equipment status of the slab continuous casting machine, the present invention systematically analyzes the influencing factors of the crystallizer liquid level fluctuation problem in the peritectic steel production process, formulates the optimization schemes of protective slag, cooling water, casting speed, etc., effectively improves the liquid level fluctuation problem, achieves the stability of the crystallizer liquid level in the process of casting peritectic steel by the continuous casting machine, and improves the surface quality of the casting. Moreover, the existing equipment of the continuous casting machine is not changed, and improvements and innovations are made according to the characteristics of the existing process equipment, which has the advantages of low investment and quick results, and has broad application prospects.

[0120] The implementation results show that by adopting the control method provided by the present invention, the liquid level fluctuation of the crystallizer of the slab continuous casting machine is stabilized at about ±1.5mm in on-site practice, the cleaning of the fallen ingots and the tracking of the rolled material quality are normal, the use effect is remarkable, the qualified rate of the ingots is increased from 97.55% to more than 99.55%, and the amount of finishing due to unqualified surface quality of the ingots is significantly reduced, the proportion of direct hot delivery of the ingots is increased, and the annual direct economic benefits are considerable.

[0121] To further illustrate the present invention, the application of the mold protection slag provided by the present invention in improving the stability of the crystallizer liquid level in the production process of peritectic steel and a method for controlling the stability of the crystallizer liquid level in the production process of peritectic steel are described in detail below in combination with the embodiments. However, it should be understood that these embodiments are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the embodiments described below.

[0122] Example

[0123] A series of comparative tests on control measures were carried out in combination with actual on-site production.

[0124] Cold water cooling intensity

[0125] It can be seen from the mechanism of liquid level fluctuation in the crystallizer during the production process of peritectic steel that the uniform and stable growth of the primary solidified shell in the crystallizer is the key to solving the liquid level fluctuation. By gradually reducing the water flow rates on the wide and narrow sides, the liquid level fluctuation changes significantly. When the liquid level fluctuation no longer changes, the appropriate crystallizer water flow rate is determined, and the continuous casting machine crystallizer water flow rate is adjusted from the value shown in Table 1 to the flow value shown in Table 2.

[0126] Table 1 Original crystallizer water flow value

[0127]

[0128] Table 2 Adjusted crystallizer water flow value

[0129]

[0130] Experiments show that reducing the water flow rate in the crystallizer to achieve weak cooling can effectively suppress the periodic and violent fluctuations of the liquid level.

[0131] Cold water cooling intensity

[0132] In order to suppress the periodic fluctuation of the liquid level caused by the thin shell of the billet after leaving the crystallizer, which is caused by the obvious bulging under the static pressure of the molten steel, the target surface temperature curve of the area above the straightening point in the second cooling zone of the second cooling model was reduced by 10℃ and 30℃ respectively, combined with the actual production on site. It can be seen from the historical trend chart of the liquid level fluctuation that after the second cooling intensity is enhanced, the liquid level fluctuation in the crystallizer is still quite violent, which shows that adjusting the cooling intensity of the second cooling zone alone has no obvious effect on controlling the periodic and violent fluctuation of the crystallizer liquid level.

[0133] Optimizing mold powder performance

[0134] During the casting process, the behavior of the protective slag layer directly affects the lubrication and heat transfer of the crystallizer. Steels of different compositions have different molten steel properties and solidification characteristics, which determines that the requirements for the performance of the protective slag of the crystallizer are also different. Therefore, special protective slag is needed. For example, for peritectic steel with strong shrinkage, in order to increase the uniformity of the billet shell, the peritectic steel protective slag is required to have a large thermal resistance to achieve the weak cooling effect of the crystallizer. High crystallization temperature and high basicity protective slag are selected to increase the ratio of the solid phase layer and the crystal phase, slow down heat transfer, and reduce the heat conductivity at the meniscus of the crystallizer, so that the primary billet shell grows uniformly. The melting point and viscosity of the existing protective slag are high, which affects the normal melting and slagging of the protective slag. For this reason, the peritectic steel protective slag is adjusted in two aspects relative to the original slag, see Table 3.

[0135] Table 3 Peritectic steel protection slag before and after adjustment of the present invention

[0136] Protective slag model <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO F <![CDATA[Na2O]]> C solid Moisture Alkalinity Melting point Viscosity Original slag 30.11 3.82 37.19 6.68 6.17 3.94 0.21 1.24 1150 0.18 Improved slag 28.45 3.91 40.73 11.57 10.47 3.51 0.16 1.42 1130 0.10

[0137] Increasing the basicity of the original peritectic steel protection slag from 1.24 to 1.42 increases the crystal phase ratio in the protection slag liquid slag, which can slow down the heat transfer in the crystallizer and make the solidification of the primary shell in the crystallizer more uniform.

[0138] The viscosity is reduced from the original 0.18Pa.S to 0.10Pa.S, the F and Na2O content is increased, the viscosity and melting point of the protective slag are reduced, the melting rate of the protective slag is increased, and the lubrication effect of the protective slag is improved. After using the improved protective slag, the fluctuation range of the peritectic steel liquid level is controlled at ±3mm, and the improvement effect is significant.

[0139] Optimizing the casting speed control model

[0140] A large number of production practices have shown that when the casting peritectic steel has periodic and violent fluctuations in the crystallizer liquid level, reducing the pulling speed has no effect and may even aggravate the fluctuations. This is mainly because reducing the speed is equivalent to indirectly enhancing the cooling of the crystallizer, but it aggravates the peritectic phase transformation reaction of the molten steel solidification process in the crystallizer. When the protective slag is not adjusted, the high viscosity protective slag cannot fill the gaps caused by the peritectic reaction in time, and the heat transfer is uneven, which will aggravate the unevenness of the shell. On the contrary, increasing the pulling speed is more conducive to controlling the liquid level fluctuations, because increasing the pulling speed is equivalent to indirectly reducing the cooling intensity of the crystallizer. It plays the same role as reducing the cooling water flow of the crystallizer. In actual production, the pulling speed is generally controlled in the range of 1.25 to 1.35 m / min.

[0141] Optimize the material and model of automatic slag adding nozzle

[0142] The continuous casting machine adopts an eddy current type tundish stopper rod automatic control system. The electromagnetic signal in the eddy current sensor generates eddy current on the surface of the molten steel, and acts on the sensor to generate induced current. The magnitude of the sensor induced current varies with the distance from the surface of the molten steel to the bottom of the sensor. The secondary instrument filters the sensor induced signal, collects the effective signal, calculates and outputs the voltage and current signal that can represent the liquid level after analog-to-digital conversion, and transmits it to the system PLC. The system PLC acts on the digital driver through comprehensive processing of various information, controls the CNC electric cylinder, and adjusts the stopper rod position. The flow of molten steel injected from the tundish into the crystallizer is adjusted by controlling the stopper rod opening, so as to achieve the purpose of stably controlling the height of the molten steel liquid level in the crystallizer, thereby realizing automatic steel casting with constant drawing speed and constant liquid level.

[0143] In order to improve the stability of the protective slag adding operation, avoid missing addition, over-addition, uneven distribution of protective slag, etc., and at the same time reduce the labor intensity of employees and improve the degree of automation of the continuous casting process, an automatic slag feeder is used. Due to the poor working environment of the slag adding nozzle of the automatic slag feeder, the equipment must be wear-resistant and high-temperature resistant, and is currently made of stainless steel.

[0144] During use, it was found that the liquid level fluctuated regularly with a fluctuation range of ±3mm, which has reached the upper limit of the on-site control standard. This regular liquid level fluctuation is a major hidden danger to the surface quality of the casting.

[0145] Through on-site tracking, it was found that the slag adding nozzle of the automatic slag adding would pass through the liquid level control system probe during the lateral movement, and the time interval was consistent with the liquid level fluctuation time interval. Therefore, it was inferred that the slag adding nozzle made of stainless steel affected the accuracy of the liquid level control system. After removing the automatic slag feeder, the liquid level fluctuation range was significantly reduced, which verified the above inference again. The liquid level fluctuation of the crystallizer was compared before and after the automatic slag feeder was used, and the liquid level fluctuation was not observed when the automatic slag device was not used. The slag adding nozzle on the side with the liquid control probe can be replaced with a ceramic material, or the external dimensions of the slag adding nozzle can be further optimized to minimize its impact on liquid level automatic control.

[0146] The present invention integrates the above methods, and through on-site practice, the liquid level fluctuation of the crystallizer of the slab continuous casting machine is stabilized at about ±1.5mm, and the cleaning of the fallen ingots and the tracking of the rolled material quality are all normal, with significant use effect.

[0147] See also Figure 3 , Figure 3 The method provided by the present invention controls the fluctuation curve (±1.3 mm) of the liquid level of the peritectic steel crystallizer of the slab continuous casting machine.

[0148] See also Figure 4 , Figure 4 The surface quality of the cleaned cast billet in peritectic steel production of the slab continuous casting machine provided by the present invention is (normal).

[0149] See also Figure 5 , Figure 5 The surface quality of peritectic steel rolled products prepared by the slab continuous casting machine provided by the present invention (normal).

[0150] The above is a detailed introduction to the application of the mold protection slag provided by the present invention in improving the stability of the mold liquid level in the production process of peritectic steel and a method for controlling the stability of the mold liquid level in the production process of peritectic steel. The principle and implementation method of the present invention are described in detail using specific examples in this article. The description of the above embodiments is only used to help understand the method and its core idea of ​​the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including manufacturing and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified in several ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. Application of mold protection slag in improving mold liquid level stability during peritectic steel production; The mold powder, measured by mass content, include: Not. 2 :28.45%; <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> :3.91%; CaO: 40.73%; F:11.57%; So 2 O:10.47%; C solid: 3.51%.

2. The use according to claim 1, It is characterized in that The moisture content of the mold protection slag is 0.16% by mass; The basicity of the mold protection slag is 1.42; The mold powder also includes a balance of inevitable impurities.

3. The use according to claim 1, It is characterized in that The melting point of the mold protection slag is 1130°C; The viscosity of the mold protection slag is 0.10 Pa.S; The application specifically also includes increasing the basicity of the mold protection slag to improve the stability of the mold liquid level during the production of peritectic steel and / or reducing the viscosity of the mold protection slag to improve the stability of the mold liquid level during the production of peritectic steel.

4. A method for controlling the stability of the crystallizer liquid level during the production of peritectic steel, It is characterized in that The following steps are involved: 1) Reduce the water flow rate on the wide surface and narrow surface of the crystallizer cavity; 2) increasing the basicity of the mold peritectic steel protection slag, reducing the viscosity of the mold peritectic steel protection slag, and adjusting the mold peritectic steel protection slag to a specific component; 3) Control the pulling speed of the crystallizer; By regulating the above steps 1) to 3) during the production of peritectic steel, the stability of the liquid level in the crystallizer is controlled.

5. The method according to claim 4, It is characterized in that The production specifications of the crystallizer are: the width of the peritectic steel slab is 2330mm and the thickness is 175mm; or, the width of the peritectic steel slab is 1663mm and the thickness is 175mm; The production specification is a crystallizer with a peritectic steel slab length of 2330 mm, a reduced wide surface water flow rate of 4300-4400 L / min, and a narrow surface water flow rate of 340-360 L / min; The production specification is a crystallizer with a peritectic steel slab length of 1663 mm, a reduced wide surface water flow rate of 2900-3000 L / min, and a narrow surface water flow rate of 340-360 L / min.

6. The method according to claim 4, It is characterized in that The adjusted mold powder, measured by mass content, includes: Not. 2 :28.45%; <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> :3.91%; CaO: 40.73%; F:11.57%; So 2 O:10.47%; C solid: 3.51%.

7. The method according to claim 4, It is characterized in that The basicity of the improved mold protection slag is 1.42; The adjusted moisture content of the mold protection slag is 0.16% by mass.

8. The method according to claim 4, It is characterized in that The viscosity of the mold protection slag after the reduction is 0.10 Pa.S; The step 2) further comprises lowering the melting point of the mold peritectic steel protection slag; The melting point of the reduced mold protection slag is 1130°C.

9. The method according to claim 4, It is characterized in that The pulling speed of the crystallizer is 1.25-1.35 m / min; The method further comprises adding a slag nozzle to the non-metallic crystallizer.

10. The method according to claim 4, It is characterized in that The crystallizer liquid level stability is controlled within ±1.5m.

Citation Information

Cited By

  • Control method for inhibiting periodic fluctuation of crystallizer liquid level in SPHC steel grade production